Precursor solution of hole transport layer as well as preparation method and application of precursor solution

By using the combination of cuprous thiocyanate and specific mixed solvents, an efficient hole transport layer was prepared, which solved the stability and harmful solvent problems of PEDOT:PSS in the prior art, and improved the efficiency and stability of organic solar cells. sex.

CN118900574APending Publication Date: 2024-11-05BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410915377.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing hole transport layer material PEDOT:PSS is easily corrosive at high temperatures, has high hydrophilicity and low infrared light transmittance, which limits the stability and efficiency of organic solar cells, and the solvent selection of alternative material cuprous thiocyanate is limited. And harmful.

Method used

Using cuprous thiocyanate as the solute, DMSO or CH3OH as the first solvent, ammonia water or DMF as the second solvent, the hole transport layer precursor solution is prepared by specific dissolution and filtration methods to form an efficient hole transport layer .

Benefits of technology

The energy conversion efficiency, short-circuit current density and fill factor of organic solar cells are improved, the stability of the device is enhanced, and the preparation cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900574A_ABST
    Figure CN118900574A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of organic solar cells, and discloses a hole transport layer precursor solution and a preparation method and application thereof. The precursor solution takes cuprous thiocyanate as a solute and takes a mixed solvent as a solvent; wherein the mixed solvent comprises a first solvent and a second solvent; the first solvent is DMSO (dimethyl sulfoxide) or CH3OH; the second solvent is ammonia water or DMF. Cuprous thiocyanate is subjected to first dissolution in a first solvent of the mixed solvent and then subjected to second dissolution in a second solvent, and the hole transport layer precursor solution is obtained. The hole transport layer prepared from the hole transport layer precursor solution has a clear structure, and the prepared organic solar cell has higher energy conversion efficiency, short-circuit current density and fill factor, and is high in PCE stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic solar cells, and in particular to a hole transport layer precursor solution and a preparation method and application thereof. Background Art

[0002] Organic solar cells (OSCs) are attractive for future applications in wearable electronics, indoor lighting, and the Internet of Things (IoT) due to their flexibility, solution processability, relatively low manufacturing cost, and wide availability of materials.

[0003] In recent years, with the exploration of new materials and continuous improvement of device processes, the photoelectric conversion efficiency (PCE) of OSCs can be greater than 20%. In addition to the photoactive layer, the material selection of the electron transport layer (ETL) responsible for transmitting electrons and the hole transport layer (HTL) responsible for transmitting holes also has an impact on the PCE and stability of OSCs. However, the research on these interface layers is relatively lagging, especially the material selection range of HTLs is relatively small.

[0004] The most commonly used hole transport layer material is poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS). This is because it has the advantages of easy preparation at low temperature, high transmittance in the visible light range, good conductivity, suitable work function (WF) and excellent film forming properties. However, this material also has the following disadvantages: (1) The strongly acidic PEDOT:PSS aqueous solution will corrode the indium tin oxide electrode material (ITO), resulting in a weakened stability of the battery; (2) PEDOT:PSS has high hydrophilicity and is easily affected by the atmospheric environment; (3) The transmittance in the infrared region is not high, resulting in a low current density of the battery device. These disadvantages not only affect the stability of the device, but also limit its future application prospects. Therefore, there is an urgent need to develop an efficient, long-term stable and easy to solution process HTL material.

[0005] In this context, a very cheap p-type semiconductor material, cuprous thiocyanate (CuSCN), has gradually become a candidate material for HTL. Compared with PEDOT:PSS, CuSCN has the advantages of good transmittance in the visible and near-infrared regions, high hole mobility, good thermal stability and suitable work function, making it very suitable as a hole transport layer for optoelectronic devices.

[0006] However, the solvent options for cuprous thiocyanate (CuSCN) are limited, currently mainly DES and DPS. Both DES and DPS are hazardous chemicals with persistent, unpleasant, pungent odors, and their use requires special attention and control, which hinders the application of cuprous thiocyanate (CuSCN).

