Laminate and method for producing laminate

By forming a mixed layer and an inorganic layer on the surface of the resin layer and laminating it, the problem of insufficient adhesion between layers is solved, and excellent adhesion between layers is achieved.

CN118900765APending Publication Date: 2024-11-05FUJIFILM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280093717.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2022-11-14
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

There is room for improvement in the adhesion between the conventional laminated body between the base material and the metal oxide film, especially the problem of insufficient adhesion between layers.

Method used

The plasma chemical vapor deposition method is used to form a mixed layer and an inorganic layer on the surface of the resin layer, and the laminates are laminated to improve the adhesion between layers. The specific process includes forming a mixing on the first resin layer and the second resin layer in sequence. The layer and the inorganic layer are stacked, or a contrast layer is formed on the resin layer and stacked.

Benefits of technology

The interlayer adhesion is significantly improved, ensuring the continuity and low porosity of the inorganic layer. The thickness of the mixed layer or the contrast layer is in the range of 1 nm to 30 nm and the surface roughness is below 2 nm, achieving excellent interlayer adhesion. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900765A_ABST
    Figure CN118900765A_ABST
Patent Text Reader

Abstract

Provided are: a laminate which is provided with a first resin layer, an inorganic layer, and a second resin layer, and which is provided with a mixed layer between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer; and a method for producing the laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminate and a method for producing the laminate. Background Art

[0002] As a method for laminating laminated bodies including a substrate and an inorganic layer such as a metal oxide provided on the surface of the substrate, there is known a method of activating and bonding the surface of the inorganic layer.

[0003] For example, Japanese Patent Publication No. 2019-119086 discloses a method of forming a metal oxide film on the surface of a substrate by sputtering, making a laminate, and bonding the metal oxide films of two laminates to each other. According to the above method, since no adhesive or the like is required, the thickness of the obtained laminate can be reduced, and the manufacturing cost can be reduced. Summary of the invention

[0004] Technical issues to be solved by the invention

[0005] Recently, the present inventors have newly obtained the following knowledge: although the laminate produced by the method disclosed in Japanese Patent Application Laid-Open No. 2019-119086 has excellent adhesion between metal oxide films, there is room for improvement in the adhesion between the substrate and the metal oxide film.

[0006] An object of one embodiment of the present invention is to provide a laminate having excellent interlayer adhesion and a method for producing the laminate.

[0007] Means for solving technical problems

[0008] The present invention includes the following aspects.

[0009] <1> A laminate comprising a first resin layer, an inorganic layer, and a second resin layer, and

[0010] A mixed layer is provided between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer.

[0011] <2> The laminate according to <1> above, wherein

[0012] The above-mentioned inorganic layer is a continuous layer.

[0013] <3> The laminate according to <1> or <2> above, wherein

[0014] The inorganic layer has a porosity of 25% or less.

[0015] <4> The laminate according to any one of <1> to <3> above, wherein

[0016] The thickness of the mixed layer is 1 nm to 30 nm.

[0017] <5> The laminate according to any one of <1> to <4> above, wherein

[0018] The inorganic layer contains one or more inorganic materials selected from the group consisting of silicon oxide, silicon nitride, aluminum oxide, and aluminum nitride.

[0019] <6> The laminate according to any one of <1> to <5> above, wherein

[0020] The inorganic layer contains silicon dioxide.

[0021] <7> The laminate according to any one of <1> to <6> above, wherein

[0022] The thickness of the inorganic layer is 5 nm or less.

[0023] <8> A laminate comprising a first resin layer and a second resin layer,

[0024] A contrast layer containing an inorganic material is provided between the first resin layer and the second resin layer.

[0025] The cross section of the stack was irradiated with an electron beam for 10 minutes at a voltage of 300 kV using a transmission electron microscope to obtain a cross-sectional image of the test piece after electron beam irradiation. The concentration measured by image analysis software decreased from the inside of the contrast layer in the cross-sectional image toward the surface.

[0026] <9> A method for producing a laminate, comprising the following steps:

[0027] Forming a mixed layer and an inorganic layer in sequence on the surfaces of the first resin layer and the second resin layer respectively by plasma chemical vapor deposition to obtain a first laminate having the first resin layer, the mixed layer and the inorganic layer and a second laminate having the second resin layer, the mixed layer and the inorganic layer; and

[0028] The inorganic layer of the first stacked body and the inorganic layer of the second stacked body are stacked.

[0029] <10> The method for producing a laminate according to <9>, wherein forming the mixed layer and the inorganic layer on the first resin layer and the second resin layer and laminating the first laminate and the second laminate are performed simultaneously.

[0030] <11> The method for producing a laminate according to <9> or <10>, wherein:

[0031] The surface roughness Ra of the inorganic layer of the first stack and the inorganic layer of the second stack is 2 nm or less.

[0032] <12> A method for producing a laminate, comprising the following steps:

[0033] Forming a contrast layer on the surface of each of the first resin layer and the second resin layer by plasma chemical vapor deposition to obtain a first laminate having the first resin layer and the contrast layer and a second laminate having the second resin layer and the contrast layer; and

[0034] The contrast layer of the first laminate and the contrast layer of the second laminate are laminated.

[0035] <13> The method for producing a laminate according to <9>, wherein forming the contrast layer on the first resin layer and the second resin layer and laminating the first laminate and the second laminate are performed simultaneously.

[0036] <14> The method for producing a laminate according to <9> or <10>, wherein:

[0037] The contrast layer of the first laminate and the contrast layer of the second laminate have a surface roughness Ra of 2 nm or less.

[0038] Effects of the Invention

[0039] According to one embodiment of the present invention, a laminate having excellent interlayer adhesion and a method for producing the laminate can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a schematic cross-sectional view showing one embodiment of the laminated body according to the first embodiment.

[0041] Figure 2 This is a schematic cross-sectional view showing one embodiment of the laminated body according to the first embodiment.

[0042] Figure 3 This is a schematic diagram showing one embodiment of an apparatus that can be used to produce the laminated body according to the first embodiment and the laminated body according to the second embodiment.

[0043] Figure 4 This is a schematic diagram showing one embodiment of an apparatus that can be used to produce the laminated body according to the first embodiment and the laminated body according to the second embodiment.

[0044] Figure 5 This is a schematic diagram showing one embodiment of an apparatus that can be used to produce the laminated body according to the first embodiment and the laminated body according to the second embodiment. DETAILED DESCRIPTION

[0045] Hereinafter, embodiments of the present invention will be described in detail. The present invention is not limited to the following embodiments. The following embodiments can be appropriately modified within the scope of the purpose of the present invention.

[0046] In the present invention, the numerical range represented by "~" represents a range including the numerical value recorded before "~" as the lower limit and the numerical value recorded before "~" as the upper limit. In the numerical range recorded in stages in the present invention, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present invention, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiment.

[0047] In the present invention, each component may also include a plurality of corresponding substances. When a plurality of substances corresponding to each component are present in the composition, unless otherwise specified, the content or content of each component represents the total content or total content of the plurality of substances present in the composition.

[0048] In the present invention, when observing a region where the layer or film exists, the term "layer" or "film" includes not only a case where the layer or film is formed on the entire region, but also a case where the layer or film is formed on only a part of the region.

[0049] In the present invention, the term "laminate" means laminating layers, and two or more layers may be bonded or detachable.

[0050] In the present invention, “(meth)acryloyl” means at least one of acryloyl and methacryloyl, and “(meth)acrylic acid” means at least one of acrylic acid and methacrylic acid.

