Method for producing treated silica-dispersed monomer composition

By mixing the silica dispersion liquid with a silane coupling agent in an aqueous solvent and combining it with a polymeric monomer, the problem of insufficient dispersion state of silica particles is solved, the mechanical characteristics and fluidity of the material are improved, and it is suitable for dentistry. Use materials.

CN118900853APending Publication Date: 2024-11-05GC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028956.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-02-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the prior art, the dispersion state of silica particles in the polymerizable monomer is insufficient, which affects the mechanical properties and fluidity of the material, making it difficult to achieve an ideal dispersion effect.

Method used

By mixing the alkaline dispersion of silica with a silane coupling agent in an aqueous solvent, preparing the silane-treated silica dispersion, and removing the aqueous phase after mixing it with the polymerizable monomer, better silica particles are obtained Dispersed state.

Benefits of technology

The uniform dispersion of silica particles is achieved, the mechanical characteristics and fluidity of the material are improved, and it is suitable for dental materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This method for producing a treated silica-dispersed monomer composition comprises: mixing an alkaline silica dispersion in which silica is dispersed in a solvent containing 10 mass% or more of water with a silane coupling agent to prepare a silane-treated silica dispersion; the silane-treated silica dispersion liquid is mixed with a polymerizable monomer to obtain a mixture, and the aqueous phase is removed from the mixture to obtain a composition in which the silane-coupling-agent-treated silica is dispersed in the polymerizable monomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a treated silica-dispersed monomer composition. Background Art

[0002] In the dental field, compositions in which silane-treated silica particles are dispersed in polymerizable monomers are known (for example, see Patent Documents 1 and 2). Such compositions have good mechanical properties and moderate fluidity (consistency, etc.), and are therefore suitable for use as dental materials.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent document 1: Japanese Patent No. 4748938.

[0006] Patent document 2: Japanese Patent No. 4800535. Summary of the invention

[0007] Problems to be solved by the invention

[0008] In the composition formed by dispersing the silane-treated silica particles in the polymerizable monomer as described above, the better the dispersion state of the silica particles in the polymerizable monomer, that is, the more uniformly the silica particles are dispersed in the polymerizable monomer, the better the dispersion state of the silica particles in the material when applied to the material, and the better the properties of the material. However, the dispersion state of the silica particles in the composition obtained by the conventional manufacturing method has room for improvement.

[0009] In view of the above, an object of one embodiment of the present invention is to provide a method for producing a composition in which silane-treated silica particles are dispersed in a polymerizable monomer, the method being capable of obtaining a better dispersion state of the silica particles.

[0010] Means for solving problems

[0011] A method for producing a treated silica-dispersed monomer composition according to one embodiment of the present invention comprises: mixing an alkaline silica dispersion in which silica is dispersed in a solvent containing 10% by mass or more of water with a silane coupling agent, preparing a silane-treated silica dispersion, mixing the silane-treated silica dispersion with a polymerizable monomer to obtain a mixture, and removing the aqueous phase from the mixture to obtain a composition in which silica treated with a silane coupling agent is dispersed in the polymerizable monomer.

[0012] Effects of the Invention

[0013] According to one embodiment of the present invention, in a method for producing a composition in which silane-treated silica particles are dispersed in a polymer monomer, a better dispersion state of the silica particles can be obtained. DETAILED DESCRIPTION

[0014] One embodiment of the present invention is a method for producing a composition in which silica particles treated with silane are dispersed in a polymerizable monomer (hereinafter, also referred to as a treated silica-dispersed monomer composition). The production method of this embodiment includes at least the following steps: a first step of preparing a silane-treated silica dispersion (sometimes referred to as a treated silica dispersion) by mixing a silica dispersion in which silica is dispersed in a solvent containing water with a silane coupling agent to treat silica; a second step of adding a polymerizable monomer to the silane-treated silica dispersion to obtain a mixture; and a third step of removing the aqueous phase from the mixture to obtain a composition in which silica treated with a silane coupling agent is dispersed in a polymerizable monomer (a silane-treated silica-dispersed monomer composition, or a treated silica-dispersed monomer composition).