[0007] In addition, when cuprous thiocyanate (CuSCN) is used in inverted perovskite solar cells with DES or DPS as solvent, the device efficiency can exceed 18%. However, when it is used in the hole transport layer of OSCs, the device efficiency is relatively low. Summary of the invention

[0008] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a hole transport layer precursor solution and a preparation method and application thereof.

[0009] In order to achieve the above-mentioned object, the first aspect of the present invention provides a hole transport layer precursor solution, wherein the precursor solution uses cuprous thiocyanate as a solute and a mixed solvent as a solvent;

[0010] Wherein, the mixed solvent comprises a first solvent and a second solvent;

[0011] The first solvent is DMSO or CH3OH; the second solvent is ammonia water or DMF.

[0012] The second aspect of the present invention provides a method for preparing the hole transport layer precursor solution described in the first aspect, wherein the method comprises: dissolving cuprous thiocyanate in a first solvent of the mixed solvent for a first time, and then dissolving it in a second solvent for a second time to obtain the hole transport layer precursor solution.

[0013] The third aspect of the present invention provides a hole transport layer precursor solution obtained by the preparation method described in the second aspect.

[0014] The fourth aspect of the present invention provides a hole transport layer prepared from the hole transport layer precursor solution described in the first aspect or the third aspect.

[0015] The fifth aspect of the present invention provides use of the hole transport layer described in the fourth aspect in preparing an organic solar cell.

[0016] A sixth aspect of the present invention provides an organic solar cell comprising the hole transport layer described in the fourth aspect.

[0017] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0018] (1) The hole transport layer precursor solution provided by the present invention uses a specific mixed solvent as a solvent, and the preparation method is simple, low-cost, and mild conditions.

[0019] (2) The hole transport layer prepared by the hole transport layer precursor solution of the present invention has a clear structure, and the prepared organic solar cell has higher energy conversion efficiency, short-circuit current density and fill factor, and has high PCE stability.

[0020] (3) Under preferred conditions, the hole transport layer provided by the present invention has a higher work function, thereby promoting the effective collection of holes and making the prepared organic solar cell have a higher open circuit voltage. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 XRD spectrum of the hole transport layer film prepared in Example 1 of the present invention;

[0022] Figure 2 XRD spectrum of the hole transport layer film prepared in Example 2 of the present invention;

[0023] Figure 3 UPS spectrum of the hole transport layer film prepared in Example 1 of the present invention;

[0024] Figure 4 UPS spectrum of the hole transport layer film prepared in Example 2 of the present invention;

[0025] Figure 5 XPS Cu spectra of the hole transport layer films prepared in Examples 1-2 of the present invention and Comparative Example 1;

[0026] Figure 6 The JV curve of the organic solar cell prepared in Application Example 1 of the present invention;

[0027] Figure 7 The JV curve of the organic solar cell prepared in Application Example 2 of the present invention;

[0028] Figure 8 The JV curve of the organic solar cell prepared in Application Example 3 of the present invention;

[0029] Fig. 9 The JV curve of the organic solar cell prepared in Application Example 4 of the present invention;

[0030] Fig.10 The JV curve of the organic solar cell prepared in Application Example 5 of the present invention;

[0031] Fig.11 The JV curve of the organic solar cell prepared in Application Example 6 of the present invention;

[0032] Fig.12 The JV curve of the organic solar cell prepared in Application Example 7 of the present invention;

[0033] Fig.13 The JV curve of the organic solar cell prepared by comparative example 1 of the present invention;

[0034] Fig.14The stability test curves of the organic solar cells prepared by Application Examples 1-2 and Comparative Example 2 of the present invention are shown. DETAILED DESCRIPTION

[0035] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0036] The first aspect of the present invention provides a hole transport layer precursor solution, wherein the precursor solution contains cuprous thiocyanate as a solute and a mixed solvent as a solvent;

[0037] Wherein, the mixed solvent comprises a first solvent and a second solvent;

[0038] The first solvent is DMSO or CH3OH; the second solvent is ammonia water or DMF.