[0051] In the present invention, the term "step" includes not only an independent step but also a step that cannot be clearly distinguished from other steps as long as the intended purpose can be achieved.

[0052] In the present invention, the thickness of each layer is measured based on a cross-sectional image obtained by a method for confirming the presence of a mixed layer described later.

[0053] In the present invention, when the embodiments are described with reference to the drawings, the structure of the embodiments is not limited to the structure shown in the drawings. In addition, the sizes of the components in the drawings are conceptual, and the relative relationship between the sizes of the components is not limited thereto.

[0054] [Laminate according to the first embodiment]

[0055] like Figure 1As shown, the laminated body 10 according to the first embodiment includes a first resin layer 11 , an inorganic layer 12 , and a second resin layer 13 , and includes a mixed layer 14 between the first resin layer 11 and the inorganic layer 12 and between the second resin layer 13 and the inorganic layer 12 .

[0056] like Figure 1 As shown in FIG. 1 , the laminated body 10 according to the first embodiment may include a support body 15 on the outermost surface thereof.

[0057] The laminated body according to the first embodiment is excellent in interlayer adhesion. The reason why the first laminated body exhibits the above-mentioned effect is not clear, but is presumed as follows.

[0058] It is speculated that the stacked body involved in the first embodiment has a mixed layer between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer, in which the materials constituting these layers are mixed. Since the above-mentioned mixed layer has excellent adhesion with the first resin layer and the inorganic layer and with the second resin layer and the inorganic layer, the adhesion between the layers is improved.

[0059] The first resin layer, the mixed layer, the inorganic layer, the mixed layer, and the second resin layer included in the laminate according to the first embodiment are preferably provided continuously.

[0060] In the present invention, "continuously disposed" means that no other layer exists between layers (that is, no interface exists).

[0061] like Figure 2 As shown, the laminated body 20 involved in the first embodiment may include a mixed layer 23, an inorganic layer 24, a mixed layer 23, and a third resin layer 25 on the surface of the second resin layer 22. In addition, a structure consisting of a mixed layer, an inorganic layer, a mixed layer, and an nth resin layer may be repeatedly provided on the surface of the third resin layer (not shown).

[0062] In addition, Figure 2 In the figure, the first resin layer is indicated by reference numeral 21 and the support is indicated by reference numeral 26 .

[0063] (First resin layer and second resin layer)

[0064] The first resin layer and the second resin layer (hereinafter collectively referred to as resin layers) may contain resins such as epoxy resin, (meth) acrylic resin, liquid crystal polymer, polyester resin, polystyrene resin, fluororesin, polyimide resin, polyamide resin, polyamideimide resin, polyetherimide resin, cellulose resin, polyurethane resin, polyether ketone resin, and polycarbonate resin.

[0065] Also, the resin layer may include a reactant of a (meth)acrylic monomer and a photopolymerization initiator.

[0066] The resin layer may have a single-layer structure or a multi-layer structure. When the resin layer has a multi-layer structure, the structures of the layers may be the same or different.

[0067] As the (meth)acrylic acid monomer, a monomer represented by the following general formula can be used.

[0068] [Chemical formula 1]

[0069]

[0070] In the general formula, R 1 represents a substituent, and each of them may be the same or different. k represents an integer of 0 to 5, and each of them may be the same or different. 1 At least one of the compounds comprises a polymerizable group.

[0071] As R 1 The substituents include -CR 2 2-(R 2 represents a hydrogen atom or a substituent. ), -CO-, -O-, phenylene, -S-, -C≡C-, -NR 3 -(R 3 represents a hydrogen atom or a substituent. ), -CR 4 =CR 5 -(R 4 , R 5 Each represents a hydrogen atom or a substituent. A group consisting of a combination of one or more of ) and a polymerizable group is preferably -CR 2 A group consisting of a combination of one or more of -2-, -CO-, -O- and phenylene and a polymerizable group.

[0072] R 2 Preferred is a hydrogen atom or a hydroxyl group.

[0073] From the viewpoint of curability, it is preferred that at least one R 1 Contains hydroxyl groups.

[0074] At least 1 R 1 The molecular weight is preferably 10-250, more preferably 70-150.

[0075] R 1 The bonding position is preferably para.

[0076] k represents an integer of 0 to 5, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 1 in both cases.

[0077] The compound represented by the above general formula is preferably 1 At least two of them have the same structure.

[0078] Furthermore, it is more preferable that n is 1 and 4 R 1 Each 2 of them have the same structure, and more preferably n is 1, 4 R 1 The same structure.

[0079] The polymerizable group is preferably a (meth)acryloyl group or an epoxy group, and more preferably a (meth)acryloyl group.

[0080] The number of polymerizable groups is preferably 2 or more, more preferably 3 or more.

[0081] Furthermore, the upper limit of the number of polymerizable groups is not particularly limited, but is preferably 8 or less, and more preferably 6 or less.

[0082] The molecular weight of the compound represented by the above general formula is preferably 600 to 1,400, more preferably 800 to 1,200.

[0083] Specific examples of the compound represented by the above general formula are shown below, but the present invention is not limited thereto.

[0084] In the following compounds, n represents an integer of 0 to 5, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 1 in both cases.

[0085] [Chemical formula 2]

[0086]

[0087] [Chemical formula 3]

[0088]

[0089] As the photopolymerization initiator, conventionally known photopolymerization initiators can be used, and examples thereof include α-carbonyl compounds, acyloin ether compounds, α-hydrocarbon-substituted aromatic acyloin compounds, polynuclear quinone compounds, a combination of a triaryl imidazole dimer and p-aminophenyl ketone, acridine compounds, phenazine compounds, oxadiazole compounds, acylphosphine oxide compounds, and the like.

[0090] The content of the resin relative to the total mass of the resin layer is not particularly limited, and may be 50 to 100 mass %, 70 to 95 mass %, or 80 to 90 mass %.

[0091] The resin layer may contain additives such as a pigment, a dye, an ultraviolet absorber, a light stabilizer, an antioxidant, and wax.

[0092] From the viewpoint of interlayer adhesion, the thickness of the resin layer is preferably 0.05 μm to 50 μm, more preferably 0.1 μm to 20 μm, and even more preferably 0.5 μm to 10 μm.

[0093] The materials such as resin contained in the first resin layer and the second resin layer may be the same or different.

[0094] Furthermore, the thicknesses of the first resin layer and the second resin layer may be the same or different.

[0095] In addition, when the laminated body involved in the first embodiment further includes resin layers (third resin layer, fourth resin layer, etc.) in addition to the first resin layer and the second resin layer, the material and thickness of these resin layers may be the same as or different from those of the first resin layer and the second resin layer.

[0096] The resin layer can be formed by applying a resin composition containing the above resins etc. on the surface of the support and drying it. Alternatively, it can be photocured by irradiating with ultraviolet rays, electron beams etc. after drying.

[0097] (Inorganic layer)

[0098] The inorganic layer can contain an inorganic material. Examples of the inorganic material include inorganic oxides, inorganic nitrides, metal oxides, and metal nitrides.

[0099] Examples of the inorganic oxide include silicon oxide and boron oxide.

[0100] Examples of the inorganic nitride include silicon nitride and boron nitride.

[0101] Examples of the metal oxide include aluminum oxide, titanium oxide, iron oxide, copper oxide, chromium oxide, magnesium oxide, and zirconium oxide.