[0015] <Step 1: Preparation of silane-treated silica dispersion>

[0016] The first step is a step of treating the surface of silica with a silane coupling agent, that is, a step of reacting silica with a silane coupling agent. In this step, an alkaline silica dispersion in which silica is dispersed in a solvent containing water is used. That is, the silane coupling agent is not directly contacted with silica, but the silane coupling agent is acted on silica already dispersed in the dispersion. Thus, in the dispersion, silica and the silane coupling agent can react, so even if the silica has a small particle size, the aggregation of silica can be suppressed, and the dispersion state of silica in the treated silica dispersion monomer composition obtained by the manufacturing method of this mode can be improved. That is, the aggregation of silica can be suppressed, and a state in which silica is uniformly dispersed in the composition is obtained.

[0017] In addition, the solvent of the silica dispersion contains water, and the amount of water is 10% by mass or more relative to the total amount of the solvent of the silica dispersion. By using the above amount of water in the silica dispersion, the dispersion state of silica in the treated silica dispersion obtained in the first step can be improved, and the dispersion state of silica in the treated silica dispersion monomer composition can be improved.

[0018] The amount of water in the solvent used for the silica dispersion is preferably 20% by mass or more, more preferably 30% by mass or more, further preferably 50% by mass or more, further preferably 70% by mass or more, further preferably 90% by mass or more, further preferably 95% by mass or more, relative to the total amount of the solvent. In addition, the solvent is preferably substantially composed of water or is water.

[0019] In addition, the silica dispersion (liquid before the addition of the silane coupling agent and / monomer) may contain solvents other than water. The solvent other than water may be an amphiphilic solvent (a solvent having two properties of hydrophilicity and hydrophobicity) that can be mixed with water and has a lower boiling point than water, and as a specific example, alcohols such as ethanol, methanol, propanol, isopropyl alcohol, butanol, acetones, ethers, etc. may be cited. In the case where the treated silica dispersion monomer composition obtained by this method is used for dental materials, etc., ethanol is preferably used from the viewpoint of safety in the case of residual solvent.

[0020] Silica is added as an inorganic filler in the treated silica monomer composition obtained by the manufacturing method of this embodiment. The silica used in this embodiment is nanoscale, that is, silica particles with an average particle size of primary particles less than 1 μm. The average particle size of silica is preferably 1 to 500 nm, more preferably 1 to 200 nm. Silica particles having an average particle size as described above are preferred from the perspective of improving the aesthetics of dental materials, for example, when the treated silica dispersed monomer composition manufactured is applied to dental materials. In addition, when measuring the particle size distribution of silica, it may have one particle size peak or may have two or more. In addition, the particle size of the particles in this specification can be measured by laser diffraction scattering method or electron microscope observation, and the average particle size may be a volume average diameter.

[0021] The silica used in this embodiment may be non-agglomerated silica. In this specification, non-agglomerated silica has a spherical shape or a substantially spherical shape. In addition, the BET specific surface area of ​​the silica may be 20 to 500 m 2 / g or so.

[0022] The silica dispersion is alkaline, so that the silica and the silane coupling agent can react under alkaline conditions. The reaction under alkaline conditions can suppress the aggregation of silica particles while performing the silica surface coupling reaction, thereby making the dispersion state of silica in the obtained treated silica dispersion monomer composition good, so it is preferred. The pH of the silica dispersion is preferably 8 to 12, and more preferably 9 to 11.

[0023] The silica dispersion may be a silica sol, colloidal silica, or the like in which silica is dispersed in a solvent containing water. Examples of the silica dispersion include Ludox (registered trademark) PW-50 (pH 9.8 to 10.6), CL-X, and PX-30 manufactured by WRGRACE, and SNOWTEX (registered trademark) ST-ZL (pH 9.0 to 11.0), ST-YL, and ST-30L manufactured by Nissan Chemical Co., Ltd. In addition, dry silica particles such as fumed silica may be dispersed in a solvent containing water to prepare the mixture. In this case, examples of dry silica particles include AEROSIL (registered trademark) OX-50, AEROSIL (registered trademark) 200, and AEROSIL (registered trademark) 380 manufactured by EVONIK.