[0039] The present invention can avoid the problem of application limitation caused by the harmfulness of the existing solvents DES and DPS by specifically selecting the solvent of cuprous thiocyanate, so as to make the application range of cuprous thiocyanate wider. In addition, when the hole transport layer prepared by the hole transport layer precursor solution of the present invention is applied to an organic solar cell, higher energy conversion efficiency, short-circuit current density, fill factor and stability can be obtained.

[0040] In some embodiments of the present invention, the mixed solvent is selected from DMSO: ammonia water, DMSO: DMF and CH3OH: ammonia water, preferably DMSO: DMF.

[0041] In some embodiments of the present invention, the mass concentration of the cuprous thiocyanate is 10-25 mg / mL, such as 10 mg / mL, 11 mg / mL, 12 mg / mL, 13 mg / mL, 14 mg / mL, 15 mg / mL, 16 mg / mL, 17 mg / mL, 18 mg / mL, 19 mg / mL, 20 mg / mL, 21 mg / mL, 22 mg / mL, 23 mg / mL, 24 mg / mL, 25 mg / mL, and any value within the range of any two of the above values, preferably 10-20 mg / mL, more preferably 15-20 mg / mL. In the present invention, if the mass concentration of cuprous thiocyanate is too low, it will affect the device performance. The hole transport layer film formed by too low concentration will be very thin and may not be able to completely cover ITO, resulting in leakage (device malfunction); if the concentration is too high, it is difficult to dissolve, and the temperature needs to be increased, which makes the preparation process complicated.

[0042] In some embodiments of the present invention, the concentration of the aqueous ammonia is 25-28 wt %.

[0043] In the present invention, the purity of DMSO, CH3OH and DMF can be selected to be 99.5% or more.

[0044] In some embodiments of the present invention, in the mixed solvent, the volume ratio of DMSO to ammonia water is 1:0.1-0.4, preferably 1:0.25.

[0045] In some embodiments of the present invention, in the mixed solvent, the volume ratio of DMSO to DMF is 1:0.5-1.2, for example 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, and any value within the range of any two of the above values, preferably 1:0.8-1.

[0046] In some embodiments of the present invention, in the mixed solvent, the volume ratio of CH3OH to ammonia water is 1:0.1-0.4, preferably 1:0.25.

[0047] In the present invention, the above volume ratio is within a specific range. A volume ratio that is too low will affect the dissolution effect, and a volume ratio that is too high will affect the device efficiency.

[0048] The second aspect of the present invention provides a method for preparing the hole transport layer precursor solution described in the first aspect, wherein the method comprises: dissolving cuprous thiocyanate in a first solvent of the mixed solvent for a first time, and then dissolving it in a second solvent for a second time to obtain the hole transport layer precursor solution.

[0049] The present invention can obtain a uniform and stable solution through the method.

[0050] In some embodiments of the present invention, when the first solvent is DMSO, the first dissolution conditions include: stirring; a dissolution temperature of 80-120° C.; and a dissolution time of 2-4 h.

[0051] In some embodiments of the present invention, when the first solvent is CH3OH, the first dissolution conditions include: stirring; room temperature.

[0052] In some embodiments of the present invention, when the second solvent is aqueous ammonia, the second dissolution conditions include: stirring or shaking; room temperature.

[0053] In some embodiments of the present invention, when the second solvent is DMF, the second dissolution conditions include: stirring; and a dissolution temperature of 80-120°C.

[0054] In some embodiments of the present invention, the preparation method further comprises: after the second dissolution, filtering to obtain the hole transport layer precursor solution.

[0055] In some embodiments of the present invention, the filtration is performed using a filter membrane with a pore size no greater than 0.45 μm.