[0102] Examples of the metal nitride include aluminum nitride, titanium nitride, iron nitride, copper nitride, chromium nitride, magnesium nitride, and zirconium nitride.

[0103] As described above, from the viewpoint of interlayer adhesion, the inorganic layer preferably contains one or more inorganic materials selected from the group consisting of silicon oxide, silicon nitride, aluminum oxide and aluminum nitride, and more preferably contains one or more inorganic materials selected from the group consisting of silicon oxide and silicon nitride.

[0104] From the viewpoint of interlayer adhesion, the inorganic layer preferably contains silicon oxide, and more preferably contains silicon dioxide.

[0105] From the viewpoint of interlayer adhesion, the content of the inorganic material relative to the total mass of the inorganic layer is preferably 50 to 100 mass %, more preferably 70 to 95 mass %, and even more preferably 80 to 90 mass %.

[0106] The inorganic layer is preferably a continuous layer. In the present invention, the continuous layer refers to a layer having a porosity of 50% or less in the inorganic layer. In the present invention, the pores do not include defects.

[0107] From the viewpoint of interlayer adhesion, the porosity of the inorganic layer is preferably 25% or less, and more preferably 10% or less. The lower limit of the porosity of the inorganic layer is not particularly limited, and may be 0%.

[0108] In the present invention, the porosity is measured as follows.

[0109] First, a cross-sectional image obtained by a method for confirming the presence of a mixed layer described later is prepared.

[0110] In the inorganic layer forming part of the cross-sectional image, the area S0 of the portion having a concentration of 0 to 50 and a length of 2 nm or more in the thickness direction is obtained, and the porosity of the inorganic layer is obtained by dividing it by the area S1 of the entire inorganic layer forming part and multiplying the result by 100.

[0111] Furthermore, even in a portion where the concentration is 0 to 50, if the length in the thickness direction is less than 2 nm, it is not a void.

[0112] Furthermore, when the laminated body according to the first embodiment includes a plurality of inorganic layers, the materials and thicknesses of the respective inorganic layers may be the same or different.

[0113] From the viewpoint of interlayer adhesion, the thickness of the inorganic layer is preferably below 30nm, more preferably below 28nm, further preferably below 23nm, and particularly preferably below 5nm. Furthermore, by having the thickness of the inorganic layer be below 30nm, the decrease in interlayer adhesion caused by bending the laminate or applying force can be suppressed.

[0114] From the viewpoint of interlayer adhesion, the thickness of the inorganic layer is preferably 1 nm or more, and more preferably 2 nm or more.

[0115] The thickness of the inorganic layer is preferably 1 nm to 30 nm, more preferably 1 nm to 28 nm, further preferably 1 nm to 23 nm, and particularly preferably 2 nm to 5 nm.

[0116] The thickness of the inorganic layer can be adjusted by changing the feeding speed of the resin layer, the flow rate of the raw materials and oxygen used in forming the inorganic layer and the mixed layer, the peak voltage, etc. in the method for producing the laminate described below.

[0117] (Mixed Layer)

[0118] The laminate according to the first embodiment includes a mixed layer between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer. The mixed layer is formed when the inorganic layer is formed on the surface of the first resin layer or the second resin layer, and its presence is confirmed by the following method.

[0119] The laminated body according to the first embodiment was cut into a size of 3 mm in length×3 mm in width to prepare a process test piece A.

[0120] The test piece A was placed in a transmission electron microscope, and an electron beam was irradiated on a cross section in the thickness direction of the test piece for 10 minutes under the condition of a voltage of 300 kV.

[0121] A cross-sectional image (magnification: 1,000,000) of the test piece A after electron beam irradiation was obtained, and the density of the cross-sectional image was measured using image analysis software.

[0122] When the concentration of the most concentrated part (inorganic layer part) in the above cross-sectional image is set to 100 and the concentration of the least concentrated part (first resin layer part and second resin layer part) is set to 0, it is confirmed that there is a part with a concentration of 10 to 90 between the inorganic layer and the resin layer (in the thickness direction). If this can be confirmed, it is considered that a mixed layer exists.

[0123] In one embodiment, the test piece A can be buried in a molten resin, and then the resin is irradiated with light to be cured to form a cured product A, which is cut into a 20 nm thick test piece B, and the cross section of the test piece B in the thickness direction is irradiated with an electron beam.

[0124] As a transmission electron microscope, JEM-2011 manufactured by JEOL Ltd. or an apparatus equivalent thereto can be used.

[0125] Furthermore, the concentration in the cross-sectional image is confirmed using image analysis software Image J or equivalent software.

[0126] Furthermore, as the above-mentioned resin, trimethylolpropane triacrylate can be used.

[0127] The mixed layer preferably contains the resin contained in the resin layer and the inorganic material contained in the inorganic layer.

[0128] From the viewpoint of interlayer adhesion, the content of the resin relative to the total mass of the mixed layer is preferably 5 to 90 mass %, more preferably 20 to 80 mass %, and further preferably 30 to 70 mass %.

[0129] From the viewpoint of interlayer adhesion, the content of the inorganic material relative to the total mass of the mixed layer is preferably 10 to 95 mass %, more preferably 20 to 80 mass %, and even more preferably 30 to 70 mass %.

[0130] From the perspective of interlayer adhesion and suppressing the decrease in interlayer adhesion caused by bending the stack or applying force, the thickness of the mixed layer is preferably 1nm to 30nm, more preferably 2nm to 25nm, further preferably 2nm to 20nm, and especially preferably 3nm to 15nm.

[0131] The thickness of the mixed layer can be adjusted by changing the feeding speed of the resin layer, the flow rate of raw materials and oxygen used in forming the inorganic layer and the mixed layer, the peak voltage, etc. in the method for producing the laminate described below.

[0132] <Support body>

[0133] The support may contain a resin such as a polyester resin, a polyolefin resin, a polystyrene resin, a polyamide resin, a polycarbonate resin, a polyimide resin, a polyamideimide resin, or a (meth)acrylic resin.

[0134] Furthermore, the support may contain the above-mentioned additives.

[0135] The support may have a single-layer structure or a multi-layer structure. When the support has a multi-layer structure, the structures of the layers may be the same or different.

[0136] The thickness of the support is not particularly limited, and can be, for example, 10 μm to 500 μm.

[0137] As the support, one produced by a conventionally known method may be used, or a commercially available support may be used.

[0138] The laminated body according to the first embodiment can be produced by the method for producing the laminated body according to the first embodiment described below.

[0139] <Laminate according to Second Embodiment>

[0140] The second embodiment involves a laminate having a first resin layer and a second resin layer, wherein a contrast layer containing an inorganic material is provided between the first resin layer and the second resin layer. A cross-section of the laminate is irradiated with an electron beam for 10 minutes under a transmission electron microscope at a voltage of 300 kV to obtain a cross-sectional image of the test piece after electron beam irradiation. The concentration measured by image analysis software decreases from the inside of the contrast layer toward the surface of the cross-sectional image.

[0141] In the present invention, the surface of the comparative layer refers to a range of 2 nm from the surface in the thickness direction as the "surface".

[0142] Also, in the present invention, the interior of the contrast layer refers to a portion excluding the surface of the contrast layer.

[0143] The laminated body according to the second embodiment may include a support body on the outermost surface thereof.

[0144] The laminated body according to the second embodiment may further include a contrast layer and a third resin layer on the surface of the second resin layer. Also, a structure including a contrast layer and an n-th resin layer may be repeatedly provided on the surface of the third resin layer.

