Urethane prepolymer composition, moisture-curable adhesive, laminate, and synthetic artificial leather
By using a carbamate prepolymer composition containing polyester polyol and toluene diisocyanate trimethylolpropane adduct in synthetic artificial leather, the softness and heat resistance of the cured layer are solved through the moisture curing reaction. The problem of unbalanced properties and storage stability has achieved excellent results in softness, heat resistance and solvent resistance.
Patent Information
- Application Number
- CN202380027320.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-05
AI Technical Summary
When the conventional urethane prepolymer composition is produced in synthetic artificial leather, the softness, heat resistance and storage stability of the cured product layer are unbalanced, and the solvent resistance is insufficient.
The cured product layer is formed by a moisture curing reaction using a urethane prepolymer composition containing 5 to 90% by mass of polyester polyol and 0.2 to 25% by mass of toluene diisocyanate trimethylolpropane adduct. The isocyanate group content is controlled to be 1.0 to 6.0 mass %, so as to improve flexibility, heat resistance and solvent resistance.
It has achieved the formation of a cured product layer with excellent storage stability, flexibility, heat resistance and solvent resistance, which is suitable for the manufacture of synthetic artificial leather.
Smart Images

Figure BDA0005040723790000111 
Figure BDA0005040723790000121 
Figure BDA0005040723790000161
Abstract
Description
Technical Field
[0001] The present invention relates to a urethane prepolymer composition, a moisture-curing adhesive, a laminate and a synthetic artificial leather. Background Art
[0002] Urethane prepolymers are used in adhesives, coatings, and sealant materials. Among them, moisture-curing urethane prepolymers cure under the presence of moisture in the air, and therefore have the advantage of being usable as a single component. Such urethane prepolymers are compounds having functional groups such as isocyanate groups (NCO groups) in the molecule that react with water (moisture) present in the air or in the coated substrate to form a cross-linked structure. Urethane prepolymers are uncured and are in liquid or solid form at room temperature, and a variety of them have been developed depending on the intended use.
[0003] For example, a moisture-curing hot melt composition has been proposed, which contains: a urethane prepolymer having a structure derived from a polyol including a polyester polyol; and a polyfunctional isocyanate such as polymerized MDI (Patent Document 1). In addition, a reactive adhesive has been proposed, which contains: a urethane prepolymer having a structure derived from a polyol such as a polyether polyol; and a polyisocyanate such as an HDI trimer (Patent Document 2). Furthermore, a moisture-curing adhesive composition has been proposed, which contains: a urethane prepolymer and polymerized MDI (Patent Document 3).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6836713
[0007] Patent Document 2: Japanese Patent Application No. 2003-515636
[0008] Patent Document 3: Japanese Patent Application Publication No. 2005-75877 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] However, carbamate prepolymers are also used as adhesives for manufacturing artificial leathers such as artificial leather and synthetic leather. Synthetic leather is used as a material for manufacturing various products such as shoes, clothes, bags, furniture, and vehicle interior materials (such as dashboards, doors, consoles, and seats). Synthetic leather is usually a laminated body in which an epidermis layer, an adhesive layer (cured layer), and a substrate layer are stacked in sequence, and the cured layer is formed by various carbamate prepolymers. For the cured layer constituting the synthetic leather used in the above-mentioned various products, it is required not only to have good flexibility, but also to have heat resistance that can withstand the heat during manufacturing and processing.
[0011] However, it cannot be said that the softness and heat resistance of the cured product layer formed by curing the conventional adhesives proposed in Patent Documents 1 to 3 are well-balanced and excellent. In addition, the conventional adhesives are prone to viscosity changes during storage, and the storage stability cannot be said to be necessarily good. In addition, there is also room for improvement in the solvent resistance of the formed cured product layer.
[0012] The present invention is made in view of the problems of the prior art, and its subject is to provide: a urethane prepolymer composition capable of forming a cured product layer having excellent storage stability, flexibility, heat resistance, and solvent resistance, and a moisture-curable adhesive using the urethane prepolymer composition. In addition, the present invention is to provide: a laminate and a synthetic artificial leather using the urethane prepolymer composition.
[0013] Solutions for solving problems
[0014] That is, according to the present invention, there is provided the urethane prepolymer composition shown below.
[0015] [1] A urethane prepolymer composition comprising: a urethane prepolymer (C) which is a reaction product of a polyol (A) and a polyisocyanate (B); and a trimethylolpropane adduct (D) of toluene diisocyanate, wherein the polyol (A) contains 5 to 90% by mass of a polyester polyol (A-1), wherein the polyester polyol (A-1) has a structural unit derived from an aromatic dicarboxylic acid, and the content of the trimethylolpropane adduct (D) of toluene diisocyanate is 0. .2 to 25 parts by mass, the isocyanate content based on the total of the aforementioned urethane prepolymer (C) and the aforementioned trimethylolpropane adduct (D) of toluene diisocyanate is 1.0 to 6.0% by mass, the aforementioned polyol (A) also contains at least one other polyol (A-2) selected from the group consisting of polyester polyols (wherein the aforementioned polyester polyol (A-1) is not included), polyether polyols, and polycarbonate polyols, and the proportion of the aforementioned other polyols (A-2) in the aforementioned polyol (A) is 10 to 95% by mass.