[0024] An alkaline salt may be added to the solvent for modulating the silica dispersion to modulate an alkaline aqueous solution. The alkaline salt may be an inorganic salt or an organic salt, for example, sodium hydroxide, sodium tripolyphosphate, sodium carbonate, etc. By adding an alkaline salt to make the silica dispersion alkaline, the possibility of volatilization caused by temperature changes, etc., and the alkalinity of the silica dispersion changing can be reduced, and the pH in the treatment process can be stably maintained in the alkaline region. In addition, the silica dispersion contains sodium ions, and the mixed solution of the silica dispersion and the silane coupling agent contains sodium ions, thereby further suppressing the aggregation of silica particles in the liquid.

[0025] The concentration of silica in the silica dispersion is preferably 20 to 70% by mass, more preferably 30 to 60% by mass. By setting the concentration within the above range, aggregation of silica can be suppressed and the efficiency of the reaction between silica and the silane coupling agent can be improved.

[0026] In the first step, a silica dispersion is mixed with a silane coupling agent. In this case, the silane coupling agent may be added directly to the silica dispersion in an untreated state, or may be added after at least a portion of the hydrolyzable group has been hydrolyzed. It is preferred to use a pre-hydrolyzed silane coupling agent because the surface treatment of silica is more rapid and the amount of flammable solvent used can be reduced.

[0027] When the silane coupling agent is pre-hydrolyzed, the silane coupling agent is dispersed in an aqueous solvent such as water or alcohol. In this case, the pH of the solvent in which the silane coupling agent is dispersed can also be made acidic or alkaline. It is preferred that the reaction between silica and the silane coupling agent is carried out under alkaline conditions as described above, so that the solvent in which the silane coupling agent is dispersed is preferably neutral or alkaline. In addition, in order to promote the hydrolysis reaction, an acid component or alkaline component other than the above-mentioned aqueous solvent can be added to the liquid in which the silane coupling agent is dispersed, and the mixed liquid after the liquid in which the silane coupling agent is dispersed and the silica dispersion is mixed is preferably alkaline. In addition, when the silane coupling agent is hydrolyzed and then mixed with the silica dispersion, the silane coupling agent can be added as a dispersion having a concentration of about 20 to 50% by mass.

[0028] The silane coupling agent is not particularly limited, but preferably has a polymerizable double bond, more specifically, an unsaturated double bond capable of free radical polymerization. From the viewpoint of transparency, the silane coupling agent having an unsaturated double bond capable of free radical polymerization is preferably a silane coupling agent having a (meth)acryloyloxy group suitable in the dental field. Specific examples of the silane coupling agent having a (meth)acryloyloxy group include methacryloxymethyltrimethoxysilane, 2-methacryloyloxyethyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane (γ-methacryloyloxypropyltrimethoxysilane), 4-methacryloyloxybutyltrimethoxysilane, 5-methacryloyloxypentyltrimethoxysilane, 6-methacryloyloxyhexyltrimethoxysilane, 7-methacryloyloxyheptyltrimethoxysilane, 8-methacryloyloxyoctyltrimethoxysilane (θ-methacryloyloxyoctyltrimethoxysilane), 9-methacryloyloxynonyltrimethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, and 12-methacryloyloxybutyltrimethoxysilane. 1-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylethyldiethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 2-(meth)acryloxyethoxypropyltrimethoxysilane, etc. Among them, from the perspective of being generally circulated and easily available, one or more of 3-methacryloxypropyltrimethoxysilane (γ-methacryloxypropyltrimethoxysilane) and 8-methacryloxyoctyltrimethoxysilane (θ-methacryloxyoctyltrimethoxysilane) are preferred. In addition, the above-mentioned silane coupling agent can be used alone or in combination of two or more.

[0029] When the silane coupling agent and the silica dispersion are mixed, the desired amount of the silane coupling agent or the dispersion of the silane coupling agent may be added at once, or the silane coupling agent or the dispersion of the silane coupling agent may be added dropwise in small amounts multiple times while stirring the silica dispersion. In addition, when the silica dispersion and the silane coupling agent are stirred, a stirring device such as an electromagnetic stirrer may be used, and ultrasonic irradiation may be performed.

[0030] <Step 2: Addition of polymerizable monomer>

[0031] The second step is a step of further mixing a polymerizable monomer into the dispersion of silane-treated silica obtained in the first step (treated silica dispersion) to obtain a mixture. In this method, the treated silica is dispersed in the liquid, so that stirring becomes easy even when a monomer is added. Compared with the overall blending method of mixing silica and monomers in advance, the state in which silica is uniformly dispersed in the mixture is maintained.