[0056] In the present invention, the purpose of filtering is to remove the incompletely dissolved cuprous thiocyanate or impurities to ensure a higher device efficiency.

[0057] The third aspect of the present invention provides a hole transport layer precursor solution obtained by the preparation method described in the second aspect.

[0058] The fourth aspect of the present invention provides a hole transport layer prepared from the hole transport layer precursor solution described in the first aspect or the third aspect.

[0059] In the present invention, the hole transport layer can be prepared by the following method: spin coating the hole transport layer precursor solution on ITO, and annealing to obtain the hole transport layer. The annealing temperature can be selected to be 60° C., and the annealing time can be selected to be 15 minutes.

[0060] The fifth aspect of the present invention provides use of the hole transport layer described in the fourth aspect in preparing an organic solar cell.

[0061] A sixth aspect of the present invention provides an organic solar cell comprising the hole transport layer described in the fourth aspect.

[0062] The present invention will be described in detail below through examples.

[0063] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0064] Example 1

[0065] This example is used to illustrate a method for preparing a cuprous thiocyanate hole transport layer (CuSCN (DMSO:DMF)) using DMSO:DMF as a mixed solvent.

[0066] (1) Add 7 mg of cuprous thiocyanate to 195 μL of DMSO and stir at 120 °C for 3 h;

[0067] (2) adding 155 μL of DMF (the volume ratio of DMSO to DMF is 1:0.8) to the solution obtained in step (1), and continuing to stir at 120° C. to obtain a black solution; wherein the mass concentration of cuprous thiocyanate is 20 mg / mL;

[0068] (3) filtering the solution obtained in step (2) through a 0.45 μm nylon filter membrane;

[0069] (4) Spin-coat the solution obtained in step (3) on ITO and anneal at 60° C. for 15 min to form a cuprous thiocyanate hole transport layer.

[0070] Example 2

[0071] This example is used to illustrate a method for preparing a cuprous thiocyanate hole transport layer (CuSCN (CH3OH: ammonia)) using CH3OH: ammonia as a mixed solvent.

[0072] (1) Take 7 mg of cuprous thiocyanate and put it into a 2 mL vial. Add 280 μL of methanol and stir to dissolve.

[0073] (2) Add 70 μL of aqueous ammonia (25%) (the volume ratio of methanol to aqueous ammonia is 1:0.25) to the vial in step (1), and stir or shake at room temperature until cuprous thiocyanate is completely dissolved;

[0074] (3) filtering the solution obtained in step (2) through a 0.45 μm nylon filter membrane; wherein the mass concentration of cuprous thiocyanate is 20 mg / mL;

[0075] (4) Spin-coat the solution obtained in step (3) on ITO and anneal at 60° C. for 15 min to form a cuprous thiocyanate hole transport layer.

[0076] Example 3

[0077] This example is used to illustrate a method for preparing a cuprous thiocyanate hole transport layer (CuSCN (DMSO: ammonia)) using DMSO: ammonia as a mixed solvent.

[0078] (1) Take 7 mg of cuprous thiocyanate and put it in a 2 mL vial. Add 280 μL of DMSO and stir at 120 °C for 2 h.

[0079] (2) Add 70 μL of 25% ammonia water (the volume ratio of DMSO to ammonia water is 1:0.25) to the vial in step (1), and stir or shake at room temperature until cuprous thiocyanate is completely dissolved;

[0080] (3) filtering the solution obtained in step (2) through a 0.45 μm nylon filter membrane; wherein the mass concentration of cuprous thiocyanate is 20 mg / mL;

[0081] (4) Spin-coat the solution obtained in step (3) on ITO and anneal at 60° C. for 15 min to form a cuprous thiocyanate hole transport layer.

[0082] Example 4

[0083] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that the volume of DMSO was 233 μL, the volume of DMF was 117 μL, and the volume ratio of the two was 1:0.5.