[0145] The resin layer and the support are the same as those of the laminated body according to the first embodiment, and thus description thereof is omitted here.

[0146] (Contrast layer)

[0147] The laminated body according to the second embodiment includes contrast layers between resin layers.

[0148] In the present invention, the contrast layer refers to a layer whose concentration measured by image analysis software decreases from the inside toward the surface of the contrast layer in a cross-sectional image obtained by a transmission electron microscope.

[0149] The presence of the contrast layer was confirmed as follows.

[0150] The laminated body according to the second embodiment was cut into a size of 3 mm in length×3 mm in width to prepare a test piece a.

[0151] The test piece a was placed in a transmission electron microscope, and an electron beam was irradiated on a cross section in the thickness direction of the test piece for 10 minutes under the condition of a voltage of 300 kV.

[0152] A cross-sectional image (magnification: 1,000,000) of the test piece a after electron beam irradiation was obtained.

[0153] The concentration data of the contrast layer is obtained from the cross-sectional image, and it is confirmed whether the concentration decreases from the inside of the contrast layer toward the surface.

[0154] In one embodiment, the test piece a can be buried in a molten resin, and then the resin is irradiated with light to be cured to form a cured product a, which is cut into a thickness of 20 nm to form a test piece b, and the cross section of the test piece b in the thickness direction is irradiated with an electron beam.

[0155] As a transmission electron microscope, JEM-2011 manufactured by JEOL Ltd. or an apparatus equivalent thereto can be used.

[0156] Furthermore, the concentration in the cross-sectional image is confirmed using image analysis software Image J or equivalent software.

[0157] Furthermore, as the above-mentioned resin, trimethylolpropane triacrylate can be used.

[0158] When the maximum concentration inside the contrast layer measured by image analysis software is set to 100 and the concentrations of the first resin layer and the second resin layer are set to 0, the contrast layer preferably has a concentration that decreases by 3 to 50 per nm from the inside toward the surface, and more preferably by 10 to 35 per nm.

[0159] The contrast layer is formed when an inorganic layer is formed on the surface of the first resin layer or the second resin layer, and may include the inorganic layer and the mixed layer, or may include only the mixed layer. The inorganic layer and the mixed layer are as described above, so they are omitted here.

[0160] From the viewpoint of interlayer adhesion, the thickness of the contrast layer is preferably 1 nm to 30 nm, more preferably 2 nm to 20 nm, further preferably 2 nm to 15 nm, and particularly preferably 2 nm to 10 nm.

[0161] The laminated body according to the second embodiment can be produced by a method for producing a laminated body to be described later.

[0162] The laminated body according to the first embodiment and the laminated body according to the second embodiment can be applied to electronic devices such as organic EL (Electroluminescence) displays, organic EL lighting, organic solar cells, CIGS (Copperindium gallium selenide) solar cells, and optical devices such as AR glasses.

[0163] <Method for producing laminate according to first embodiment>

[0164] The method for manufacturing a laminate according to the first embodiment includes the following steps: forming a mixed layer and an inorganic layer in sequence on the surfaces of a first resin layer and a second resin layer by plasma chemical vapor deposition to obtain a first laminate having a first resin layer, a mixed layer and an inorganic layer and a second laminate having a second resin layer, a mixed layer and an inorganic layer (hereinafter also referred to as a step of forming a mixed layer and an inorganic layer); and

[0165] A step of laminating the inorganic layer of the first laminate and the inorganic layer of the second laminate (hereinafter also referred to as a lamination step).

[0166] According to the method for producing a laminated body according to the first embodiment, a laminated body having excellent interlayer adhesion can be produced. The reason why the above-mentioned effect is exerted is not clear, but it is presumed as follows.

[0167] In the method for manufacturing the laminated body according to the first embodiment, the inorganic layer is formed on the first resin layer and the second resin layer by plasma chemical vapor deposition, thereby forming the mixed layer. It is presumed that this is because the surfaces of the first resin layer and the second resin layer are etched by plasma chemical vapor deposition, and the inorganic material for forming the inorganic layer intrudes into the etched portion, thereby forming the mixed layer.

[0168] In addition, it is speculated that the above-mentioned mixed layer has excellent adhesion with the first resin layer and the inorganic layer, and excellent adhesion with the second resin layer and the inorganic layer, and the inorganic layer formed by the plasma chemical vapor deposition method is surface activated, and the adhesion between the inorganic layers is also excellent by stacking the inorganic layers. Therefore, the interlayer adhesion of the stacked body manufactured by the manufacturing method of the stacked body involved in the first embodiment is excellent.

[0169] The method for producing the laminated body according to the first embodiment may repeat the steps of forming the mixed layer and the inorganic layer and the laminating step a plurality of times.

[0170] For example, the method for manufacturing a laminated body according to the first embodiment includes the following steps: forming a mixed layer and an inorganic layer in sequence on the surfaces of the second resin layer of the manufactured laminated body and the third resin layer prepared separately by plasma chemical vapor deposition, thereby obtaining a third laminated body including a first resin layer, a mixed layer, an inorganic layer, a mixed layer, a second resin layer, a mixed layer and an inorganic layer, and a fourth laminated body including a third resin layer, a mixed layer and an inorganic layer; and

[0171] The inorganic layer included on the outermost surface of the third stack and the inorganic layer of the fourth stack are stacked.

[0172] (Step of forming a mixed layer and an inorganic layer)

[0173] The manufacturing method of the stacked body involved in the first embodiment includes the following steps: a mixed layer and an inorganic layer are formed in sequence on the surfaces of the first resin layer and the second resin layer respectively by plasma chemical vapor deposition (hereinafter also referred to as plasma CVD method), thereby obtaining a first stacked body comprising the first resin layer, the mixed layer and the inorganic layer and a second stacked body comprising the second resin layer, the mixed layer and the inorganic layer.

[0174] The details of the first resin layer, the second resin layer, the mixed layer, and the inorganic layer are as described above, and therefore description thereof is omitted here.

[0175] The mixed layer and the inorganic layer are formed on the resin layer by a plasma chemical vapor deposition method. More specifically, the mixed layer and the inorganic layer can be formed by the following method: oxygen containing raw materials for forming the inorganic layer such as silane and the mixed layer is put into a plasma state by using plasma excitation power, and the surface of the resin layer is plasma-treated using the oxygen in the plasma state.

[0176] Examples of the plasma treatment method include a method of irradiating the surface of the resin layer with plasma using a plasma irradiation device and a method of passing the resin layer between an electrode roll and a backup roll in the above-mentioned oxygen atmosphere.

[0177] In addition to the oxygen gas contained in the raw material, hydrogen gas, a gas containing nitrogen atoms, an inert gas, or the like can also be used.

[0178] Examples of the gas containing nitrogen atoms include nitrogen gas (N2), ammonia gas (NH3), and nitrous gas (N2O).

[0179] Examples of the inert gas include helium, neon, argon, krypton, xenon, and radon.

[0180] From the viewpoint of forming a mixed layer and an inorganic layer on the surface of the resin layer and improving the adhesion between the layers, the flow rate of oxygen is preferably 30 mL / min to 350 mL / min, more preferably 40 mL / min to 300 mL / min, and further preferably 50 mL / min to 250 mL / min.