[0032] A polymerizable monomer is a monomer containing a polymerizable double bond, more specifically, a monomer having an unsaturated double bond capable of free radical polymerization. The monomer containing a polymerizable double bond is not particularly limited, but from the viewpoint of high transparency, a polymerizable monomer having a (meth)acryloyloxy group suitable for the dental field is preferred. In addition, in this specification, the so-called "having a (meth)acryloyloxy group" means having an acryloyloxy group or a methacryloyloxy group, or both. In addition, the so-called "(meth)acrylate" refers to a monomer, oligomer, or prepolymer of acrylate and / or methacrylate.

[0033] Specific examples of the polymerizable monomer having a (meth)acryloyloxy group include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, hydroxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxy-1,3-di(meth)acryloyloxypropane, ethylene glycol di(meth)acrylate, and the like. Acrylates, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolmethane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, polybutylene glycol di(meth)acrylate, bisphenol A diglycidyl (meth)acrylate, dimethacrylate [(dimethylmethylene)bis(4,1-phenyleneoxyethylene)]ester (Bis-MEPP). Furthermore, as specific examples of the polymerizable monomer having a (meth)acryloyloxy group, as (meth)acrylates having a urethane bond, di-2-(meth)acryloyloxyethyl-2,2,4-trimethylhexamethylene dicarbamate, 1,3,5-tris[1,3-bis{(meth)acryloyloxy}-2-propoxycarbonylaminohexane]-1,3,5-(1H,3H,5H)triazine-2,4,6-trione, 2,2-bis[4-{3-(meth)acryloyloxy-2-hydroxypropyl}phenyl]propane, 2,2-bis[4-{(meth)acryloyloxyethoxy}phenyl]propane, etc. can be mentioned. In addition, examples include (meth)acrylates of urethane oligomers containing 2,2'-bis(4-hydroxycyclohexyl)propane, 2-oxacycloheptanone, 1,6-hexamethylene diisocyanate, and 2-hydroxyethyl (meth)acrylate, (meth)acrylates of urethane oligomers containing 1,3-butanediol, 1,6-hexamethylene diisocyanate, and 2-hydroxyethyl (meth)acrylate, and urethane dimethacrylate (UDMA) are also included. Among these, polyfunctional (meth)acrylates are preferred, di(meth)acrylates are particularly preferred, and dimethacrylates [(dimethylmethylene)bis(4,1-phenyleneoxyethylene)] dimethacrylate (Bis-MEPP) and urethane dimethacrylate (UDMA) are preferred.Polyfunctional (meth)acrylates have a higher boiling point than monofunctional (meth)acrylates and are therefore less likely to volatilize and boil in the subsequent heating step (the fourth step, described later) at 80° C. to 150° C., and are therefore preferred. The polymerizable monomers may be used alone or in combination of two or more.

[0034] The amount of the polymerizable monomer and the amount of silica can be adjusted according to the properties of the treated silica-dispersed monomer composition or its cured product to be obtained, and the amount of silica can be preferably 50 to 300 parts by mass, more preferably 100 to 250 parts by mass, per 100 parts by mass of the polymerizable monomer.

[0035] In the second step, when the treated silica dispersion obtained in the first step is mixed with the polymerizable monomer, this can be carried out using a mixer such as a rotation-revolution mixer.

[0036] <Step 3: Removal of aqueous phase>

[0037] A step of removing unnecessary components from the mixture of the treated silica dispersion liquid and the polymerizable monomer obtained in the above-mentioned second step to obtain a treated silica dispersion monomer composition. The mixture at the end of the second step contains an oil phase and an aqueous phase. The oil phase mainly contains polymerizable monomers and silica treated with silane, and residual silane coupling agent. On the other hand, the aqueous phase mainly contains water, an aqueous solvent, ions such as sodium ions, silica not treated with silane, etc.