[0016] [2] The urethane prepolymer composition according to [1] above, wherein the urethane prepolymer (C) does not contain a resin having a carboxyl group or an aminosulfonic acid (salt) group.
[0017] [3] The urethane prepolymer composition according to [1] or [2], wherein the proportion of the polyester polyol (A-1) in the polyol (A) is 5 to 70% by mass, and the proportion of the other polyol (A-2) in the polyol (A) is 30 to 95% by mass.
[0018] [4] The urethane prepolymer composition according to any one of [1] to [3], wherein the molar ratio (NCO group / OH group) of the polyisocyanate (B) to the polyol (A) is 1.3 to 2.0.
[0019] [5] The urethane prepolymer composition according to any one of [1] to [4], wherein the melt viscosity of the urethane prepolymer (C) at 100°C is 110 dPa·s or less.
[0020] Furthermore, according to the present invention, there are provided the moisture-curable adhesive, laminated body and synthetic artificial leather shown below.
[0021] [6] A moisture-curable adhesive comprising the urethane prepolymer composition according to any one of [1] to [5].
[0022] [7] A laminate comprising: a substrate; and a cured product layer formed on the substrate and comprising a cured product of the moisture-curable adhesive according to [6] above.
[0023] [8] A synthetic artificial leather comprising: a skin layer; a cured product layer formed from a cured product of the moisture-curable adhesive according to [6] and disposed on the skin layer; and a base material layer disposed on the cured product layer.
[0024] Effects of the Invention
[0025] According to the present invention, there can be provided: a urethane prepolymer composition capable of forming a cured product layer having excellent storage stability and excellent flexibility, heat resistance, and solvent resistance, and a moisture-curable adhesive using the urethane prepolymer composition. In addition, according to the present invention, there can be provided: a laminate and a synthetic artificial leather using the urethane prepolymer composition. DETAILED DESCRIPTION
[0026] <Urethane prepolymer composition>
[0027] Hereinafter, the embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. One embodiment of the urethane prepolymer composition of the present invention contains: a urethane prepolymer (C) as a reactant of a polyol (A) and a polyisocyanate (B); and a trimethylolpropane adduct (D) of toluene diisocyanate. The polyol (A) contains 5 to 90% by mass of a polyester polyol (A-1), and the polyester polyol (A-1) has a structural unit derived from an aromatic dicarboxylic acid. In addition, the content of the trimethylolpropane adduct (D) of toluene diisocyanate is 0.2 to 25 parts by mass relative to 100 parts by mass of the urethane prepolymer (C). Moreover, the isocyanate group content based on the total of the urethane prepolymer (C) and the trimethylolpropane adduct (D) of toluene diisocyanate is 1.0 to 6.0% by mass. Hereinafter, the details of the urethane prepolymer composition of the present embodiment will be described.
[0028] (Urethane prepolymer (C))
[0029] The urethane prepolymer (C) (hereinafter, also referred to as "prepolymer (C)") is a reaction product of a polyol (A) and a polyisocyanate (B). The molar ratio (NCO group / OH group) of the polyisocyanate (B) to the polyol (A) constituting the prepolymer (C) is preferably 1.1 to 2.2, more preferably 1.3 to 2.0, and particularly preferably 1.4 to 1.9. By making the molar ratio (NCO group / OH group) of the isocyanate group (NCO group) of the polyisocyanate (B) relative to the hydroxyl group (OH group) of the polyol (A) within the above range, the processability is improved, and a synthetic artificial leather with a better hand feel can be produced. If the NCO group / OH group (molar ratio) exceeds 2.2, the softness of the formed cured layer sometimes becomes easy to decrease. It should be noted that the urethane prepolymer (C) does not contain a resin having a carboxyl group or an aminosulfonic acid (salt) group. That is, the urethane prepolymer (C) does not contain a resin having a carboxyl group or a resin having an aminosulfonic acid (salt) group.
[0030] The melt viscosity of the prepolymer (C) at 100°C is preferably 120 dPa·s or less, more preferably 110 dPa·s or less, and particularly preferably 105 dPa·s or less. If the melt viscosity of the prepolymer (C) exceeds 120 dPa·s, it becomes viscous, the operability becomes easily reduced, and sometimes the processing becomes difficult. The melt viscosity of the prepolymer (C) can be controlled by, for example, the proportion of the polyester polyol (A-1) in the polyol (A). It should be noted that the melt viscosity of the prepolymer (C) at 100°C can be measured using a cone and plate viscometer.
[0031] From the viewpoint of physical properties after curing, such as the softness when forming synthetic artificial leather, the isocyanate group (NCO group) content of the prepolymer (C) is preferably 0.5 to 8.0 mass %, more preferably 1.0 to 6.0 mass %, and particularly preferably 1.5 to 4.0 mass %. The "NCO group content (mass %)" in this specification is a value measured by potentiometric titration in accordance with JIS K 1603-1:2007.