[0084] Example 5

[0085] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that the volume of DMSO was 159 μL, the volume of DMF was 191 μL, and the volume ratio of the two was 1:1.2.

[0086] Example 6

[0087] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that the volume of DMSO was 175 μL, the volume of DMF was 175 μL, and the volume ratio of the two was 1:1.

[0088] Example 7

[0089] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that the volume of DMSO was 389 μL, the volume of DMF was 311 μL, and the mass concentration of cuprous thiocyanate was 10 mg / mL.

[0090] Example 8

[0091] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that the volume of DMSO was 259 μL, the volume of DMF was 208 μL, and the mass concentration of cuprous thiocyanate was 15 mg / mL.

[0092] Example 9

[0093] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that the volume of DMSO was 156 μL, the volume of DMF was 124 μL, and the mass concentration of cuprous thiocyanate was 25 mg / mL.

[0094] Comparative Example 1

[0095] The cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that DES was used as solvent (350 μL) and dissolved by stirring at 60° C. for 3 h.

[0096] Comparative Example 2

[0097] A cuprous thiocyanate hole transport layer was prepared according to the method of Example 1, except that PEDOT:PSS was used as the hole transport layer material.

[0098] Test Example 1

[0099] The solution prepared in step (3) of Examples 1 and 2 was spin-coated on a glass sheet for X-ray diffraction (XRD). The test results are as follows: Figure 1-2 The hole transport layer films prepared in Examples 1, 2 and Comparative Example 1 were subjected to ultraviolet photoelectron spectroscopy (UPS) testing. The test results are shown in FIG. Figure 3-4 The solutions prepared in Examples 1, 2 and Comparative Example 1 were spin-coated on a glass sheet for XPS characterization. The test results are shown in Figure 5 shown.

[0100] Depend on Figure 1 and 2 It can be seen that the hole transport layer film prepared by the present invention has a clear chemical structure. Figure 3 and 4 It can be seen that compared with the hole transport layer obtained by dissolving with DES solvent, the work function (WF) of the hole transport layer prepared in the present invention is higher.

[0101] from Figure 5 It can be seen that part of the monovalent copper in the hole transport layer thin films of Examples 1 and 2 is converted into divalent copper, while no conversion occurs in the hole transport layer thin film of Comparative Example 1. This may be the reason for the change in work function.

[0102] Application Example 1

[0103] This example is used to illustrate the preparation of an organic solar cell.

[0104] (1) Preparation of hole transport layer: A CuSCN hole transport layer was prepared by the method of Example 1;

[0105] (2) Preparation of an organic light-absorbing layer: PM6 and L8-BO were added to chloroform at a mass ratio of 1:1.2 to form a solution with a concentration of 16 mg / mL, and then 14 mg / mL of 1,3-dibromo-5-chlorobenzene was added; the above solution was spin-coated on the CuSCN hole transport layer using a sizing machine, and then annealed at 80°C for 5 min to obtain an organic light-absorbing layer with a thickness of 100 nm;

[0106] (3) Preparation of electron transport layer: 1 mg / mL PDINN was spin-coated on the organic light absorbing layer to form an electron transport layer with a thickness of 5 nm;

[0107] (4) Preparation of top electrode: Vacuum evaporation of metallic silver onto the surface of the electron transport layer to form an anode layer with a thickness of 80 nm, thereby obtaining an organic solar cell.

[0108] Application Example 2

[0109] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 2.

[0110] Application Example 3

[0111] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 3.

[0112] Application Example 4

[0113] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 4.

[0114] Application Example 5

[0115] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 5.

[0116] Application Example 6

[0117] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 6.

[0118] Application Example 7

[0119] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 7.

[0120] Application Example 8

[0121] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 8.

[0122] Application Example 9

[0123] An organic solar cell was prepared according to the method of Application Example 1, except that the CuSCN hole transport layer was prepared using the method of Example 9.