[0038] When the mixture at the end of the second operation is visually separated from the water phase, the oil phase of the supernatant can be taken out by known methods such as the tilting method to remove the water phase. In addition, even if the mixture at the end of the second operation is clearly separated from the water phase, even if it is not separated, the mixture can be separated from the water phase and / or the water phase by applying any energy such as mechanical energy and thermal energy as needed. The above-mentioned treatment can be, for example, centrifugal separation, filtration, heating, freeze drying, solvent distillation removal, etc. In the case of centrifugal separation for the separation of the above-mentioned oil phase and the water phase, the specific gravity of the polymerizable monomer is preferably more than 1. In addition, particularly in the case where the separation of the oil phase and the water phase cannot be visually confirmed, the mixture can also be irradiated with ultrasound to separate the oil phase and the water phase.

[0039] Furthermore, when removing the aqueous phase in the third step, water or acidic water may be added to the oil phase temporarily removed as described above, so that unnecessary components in the oil phase (e.g., residual unreacted silane coupling agent, residual untreated silica, residual sodium ions, etc.) are dispersed in the aqueous phase, and the aqueous phase is removed. Such addition of water or acidic water may also be performed on the mixture obtained at the end of the second step.

[0040] The oil phase remaining after removing the water phase in the third step becomes the treated silica dispersed monomer composition. The water phase may not be completely removed by the third step, and the water phase may remain in the obtained treated silica dispersed monomer composition (oil phase). However, it is preferred that no phase separation is observed in the treated silica dispersed monomer composition. If the properties of the treated silica dispersed monomer composition (oil phase) have a certain degree of fluidity, it may be in a slurry, paste or clay state.

[0041] In this way, a composition (treated silica-dispersed monomer composition) in which silica treated with a silane coupling agent is dispersed in a polymerizable monomer is obtained by a manufacturing method including at least the above-mentioned first to third steps. The evaluation of the dispersion state of silica (filler) in such a treated silica-dispersed monomer composition can be performed by directly observing the composition, and the good dispersion state of the treated silica-dispersed monomer composition is reflected as a good dispersion state in the cured product, which can be observed as a cured product obtained by curing the treated silica-dispersed monomer composition. In this case, for example, the evaluation can be performed by observing the agglomerates in the cured product using an electron microscope or the like on the flat surface or cross section of the cured product.

[0042] <Step 4: Heating>

[0043] The fourth step is a step of heating the oil phase obtained in the third step as needed. By heating, the dehydration condensation of the silane coupling agent proceeds. The silane coupling agent undergoes dehydration condensation, so that the silane coupling agent is fixed on the surface of silica, and the dispersibility of silica in the composition is improved. In addition, by heating in the fourth step, if a solvent remains, the solvent can be removed by evaporation.

[0044] The heating temperature is preferably 80° C. to 150° C., more preferably 100° C. to 130° C. The heating time is preferably about 30 to 360 minutes.

[0045] [Use of treated silica-dispersed monomer composition]

[0046] The obtained treated silica dispersion monomer composition can be used for dental curable materials, such as photopolymerizable dental curable materials. In particular, it can be suitable for dental composite resins and one-dose dental composite resins. When used as a dental composite resin, additional components can be added to the above-mentioned treated silica dispersion monomer composition, such as photopolymerization initiators, fillers such as barium glass, inhibitors, ultraviolet absorbers, fluorescent agents, pigments, etc. Therefore, one embodiment of the present invention can be a method for manufacturing a dental curable material by adding additional components to the above-mentioned treated silica dispersion monomer composition.

[0047] Example

[0048] In each of the following examples, a composition in which treated silica was dispersed in a monomer (treated silica monomer composition) was obtained by a different method. In addition, a cured product of the obtained composition was prepared, and the dispersion state of silica in the cured product was evaluated.

[0049] <Silica dispersibility evaluation method>

[0050] In the composition obtained from each of the above examples, a photopolymerization initiator (triethylene glycol dimethacrylate (TEGDMA) in which camphorquinone / dimethylaminoethyl methacrylate is dissolved) is mixed in a ratio of [amount of monomers in the composition]: [amount of TEGDMA] = 80:20 to obtain a photopolymerizable composition. The photopolymerizable composition is polymerized by irradiation with visible light to prepare a cured product, and the surface of the cured product is mirror-polished with water-resistant abrasive paper to form a smooth surface, which is observed using a scanning electron microscope (SEM). Specifically, images are obtained at a magnification that can be confirmed in the range of 50 μm×40 μm at any three locations on the smooth surface. The number of agglomerates larger than 3 μm is counted in each of the three images obtained, and the average number of agglomerates per image is calculated. The evaluation criteria are as follows:

[0051] Excellent: Average value is less than 1

[0052] Good: The average value is 1 or more and less than 3

[0053] No: Average value must be 3 or above

[0054] (Example 1)

[0055] 20 g of a colloidal silica aqueous dispersion ("Ludox (registered trademark) PW-50" manufactured by WRGRACE, silica concentration: 50% by mass, sodium ion stabilized, pH 9.8-10.6, silica particle size peaks of 20-30 nm and 50 nm) and 3.5 g of γ-methacryloxypropyltrimethoxysilane ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.) were stirred for 10 minutes at 23°C using an electromagnetic stirrer, and then ultrasonic waves were irradiated at a vibration frequency of 38 kHz and 120 W for 30 minutes to mix, thereby obtaining a treated silica dispersion.

[0056] Next, 5.5 g of [(dimethylmethylene)bis(4,1-phenyleneoxyethylene)]dimethacrylate (Bis-MEPP, dimethacrylate monomer) was added, and the mixture was further stirred at a revolution speed of 1000 rpm for 10 minutes using an autorotational mixer to obtain a mixture.

[0057] Furthermore, the aqueous phase was removed from the mixture in which the oil phase and the aqueous phase were separated to obtain the oil phase. 25 mL of acidic water (aqueous acetic acid solution at pH 3.5) was further added to the obtained oil phase and stirred to remove the separated aqueous phase. The treated silica dispersed monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane and dispersed in Bis-MEPP) was obtained by heating at 120° C. with a steam dryer for 120 minutes. A cured product was prepared using the obtained treated silica dispersed monomer composition, and the dispersion state of silica was evaluated as described above, with the result being "excellent".

[0058] (Example 2)

[0059] A treated silica dispersion monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane is dispersed in Bis-MEPP) was obtained in the same manner as in Example 1 except that 20 g of another colloidal silica dispersion ("SNOWTEX (registered trademark) ST-ZL" manufactured by Nissan Chemical Co., Ltd., silica concentration: 40% by mass, sodium ion stabilized, pH: 9.0 to 11.0, silica average particle size: 70 to 100 nm) was used instead of the colloidal silica aqueous dispersion of Example 1, the amount of γ-methacryloxypropyltrimethoxysilane ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed to 2.4 g, and the amount of Bis-MEPP was changed to 5.0 g. A cured product was prepared using the obtained treated silica dispersion monomer composition, and the dispersion state of silica was evaluated as described above, and the result was "good".

[0060] (Example 3)

[0061] 10 g of fumed silica ("AEROSIL (registered trademark) OX-50" manufactured by EVONIK, the average particle size of silica is about 40 nm, and the particle size distribution is 10 to 100 nm) was added to 20 g of an aqueous sodium hydroxide solution adjusted to pH 10, and the mixture was stirred for 10 minutes at 23°C using an electromagnetic stirrer. Furthermore, ultrasonic waves were irradiated at a vibration frequency of 38 kHz and 120 W for 30 minutes to disperse the silica substantially to primary particles, thereby obtaining a silica aqueous dispersion (silicon dioxide slurry). 4.0 g of γ-methacryloxypropyltrimethoxysilane ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 30 g of the obtained silica aqueous dispersion, and the mixture was stirred for 10 minutes at 23°C using an electromagnetic stirrer. Ultrasonic waves were further irradiated at a vibration frequency of 38 kHz and 120 W for 30 minutes to obtain a treated silica dispersion.

[0062] Next, the mixture was obtained in the same manner as in Example 1 except that the amount of Bis-MEPP added was 6.0 g, and a treated silica-dispersed monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane was dispersed in Bis-MEPP) was further obtained. A cured product was prepared using the obtained treated silica-dispersed monomer composition, and the dispersion state of silica was evaluated as described above, and the result was "good".