[0181] From the viewpoint of forming a mixed layer and an inorganic layer on the surface of the resin layer and improving interlayer adhesion, the flow rate of the raw material is preferably 2 to 17 mg / min, more preferably 3 to 15 mg / min, and even more preferably 4 to 10 mg / min.

[0182] From the perspective of interlayer adhesion, the peak voltage of the plasma excitation power used for plasmatizing the raw gas for forming a mixed layer and an inorganic layer on the surface of the resin layer and improving interlayer adhesion is preferably 3 kV to 17 kV, more preferably 4 kV to 15 kV, and further preferably 6 kV to 10 kV.

[0183] In the present invention, the "peak voltage of plasma excitation power" refers to the maximum value of the plasma excitation power when the source gas is converted into plasma.

[0184] (Lamination process)

[0185] The lamination method of the first laminate and the second laminate is not particularly limited, and the lamination can be performed by making the inorganic layer of the first laminate and the inorganic layer of the second laminate face each other and press-bonding them.

[0186] The pressure bonding of the laminated bodies can be performed by overlapping the laminated bodies and passing the laminated bodies between rollers.

[0187] The pressure applied to the laminate by the roller is not particularly limited, and can be, for example, 0.1 MPa to 5 MPa.

[0188] In the method for manufacturing the laminated body involved in the first embodiment, it is preferred that the steps of forming the mixed layer and the inorganic layer on the first resin layer and the second resin layer and laminating the first laminated body and the second laminated body are performed simultaneously. Thus, the steps of forming concavoconvex portions on the surface of the resin layer by etching and allowing the material forming the inorganic layer to intrude into the concavoconvex portions, and laminating the inorganic layers of the laminated body are performed simultaneously, so that the smoothness of the interface between the laminated inorganic layers tends to be improved, and the adhesion between the layers tends to be improved.

[0189] From the viewpoint of interlayer adhesion, the surface roughness Ra of the inorganic layer of the first stack and the inorganic layer of the second stack is preferably 2 nm or less, more preferably 1.5 nm or less. The lower limit of the surface roughness is not particularly limited, and can be, for example, 0.3 nm or more.

[0190] In addition, in the present invention, the surface roughness Ra is measured in accordance with "JIS B 0601 (2013)".

[0191] The measurement was performed using an AFM (SPA400 manufactured by Hitachi High-Tech Corporation) or an apparatus equivalent thereto.

[0192] Below, reference Figure 3 to Figure 5 , one embodiment of the method for producing the laminated body according to the first embodiment will be described.

[0193] Figure 3 One embodiment of an apparatus that can be used in the method for producing a laminated body according to the first embodiment is shown.

[0194] Figure 3 The device 30 shown includes a delivery roller 33 for delivering the first resin layer 31 and the second resin layer 32 .

[0195] In addition, the first resin layer 31 and the second resin layer 32 are respectively formed on the surface of the support, and a laminate including the support and the resin layers can be rolled out.

[0196] Furthermore, the apparatus 30 includes a plasma irradiation device 34 that forms a mixed layer and an inorganic layer on the surfaces of the first resin layer 31 and the second resin layer 32 and irradiates plasma for forming the first stacked body and the second stacked body.

[0197] Furthermore, the device 30 includes a press roll 35 for laminating the inorganic layer of the first laminate and the inorganic layer of the second laminate.

[0198] Furthermore, the device 30 includes a roller 36 (winding roller) that winds up a stacked body obtained by stacking the first stacked body and the second stacked body using a press roller.

[0199] According to the apparatus 30 , it is possible to simultaneously perform the formation of the mixed layer and the inorganic layer on the first resin layer and the second resin layer, and the lamination of the first laminate and the second laminate.

[0200] First, the first resin layer 31 and the second resin layer 32 are fed out from the feed roll 33 .

[0201] Next, plasma is irradiated toward the joining portion of the pressure roller 35 using a plasma irradiation device 34, thereby forming a mixed layer and an inorganic layer on the surfaces of the first resin layer 31 and the second resin layer 32, obtaining a first stack and a second stack, and stacking the inorganic layer of the first stack and the inorganic layer of the second stack.

[0202] Figure 4 Another embodiment of the apparatus that can be used for the method for producing the laminated body according to the first embodiment is shown.

[0203] according to Figure 4 The apparatus 40 shown in the figure forms a mixed layer and an inorganic layer on the first resin layer and the second resin layer, and then stacks the first stacked body and the second stacked body.

[0204] In the device 40 , reference numeral 41 denotes a first resin layer, reference numeral 42 denotes a second resin layer, reference numeral 43 denotes a delivery roll, reference numeral 44 denotes a plasma irradiation device, reference numeral 45 denotes a pressure roll, and reference numeral 47 denotes a take-up roll.

[0205] Figure 5 Still another embodiment of the apparatus that can be used for the method for producing the laminated body according to the first embodiment is shown.

[0206] Figure 5 The device 50 shown in the figure includes an electrode roll 56 and a support roll 57. Between these rolls, oxygen gas containing a raw material can be converted into plasma to form a mixed layer and an inorganic layer on the surface of the first resin layer and the second resin layer.

[0207] and, Figure 5 The device 50 shown may include a housing 58 filled with the oxygen gas and a nozzle (not shown) for introducing the oxygen gas between the electrode roller 56 and the support roller 57 .

[0208] exist Figure 5In the figure, reference numeral 51 denotes a first resin layer, reference numeral 52 denotes a second resin layer, reference numeral 53 denotes a delivery roll, reference numeral 54 denotes a pressure roll, and reference numeral 55 denotes a take-up roll.

[0209] <Method for producing laminate according to second embodiment>

[0210] The method for manufacturing a laminate according to the second embodiment includes the following steps: forming a contrast layer on the surface of each of the first resin layer and the second resin layer by plasma chemical vapor deposition to obtain a first laminate having the first resin layer and the contrast layer and a second laminate having the second resin layer and the contrast layer (hereinafter also referred to as a step of forming the contrast layer); and

[0211] A step of laminating the contrast layer of the first laminate and the contrast layer of the second laminate (hereinafter also referred to as a laminating step).

[0212] The method for producing a laminated body according to the second embodiment may repeat the step of forming the contrast layer and the step of laminating a plurality of times.

[0213] For example, the manufacturing method of the stacked body involved in the second embodiment may include the following steps: forming a contrast layer on the respective surfaces of the second resin layer of the manufactured stacked body and the third resin layer prepared separately by plasma chemical vapor deposition, thereby obtaining a third stacked body comprising a first resin layer, a contrast layer, a second resin layer and a contrast layer, and a fourth stacked body comprising a third resin layer and a contrast layer; and a contrast layer between the contrast layer on the outermost surface of the stacked third stack and the contrast layer of the fourth stack.

[0214] (Step of forming a contrast layer)

[0215] The method for manufacturing a laminate according to the second embodiment includes the following steps: forming a contrast layer on the surface of each of the first resin layer and the second resin layer by plasma chemical vapor deposition to obtain a first laminate having the first resin layer and the contrast layer and a second laminate having the second resin layer and the contrast layer.

[0216] The details of the first resin layer, the second resin layer, and the comparison layer are as described above, and therefore their description is omitted here.

[0217] The contrast layer is formed on the resin layer by plasma chemical vapor deposition. More specifically, the contrast layer can be formed by using an excitation power to make a gas mixed with a raw material gas such as silane and oxygen into a plasma state, and using the gas in the plasma state to perform plasma treatment on the surface of the resin layer.