[0124] Application Comparative Example 1

[0125] An organic solar cell was prepared according to the method of Application Example 1, except that a CuSCN hole transport layer was prepared using the method of Comparative Example 1.

[0126] Application Comparative Example 2

[0127] An organic solar cell was prepared according to the method of Application Example 1, except that a hole transport layer was prepared using the method of Comparative Example 2.

[0128] Test Example 2

[0129] The organic solar cells prepared in Example 1-7 and Comparative Example 1 were placed in a standard solar simulator (AM1.5G, 100 mW / cm 2 ) The current density-voltage curve is measured under irradiation conditions, such as Figure 6-13 shown.

[0130] The specific results are shown in Table 1.

[0131] Table 1

[0132]

[0133]

[0134] It can be seen from the results in Table 1 that the organic solar cell prepared by the present invention can obtain higher energy conversion efficiency, short-circuit current density and fill factor. Among them, the application of Example 1 can also obtain a higher open circuit voltage, and the energy conversion efficiency, short-circuit current density and fill factor are also the highest.

[0135] Test Example 3

[0136] The organic solar cells prepared in Example 1-2 and Comparative Example 2 were placed in a 70°C environment and the energy conversion efficiency values ​​were tested at regular intervals. Fig.14 shown.

[0137] from Fig.14 It can be seen that the organic solar cell prepared using Example 1-2 is more stable.

[0138] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A hole transport layer precursor solution, characterized in that: The precursor solution uses cuprous thiocyanate as solute and a mixed solvent as solvent; Wherein, the mixed solvent comprises a first solvent and a second solvent; The first solvent is DMSO or CH3OH; the second solvent is ammonia water or DMF.

2. The precursor solution according to claim 1, wherein The mixed solvent is selected from DMSO: ammonia water, DMSO: DMF and CH3OH: ammonia water, preferably DMSO: DMF; Preferably, the mass concentration of cuprous thiocyanate is 10-25 mg / mL, preferably 10-20 mg / mL, and more preferably 15-20 mg / mL; Preferably, the concentration of the aqueous ammonia is 25-28 wt %.

3. The precursor solution according to claim 1 or 2, wherein: In the mixed solvent, the volume ratio of DMSO to ammonia water is 1:0.1-0.4, preferably 1:0.25; Preferably, in the mixed solvent, the volume ratio of DMSO to DMF is 1:0.5-1:2, preferably 1:0.8-1; Preferably, in the mixed solvent, the volume ratio of CH3OH to aqueous ammonia is 1:0.1-0.4, preferably 1:0.

25.

4. A method for preparing a hole transport layer precursor solution according to any one of claims 1 to 3, characterized in that: The method comprises: performing a first dissolution of cuprous thiocyanate in a first solvent of the mixed solvent, and then performing a second dissolution in a second solvent to obtain the hole transport layer precursor solution.

5. The preparation method according to claim 4, wherein When the first solvent is DMSO, the first dissolution conditions include: stirring; dissolution temperature is 80-120° C.; dissolution time is 2-4 h; Preferably, when the first solvent is CH3OH, the first dissolution conditions include: stirring; room temperature; Preferably, when the second solvent is aqueous ammonia, the second dissolution conditions include: stirring or shaking; room temperature; Preferably, when the second solvent is DMF, the second dissolution conditions include: stirring; and a dissolution temperature of 80-120°C.

6. The preparation method according to claim 4 or 5, wherein: The preparation method further comprises: after performing the second dissolution, filtering to obtain the hole transport layer precursor solution; Preferably, the filtration is performed using a filter membrane with a pore size no greater than 0.45 μm.

7. A hole transport layer precursor solution obtained by the preparation method according to any one of claims 4 to 6.

8. A hole transport layer prepared from the hole transport layer precursor solution according to any one of claims 1 to 4 and 7.

9. Use of the hole transport layer according to claim 8 in preparing an organic solar cell. 10 . An organic solar cell comprising the hole transport layer according to claim 8 .