[0063] (Example 4)

[0064] 20 g of colloidal silica aqueous dispersion ("Ludox PW-50" manufactured by WRGRACE) was prepared. On the other hand, 3.0 g of θ-methacryloyloxyoctyltrimethoxysilane ("KBM-5803" manufactured by Shin-Etsu Chemical Co., Ltd.) was dissolved in a mixed solvent of 40 g of ethanol and 10 g of distilled water, and stirred at room temperature for 24 hours to hydrolyze θ-methacryloyloxyoctyltrimethoxysilane. Furthermore, the colloidal silica aqueous dispersion and the solution of the hydrolyzed θ-methacryloyloxyoctyltrimethoxysilane were mixed by stirring to obtain a treated silica dispersion.

[0065] Next, 6.0 g of Bis-MEPP was added to the silica dispersion, followed by stirring to obtain a mixture.

[0066] The obtained mixture was evaporated to distill off the ethanol, and a mixture in which the oil phase and the water phase were separated was obtained. The oil phase was taken out from the mixture, and acidic water was further added to the obtained oil phase and stirred, and then the water phase was removed. The treated silica dispersion monomer composition (a composition in which silica treated with θ-methacryloxypropyltrimethoxysilane was dispersed in Bis-MEPP) was obtained by heating at 120° C. for 120 minutes in a steam dryer. A cured product was prepared using the obtained treated silica dispersion monomer composition, and the dispersion state of silica was evaluated as described above, and the result was "excellent".

[0067] (Example 5)

[0068] 20 g of colloidal silica aqueous dispersion ("Ludox PW-50" manufactured by WRGRACE) was prepared. On the other hand, 3.5 g of γ-methacryloxypropyltrimethoxysilane ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.) was dissolved in a mixed solvent of 40 g of ethanol and 10 g of distilled water, and stirred at room temperature for 24 hours to hydrolyze the γ-methacryloxypropyltrimethoxysilane. Furthermore, the colloidal silica aqueous dispersion and the solution of the hydrolyzed γ-methacryloxypropyltrimethoxysilane were mixed by stirring to obtain a treated silica dispersion.

[0069] Next, 5.5 g of urethane dimethacrylate (UDMA, a dimethacrylate monomer) was added to the silica dispersion, followed by stirring to obtain a mixture.

[0070] The obtained mixture was evaporated in the same manner as in Example 4, and the oil phase was taken out to obtain a treated silica dispersion monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane was dispersed in UDMA). A cured product was prepared using the obtained treated silica dispersion monomer composition, and the dispersion state of silica was evaluated as described above, with the result being "excellent".

[0071] (Comparative Example 1)

[0072] 10 g of fumed silica ("AEROSIL OX-50" manufactured by EVONIK) was placed in a mortar, and 3.5 g of γ-methacryloxypropyltrimethoxysilane ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.) was added dropwise while stirring in the mortar. After stirring until the agglomeration of silica (filler) was basically invisible, the mixture was heated at 120° C. for 120 minutes in a steam dryer to condense γ-methacryloxypropyltrimethoxysilane (silane coupling agent) on the surface of silica, thereby obtaining silica treated with a silane coupling agent (silane-treated silica). Then, 5.5 g of Bis-MEPP was added to the silica treated with a silane coupling agent (silane-treated silica), and the mixture was mixed to obtain a treated silica-dispersed monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane was dispersed in Bis-MEPP). A cured product was prepared using the obtained treated silica-dispersed monomer composition, and the dispersion state of silica was evaluated as described above. The result was "unacceptable".

[0073] (Comparative Example 2)

[0074] A treated silica dispersion monomer composition (a composition in which silica treated with θ-methacryloxyoctyltrimethoxysilane is dispersed in UDMA) was obtained in the same manner as in Comparative Example 1 except that 3.0 g of θ-methacryloxyoctyltrimethoxysilane (“KBM-5803” manufactured by Shin-Etsu Chemical Co., Ltd.) was used instead of 3.5 g of γ-methacryloxypropyltrimethoxysilane (“KBM-503” manufactured by Shin-Etsu Chemical Co., Ltd.) and the amount of Bis-MEPP was changed to 6.0 g. The cured product was prepared using the obtained treated silica dispersion monomer composition, and the dispersion state of silica was evaluated as described above, which was “unacceptable”.