[0218] The contrast layer is formed when the etching rate on the surface of the resin layer is greater than the rate at which the inorganic layer is formed on the surface of the resin layer. The formation rate of the inorganic layer can be adjusted by changing the flow rate of oxygen and raw materials. The etching rate can be adjusted by changing the peak voltage.

[0219] Examples of the plasma treatment method include a method of irradiating the surface of the resin layer with plasma using a plasma irradiation device and a method of passing the resin layer between an electrode roll and a backup roll in the above-mentioned oxygen atmosphere.

[0220] In addition to the raw material gas and oxygen, hydrogen gas, a gas containing nitrogen atoms, an inert gas, etc. can also be used.

[0221] Examples of the gas containing nitrogen atoms include nitrogen gas (N2), ammonia gas (NH3), and nitrous gas (N2O).

[0222] Examples of the inert gas include helium, neon, argon, krypton, xenon, and radon.

[0223] From the viewpoint of forming a contrast layer on the surface of the resin layer and improving interlayer adhesion, the flow rate of oxygen is preferably 30 mL / min to 350 mL / min, more preferably 40 mL / min to 300 mL / min, and even more preferably 50 mL / min to 250 mL / min.

[0224] From the viewpoint of forming a contrast layer without an inorganic layer on the surface of the resin layer and improving the adhesion between the layers, the flow rate of oxygen is preferably 5 mL / min to 28 mL / min, more preferably 6 mL / min to 25 mL / min, and further preferably 7 mL / min to 23 mL / min.

[0225] From the viewpoint of forming a contrast layer on the resin layer surface and improving interlayer adhesion, the flow rate of the raw material is preferably 2 to 17 mg / min, more preferably 3 to 15 mg / min, and even more preferably 4 to 10 mg / min.

[0226] From the viewpoint of forming a contrast layer without an inorganic layer on the surface of the resin layer and improving the adhesion between the layers, the flow rate of the raw material is preferably 0.1 mg / min to 1.8 mg / min, more preferably 0.3 mg / min to 1.5 mg / min, and further preferably 0.5 mg / min to 1.3 mg / min.

[0227] From the perspective of interlayer adhesion, the peak voltage of the plasma excitation power used for plasmatizing the raw gas that forms a contrast layer on the surface of the resin layer and improves interlayer adhesion is preferably 3 kV to 17 kV, more preferably 4 kV to 15 kV, and further preferably 6 kV to 10 kV.

[0228] (Lamination process)

[0229] The lamination method of the first laminate and the second laminate is not particularly limited, and the lamination may be performed by placing the contrast layer of the first laminate and the contrast layer of the second laminate facing each other and press-bonding them.

[0230] The pressure bonding of the laminated bodies can be performed by overlapping the laminated bodies and passing the laminated bodies between rollers.

[0231] The pressure applied to the laminate by the roller is not particularly limited, and can be, for example, 0.1 MPa to 5 MPa.

[0232] In the method for producing a laminated body according to the second embodiment, it is preferred that the steps of forming a contrast layer on the first resin layer and the second resin layer and laminating the first laminated body and the second laminated body are performed simultaneously. Thus, the steps of forming concavities and convexities on the surface of the resin layer by etching and allowing the material forming the contrast layer to intrude into the concavities and convexities and the step of laminating the contrast layers of the laminated body are performed simultaneously, so that the smoothness of the interface between the laminated contrast layers tends to be improved, and the adhesion between the layers tends to be improved.

[0233] From the viewpoint of interlayer adhesion, the surface roughness of the contrast layer of the first laminate and the contrast layer of the second laminate is preferably 2 nm or less, more preferably 1.5 nm or less.

[0234] The method for producing a laminated body according to the second embodiment can also use the apparatus that can be used in the method for producing a laminated body according to the first embodiment.

[0235] Example

[0236] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the following examples.

[0237] <Example 1>

[0238] As a support, two polyethylene terephthalate films (A4100, manufactured by TOYOBO CO., LTD.) having a thickness of 100 μm and a width of 50 mm were prepared.

[0239] A resin composition having the following composition was applied on one surface of each support, dried, and photocured to form a first resin layer and a second resin layer having a thickness of 2 μm.

[0240] (Composition of resin composition)

[0241] Acrylic acid monomer (manufactured by SHIN-NAKAMURA CHEMICAL Co., Ltd., TMPTA) 95.5 mass%

[0242] Photopolymerization initiator (KTO46 manufactured by Lamberti SpA) 4.5 mass%

[0243] Prepared Figure 3 The device 30 is shown.

[0244] A laminate including a support and a first resin layer and a laminate including a support and a second resin layer were respectively fed from the unwinding roll 33 at a speed of 1 m / min.

[0245] Under the following conditions, plasma was irradiated from the following plasma irradiation device 34 toward the joint part of the pressure roller 35 provided in the device 30, and a mixed layer and an inorganic layer (5 nm) were formed on the surface of the first resin layer and the second resin layer to produce the first laminate and the second laminate, and the inorganic layer (silicon dioxide) of the first laminate and the inorganic layer (silicon dioxide) of the second laminate were laminated to obtain a laminate. In addition, the pressure applied to the laminate by the pressure roller was set to 0.2 MPa. The thickness of the inorganic layer in the laminate was 10 nm.

[0246] In order to measure the surface roughness Ra of the inorganic layer of the first stack and the inorganic layer of the second stack, the first stack and the second stack were prepared under the same conditions as above, and the surface roughness Ra of the inorganic layer of each stack was measured using AFM (manufactured by Hitachi High-Tech Corporation, SPA400) according to "JIS B 0601 (2013)", and the results were all 0.9 nm.

[0247] (Plasma irradiation device)

[0248] ·Atmospheric pressure plasma jet device (drip nozzle double tube type)

[0249] ·Double tube structure: outer tube diameter Φ15mm, inner tube diameter Φ8mm

[0250] ·Copper electrodes are placed on the outside of the outer tube

[0251] Peak voltage: 8kV

[0252] Pulse width: 5 microseconds

[0253] Bipolar pulse: 10kHz

[0254] Gas flowing through the outer tube: Helium (plasma generation gas, flow rate: 10L / min)

[0255] Gases flowing through the inner tube: tetraethoxysilane (also called TEOS. Flow rate: 5 mg / min), oxygen (flow rate: 100 mL / min), nitrogen (flow rate: 500 mL / min)

[0256] The laminated body produced as described above was cut into a size of 3 mm in length×3 mm in width to prepare a test piece A.

[0257] The above-mentioned test piece A was buried in molten trimethylolpropane triacrylate and then irradiated with light to prepare a cured product A (thickness 200μm, length 5mm, width 10mm). The cured product A was cut into pieces with a thickness of 20nm to prepare a test piece B. The cross section of the test piece B in the thickness direction was irradiated with an electron beam for 10 minutes at 300kV.

[0258] A cross-sectional image (magnification: 1,000,000) of the test piece B after electron beam irradiation was obtained, and the density of the cross-sectional image was measured using image analysis software.

[0259] When the concentration of the most concentrated part (inorganic layer part) in the above cross-sectional image is set to 100 and the concentration of the least concentrated part (first resin layer part and second resin layer part) is set to 0, it is confirmed that there are parts with a concentration of 10 to 90 between the inorganic layer and the first resin layer and between the inorganic layer and the second resin layer.

[0260] In addition, as a transmission electron microscope, JEM-2011 manufactured by JEOL Ltd. was used.