[0075] (Comparative Example 3)

[0076] A treated silica dispersion monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane is dispersed in Bis-MEPP) was obtained in the same manner as in Example 1 except that 40 g of a colloidal silica dispersion ("SNOWTEX (registered trademark) ST-OL" manufactured by Nissan Chemical Co., Ltd., silica concentration: 20% by mass, pH: 2.0 to 4.0, average particle size: 40 to 50 nm) was used instead of 20 g of the colloidal silica dispersion in Example 1 and the amount of γ-methacryloxypropyltrimethoxysilane ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed to 2.4 g. The cured product was prepared using the treated silica dispersion monomer composition obtained, and the dispersion state of silica was evaluated as described above, and the result was "unacceptable".

[0077] (Comparative Example 4)

[0078] A treated silica dispersion was obtained in the same manner as in Example 3 except that 20 g of ethanol was used instead of 20 g of the sodium hydroxide aqueous solution adjusted to pH 10.

[0079] Next, 6.0 g of Bis-MEPP was added and stirred to obtain a mixture.

[0080] The mixture was evaporated, ethanol was distilled off, and then heated at 120°C for 120 minutes in a steam dryer to obtain a treated silica dispersion monomer composition (a composition in which silica treated with γ-methacryloxypropyltrimethoxysilane was dispersed in Bis-MEPP). A cured product was prepared using the obtained treated silica dispersion monomer composition, and the dispersion state of silica was evaluated as described above, and the result was "unacceptable".

[0081] Thus, it can be seen that in Examples 1 to 4, which include the steps of mixing a silica dispersion liquid in which silica is dispersed in a solvent containing water and a silane coupling agent, and treating silica under alkaline conditions, the dispersion state in the cured product produced using the treated silica dispersion monomer composition obtained is good. In particular, the result of Example 1, which uses colloidal silica and has a relatively small silica particle size, is excellent. On the other hand, in Comparative Examples 1 and 2, which do not use a solvent but mix silica and a silane coupling agent, the dispersion state of silica in the cured product produced using the treated silica dispersion monomer composition obtained is inferior to the results of Examples 1 to 4. In addition, in Comparative Example 3, which reacts under acidic solvent conditions, and Comparative Example 4, which uses ethanol as the medium, the dispersion state of silica in the prepared photopolymerizable composition is inferior to the results of Examples 1 to 4.

[0082] As mentioned above, although embodiment of this invention is described, this invention is not limited to a specific embodiment, Various deformation|transformation and change are possible within the scope of the invention described in a claim.

[0083] This application claims the benefit of priority based on Japanese Patent Application No. 2022-061122 filed on March 31, 2022, the entire contents of which are incorporated herein by reference.

Claims

1. A method for preparing a processed silicon dioxide dispersed monomer composition, comprising: A silane-treated silica dispersion is prepared by mixing an alkaline silica dispersion in which silica is dispersed in a solvent containing 10% by mass or more of water with a silane coupling agent. The silane-treated silica dispersion is mixed with a polymerizable monomer to obtain a mixture, The aqueous phase is removed from the mixture to obtain a composition in which silica treated with a silane coupling agent is dispersed in a polymerizable monomer.

2. The method for producing a treated silica-dispersed monomer composition according to claim 1, The polymerizable monomer is a polymerizable monomer having a (meth)acryloyloxy group.

3. The method for producing a treated silica-dispersed monomer composition according to claim 2, The polymerizable monomer having a (meth)acryloyloxy group is a di(meth)acrylate.

4. The method for producing a treated silica-dispersed monomer composition according to any one of claims 1 to 3, The silane coupling agent is a silane coupling agent having a (meth)acryloyloxy group.

5. The method for producing a treated silica-dispersed monomer composition according to any one of claims 1 to 4, The pH of the silicon dioxide dispersion is 9-11.

6. The method for producing a treated silica-dispersed monomer composition according to any one of claims 1 to 5, The silicon dioxide is colloidal silicon dioxide.

7. The method for producing a treated silica-dispersed monomer composition according to any one of claims 1 to 6, The solvent contains sodium ions.

8. The method for producing a treated silica-dispersed monomer composition according to any one of claims 1 to 7, Removing the aqueous phase from the mixture includes stirring by adding water or acidic water to remove the separated aqueous phase.

9. The method for producing a treated silica-dispersed monomer composition according to any one of claims 1 to 8, It comprises heating at 80°C to 150°C after removing the aqueous phase.