[0261] Furthermore, the concentration in the cross-sectional image was confirmed using the image analysis software Image J.

[0262] The thicknesses of the inorganic layer and the mixed layer included in the laminate were measured from the cross-sectional image and were found to be 10 nm and 5 nm, respectively.

[0263] In the inorganic layer forming part of the above-mentioned cross-sectional image, the area S0 of the part where the concentration is 0 to 50 and the length in the thickness direction is greater than 2 nm is calculated. The porosity of the inorganic layer is calculated by dividing it by the entire area S1 of the inorganic layer forming part and multiplying it by 100. The result is less than 5%.

[0264] <Example 2>

[0265] A laminated body was produced in the same manner as in Example 1 except that the peak voltage was changed to 6 kV.

[0266] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 9 nm and 2 nm, respectively.

[0267] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0268] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 0.9 nm.

[0269] <Example 3>

[0270] A laminated body was produced in the same manner as in Example 1 except that the peak voltage was changed to 10 kV.

[0271] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 12 nm and 10 nm, respectively.

[0272] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0273] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 1.0 nm.

[0274] <Example 4>

[0275] A laminated body was produced in the same manner as in Example 1 except that the peak voltage was changed to 15 kV.

[0276] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 14 nm and 28 nm, respectively.

[0277] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0278] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 1.2 nm.

[0279] <Example 5>

[0280] A laminated body was produced in the same manner as in Example 1 except that the flow rates of tetraethoxysilane gas and oxygen were changed to 10 mg / min and 200 mL / min, respectively.

[0281] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 22 nm and 5 nm, respectively.

[0282] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0283] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 1.3 nm.

[0284] <Example 6>

[0285] A laminated body was produced in the same manner as in Example 1 except that the flow rates of tetraethoxysilane gas and oxygen were changed to 15 mg / min and 300 mL / min, respectively.

[0286] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 28 nm and 5 nm, respectively.

[0287] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0288] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 1.4 nm.

[0289] <Example 7>

[0290] A laminated body was produced in the same manner as in Example 1 except that the flow rates of tetraethoxysilane gas and oxygen were changed to 2 g / min and 40 mL / min, respectively.

[0291] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 4 nm and 5 nm, respectively.

[0292] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0293] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 0.8 nm.

[0294] <Example 8>

[0295] A laminate was produced in the same manner as in Example 1 except that tetraethoxysilane was changed to trimethylaluminum.

[0296] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer (aluminum oxide) and the mixed layer included in the laminate were measured. The results were 10 nm and 4 nm, respectively.

[0297] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and found to be less than 5%.

[0298] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and found to be 1 nm.

[0299] <Example 9>

[0300] Prepared Figure 4 A manufacturing apparatus 40 of a laminate is shown.

[0301] The laminate including the support and the first resin layer and the laminate including the support and the second resin layer were respectively fed from the unwinding roll 43 at a speed of 1 m / min.

[0302] Plasma was irradiated from the following plasma irradiation device under the following conditions to form a mixed layer and an inorganic layer on the surfaces of the first resin layer and the second resin layer, thereby obtaining a first laminate and a second laminate.

[0303] A laminate was obtained by laminating the inorganic layer of the first laminate and the inorganic layer of the second laminate using the press roller 45 provided in the apparatus 40. The pressure applied to the laminate by the press roller was set to 0.2 MPa.

[0304] (Plasma irradiation device)

[0305] ·Atmospheric pressure plasma jet device (drip nozzle double tube type)

[0306] ·Double tube structure: outer tube diameter Φ15mm, inner tube diameter Φ8mm

[0307] ·Copper electrodes are placed on the outside of the outer tube

[0308] Peak voltage: 8kV

[0309] Pulse width: 5 microseconds

[0310] Bipolar pulse: 10kHz

[0311] Gas flowing through the outer tube: Helium (plasma generation gas, flow rate: 10L / min)

[0312] Gases flowing through the inner tube: tetraethoxysilane gas (flow rate: 2 mg / min), oxygen (flow rate: 40 mL / min), nitrogen (flow rate: 500 mL / min)

[0313] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 4 nm and 5 nm, respectively.

[0314] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and the result was 25%.

[0315] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 0.8 nm.

[0316] <Example 10>

[0317] A laminated body was produced in the same manner as in Example 9, except that the housing was used to surround the plasma irradiation portion to the pressure roller and the interior of the housing was set to a nitrogen atmosphere.

[0318] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 4 nm and 5 nm, respectively.

[0319] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and the result was 10%.

[0320] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 0.8 nm.

[0321] <Example 11>

[0322] Prepared Figure 5 A manufacturing apparatus 50 of a laminate is shown.

[0323] The laminate including the support and the first resin layer and the laminate including the support and the second resin layer were respectively fed from the unwinding roll 53 at a speed of 1 m / min.

[0324] Tetraethoxysilane gas (flow rate: 5 mg / min), oxygen (flow rate: 100 mL / min) and nitrogen (flow rate: 500 mL / min) are introduced into the shell 58 from the nozzle, so that a stack comprising a support and a first resin layer and a stack comprising a support and a second resin layer pass between an electrode roller 56 and a support roller 57 arranged in the shell 58, thereby forming a mixed layer and an inorganic layer on the surface of the first resin layer and the second resin layer, thereby obtaining a first stack and a second stack.

[0325] A laminate was obtained by laminating the inorganic layer of the first laminate and the inorganic layer of the second laminate using the press roller 54 provided in the apparatus 50. The pressure applied to the laminate by the press roller was set to 0.2 MPa.

[0326] The presence of the mixed layer was confirmed in the same manner as in Example 1, and the thicknesses of the inorganic layer and the mixed layer included in the laminate were measured. The results were 3 nm and 6 nm, respectively.

[0327] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and the result was 25%.

[0328] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and was found to be 0.8 nm.

[0329] <Comparative Example 1>

[0330] A laminated body was produced in the same manner as in Example 1 except that a sputtering device was provided instead of the atmospheric pressure plasma jet device and an inorganic layer (silicon dioxide) was formed on the surfaces of the first resin layer and the second resin layer by a sputtering method under the following conditions.

[0331] (Conditions of the sputtering method)

[0332] Argon flow rate: 100mL / min

[0333] Power: 200W

[0334] Frequency: 13.56MHz

[0335] The presence of the mixed layer was confirmed in the same manner as in Example 1, but no mixed layer was confirmed. The thickness of the inorganic layer included in the laminate was measured and found to be 10 nm.

[0336] Furthermore, the porosity of the inorganic layer was determined in the same manner as in Example 1 and the result was 27%.

[0337] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and the result was 0.7 nm.

[0338] <Adhesion Evaluation-1>

[0339] When the first resin layer is formed on the surface of the support, a film of 50 mm in width × 10 mm in length is clamped at the end of the support to provide a portion where the support and the first resin layer are not in close contact. Otherwise, the laminate is manufactured in the same manner as the above-mentioned embodiments and comparative examples.

[0340] The laminated body was cut into a size of 50 mm in the conveying direction×25 mm in the width direction to prepare a test piece, and the support on the second resin layer side was adhered and fixed to a base with a double-sided tape.

[0341] Next, the non-adherent portion of the support that was in contact with the first resin layer included in the test piece was folded back.

[0342] The folded portion was pulled in a 180° direction (peeling speed: 5 mm / sec) using a peel tester (manufactured by SHIMADZU CORPORATION, universal testing machine AGS-100NX), and the maximum load (N / 25 mm) was measured. The measurement results are summarized in Table 1.

[0343] <Adhesion Evaluation-2>

[0344] The test pieces prepared in Adhesion Evaluation-1 were subjected to the following bending test, and then the maximum load (N / 25 mm) was measured in the same manner as in Adhesion Evaluation-1. The results are summarized in Table 1.

[0345] One end of the test piece in the longitudinal direction was fixed. A Φ10 mm rod was placed at the center of the test piece, and the unfixed end of the test piece was bent 180° using this as a fulcrum, and then returned to its original state. The bending was repeated 10,000 times.

[0346]

[0347] <Example 12>

[0348] As a support, two polyethylene terephthalate films (A4100, manufactured by TOYOBO CO., LTD.) having a thickness of 100 μm and a width of 50 mm were prepared.

[0349] A resin composition having the following composition was applied on one surface of each support, dried, and photocured to form a first resin layer and a second resin layer having a thickness of 2 μm.

[0350] (Composition of resin composition)

[0351] Acrylic acid monomer (manufactured by SHIN-NAKAMURA CHEMICAL Co., Ltd., TMPTA) 95.5 mass%

[0352] Photopolymerization initiator (KTO46 manufactured by Lamberti SpA) 4.5 mass%

[0353] Prepared Figure 3 The device 30 is shown.

[0354] A laminate including a support and a first resin layer and a laminate including a support and a second resin layer were respectively fed from the unwinding roll 33 at a speed of 1 m / min.

[0355] Under the following conditions, plasma was irradiated from the following plasma irradiation device 34 toward the joint portion of the pressure roller 35 provided in the device 30, and contrast layers were formed on the surfaces of the first resin layer and the second resin layer to produce the first laminate and the second laminate, and the contrast layer of the first laminate and the contrast layer of the second laminate were laminated to obtain the laminate. In addition, the pressure applied to the laminate by the pressure roller was set to 0.2 MPa.

[0356] (Plasma irradiation device)

[0357] ·Atmospheric pressure plasma jet device (drip nozzle double tube type)

[0358] Double tube structure: outer tube diameter Φ15mm, inner tube diameter Φ8mm

[0359] ·Copper electrodes are placed on the outside of the outer tube

[0360] Peak voltage: 8kV

[0361] Pulse width: 5 microseconds

[0362] Bipolar pulse: 10kHz

[0363] Gas flowing through the outer tube: Helium (plasma generation gas, flow rate: 10L / min)

[0364] Gases flowing through the inner tube: tetraethoxysilane (also known as TEOS. Flow rate: 1 mg / min), oxygen (flow rate: 20 mL / min), nitrogen (flow rate: 500 mL / min)

[0365] The laminated body produced as described above was cut into a size of 3 mm in length×3 mm in width to prepare a test piece a.

[0366] The above-mentioned test piece a was buried in molten trimethylolpropane triacrylate and then irradiated with light to prepare a cured product b (thickness 200 μm, length 5 mm, width 10 mm). The cured product b was cut into a thickness of 20 nm to prepare a test piece b. The cross section of the test piece b in the thickness direction was irradiated with an electron beam for 10 minutes at 300 kV.

[0367] A cross-sectional image of the test piece b after electron beam irradiation (magnification: 1,000,000 times) was obtained, and the density of the cross-sectional image was measured using image analysis software.

[0368] When the maximum concentration inside the contrast layer in the cross-sectional image is set to 100 and the concentrations of the first resin layer and the second resin layer are set to 0, it is confirmed that the concentration decreases by 25 per 1 nm from the inside to the surface of the contrast layer.

[0369] Furthermore, the porosity of the comparative layer was determined in the same manner as in Example 1 and the result was less than 5%.

[0370] Furthermore, the surface roughness Ra of the inorganic layer was determined in the same manner as in Example 1 and the result was 0.6 nm.

[0371] Adhesion Evaluation-1 and Adhesion Evaluation-2 were performed in the same manner as in Example 1, etc., and the maximum load was 12 N / 25 mm in both cases.

[0372] As can be seen from the above examples and comparative examples, the laminates produced in the examples have superior interlayer adhesion compared to the laminates produced in the comparative examples.

[0373] The disclosure of Japanese Patent Application No. 2022-050807 filed on March 25, 2022 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each document, patent application, and technical standard were specifically and individually described as being incorporated by reference.

Claims

1. A laminate comprising a first resin layer, an inorganic layer and a second resin layer, and A mixed layer is provided between the first resin layer and the inorganic layer and between the second resin layer and the inorganic layer.

2. The laminate according to claim 1, wherein The inorganic layer is a continuous layer.

3. The laminate according to claim 1 or 2, wherein: The porosity of the inorganic layer is 25% or less.

4. The laminate according to any one of claims 1 to 3, wherein The thickness of the mixed layer is 1 nm to 30 nm.

5. The laminate according to any one of claims 1 to 4, wherein The inorganic layer contains one or more inorganic materials selected from the group consisting of silicon oxide, silicon nitride, aluminum oxide, and aluminum nitride.

6. The laminate according to any one of claims 1 to 5, wherein The inorganic layer includes silicon dioxide.

7. The laminate according to any one of claims 1 to 6, wherein The thickness of the inorganic layer is less than 5 nm.

8. A laminate comprising a first resin layer and a second resin layer, A contrast layer containing an inorganic material is provided between the first resin layer and the second resin layer, The cross section of the stack was irradiated with an electron beam for 10 minutes at a voltage of 300 kV using a transmission electron microscope to obtain a cross-sectional image of the test piece after electron beam irradiation. The concentration measured by image analysis software decreased from the inside of the contrast layer toward the surface of the cross-sectional image.

9. A method for manufacturing a laminate, comprising the following steps: Forming a mixed layer and an inorganic layer in sequence on the surfaces of a first resin layer and a second resin layer respectively by plasma chemical vapor deposition to obtain a first laminate and a second laminate, wherein the first laminate comprises the first resin layer, the mixed layer and the inorganic layer, and the second laminate comprises the second resin layer, the mixed layer and the inorganic layer; and The inorganic layer of the first stack is stacked on the inorganic layer of the second stack. 10 . The method for producing a laminate according to claim 9 , wherein formation of the mixed layer and the inorganic layer on the first resin layer and the second resin layer and lamination of the first laminate and the second laminate are performed simultaneously.

11. The method for producing a laminate according to claim 9 or 10, wherein: The surface roughness Ra of the inorganic layer of the first stack and the inorganic layer of the second stack is 2 nm or less.

12. A method for manufacturing a laminate, comprising the following steps: Forming a contrast layer on the surface of each of the first resin layer and the second resin layer by plasma chemical vapor deposition to obtain a first laminate and a second laminate, wherein the first laminate comprises the first resin layer and the contrast layer, and the second laminate comprises the second resin layer and the contrast layer; and The contrast layer of the first stack and the contrast layer of the second stack are stacked. 13 . The method for producing a laminate according to claim 9 , wherein the formation of the contrast layer on the first resin layer and the second resin layer and the lamination of the first laminate and the second laminate are performed simultaneously.

14. The method for producing a laminate according to claim 9 or 10, wherein: The contrast layer of the first stack and the contrast layer of the second stack have a surface roughness Ra of 2 nm or less.

Citation Information

Patent Citations

  • Gas barrier film and method for producing gas barrier film

    CN110603148A

  • Gas barrier film

    CN111065514A

  • Method for modifying battery isolating membrane

    CN113629351A