[0032] [Polyol (A)]
[0033] The polyol (A) comprises a polyester polyol (A-1) having a structural unit derived from an aromatic dicarboxylic acid. As the aromatic dicarboxylic acid, isophthalic acid, terephthalic acid, etc. can be cited. Among them, if melt viscosity, softness, etc. are considered, isophthalic acid is preferred. It should be noted that the polyol (A) is preferably a diol having two hydroxyl groups in one molecule.
[0034] Polyester polyol (A-1) is usually a reaction product of an aromatic dicarboxylic acid and a glycol. Examples of the glycol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,2-propylene glycol, n-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, isohexanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 1,9-nonanediol, and neopentyl glycol.
[0035] In the polyol (A), the proportion of the polyester polyol (A-1) is 5 to 90% by mass, preferably 10 to 80% by mass, more preferably 20 to 70% by mass, and particularly preferably 25 to 60% by mass. By making the proportion of the polyester polyol (A-1) in the polyol (A) within the above range, a prepolymer (C) having good operability and a moderate melt viscosity during, for example, gravure coating can be formed.
[0036] The number average molecular weight (Mn) of the polyester polyol (A-1) is preferably 4000 or less, more preferably 3000 or less, and particularly preferably 2800 or less. If the number average molecular weight (Mn) of the polyester polyol (A-1) exceeds 4000, the viscosity becomes excessively high, so that the practicality is sometimes reduced. There is no particular limitation on the lower limit of the number average molecular weight (Mn) of the polyester polyol (A-1), for example, it is preferably 500 or more. It should be noted that the "number average molecular weight (Mn)" in this specification is a value converted to polystyrene measured by gel permeation chromatography (GPC).
[0037] The polyol (A) usually further includes other polyols (A-2) other than the polyester polyol (A-1). The other polyol (A-2) is at least one selected from the group consisting of polyester polyols (excluding the polyester polyol (A-1)), polyether polyols, and polycarbonate polyols.
[0038] As polyester polyols other than polyester polyol (A-1), a reaction product of an aliphatic dicarboxylic acid and a diol can be used. Examples of the aliphatic dicarboxylic acid include succinic acid, adipic acid, sebacic acid, glutaric acid, and azelaic acid. Examples of the diols include the same diols as those that can constitute the polyester polyol (A-1).
[0039] Examples of the polyether polyol include polyethylene glycol, polypropylene glycol, polyethylene glycol-polytetramethylene glycol (block or random), polytetramethylene glycol, and polyhexamethylene glycol. Among them, polytetramethylene glycol is preferred from the viewpoint of flexibility.
[0040] Examples of the polycarbonate polyol include polytetramethylene carbonate diol, polypentamethylene carbonate diol, polyneopentyl carbonate diol, polyhexamethylene carbonate diol, poly(1,4-cyclohexanedimethylene carbonate) diol, and random / block copolymers thereof.
[0041] In the polyol (A), the ratio of other polyols (A-2) is preferably 10 to 95% by mass, more preferably 20 to 90% by mass, particularly preferably 30 to 80% by mass, and most preferably 40 to 75% by mass. It should be noted that in the polyol (A), the total of polyester polyol (A-1) and other polyols (A-2) is preferably 100% by mass. By further including other polyols (A-2) in the polyol (A), a cured product layer with better flexibility can be formed.
[0042] The number average molecular weight (Mn) of the other polyol (A-2) is preferably 4000 or less, more preferably 3000 or less, and particularly preferably 2800 or less. If the number average molecular weight (Mn) of the other polyol (A-2) exceeds 3000, the viscosity becomes excessively high, so that the practicality may be reduced. It should be noted that the number average molecular weight (Mn) of the other polyol (A-2) is preferably 500 or more. That is, the other polyol (A-2) preferably does not contain so-called short-chain diols (low molecular weight diols) such as neopentyl glycol.
[0043] [Polyisocyanate (B)]
[0044] As the polyisocyanate, bifunctional polyisocyanates such as aliphatic diisocyanate, alicyclic diisocyanate and aromatic diisocyanate are preferably used.
[0045] Specific examples of polyisocyanates include toluene diisocyanate, 4-methoxy-1,3-phenylene diisocyanate, 4-isopropyl-1,3-phenylene diisocyanate, 4-chloro-1,3-phenylene diisocyanate, 4-butoxy-1,3-phenylene diisocyanate, 2,4-diisocyanate-diphenyl ether, mesitylene diisocyanate, 4,4'-diphenylmethane diisocyanate, durylene diisocyanate, diisocyanate), 1,5-naphthalene diisocyanate, benzidine diisocyanate, o-nitrobenzidine diisocyanate, 4,4-diisocyanate benzyl, 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,10-decamethylene diisocyanate, 1,4-cyclohexylene diisocyanate, xylene diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), 1,5-tetrahydronaphthalene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane 4,4'-diisocyanate. Among them, 4,4'-diphenylmethane diisocyanate (MDI) is preferred.
[0046] (Method for producing urethane prepolymer (C))
[0047] For example, the prepolymer (C) can be produced by reacting the polyol (A) and the polyisocyanate (B) at preferably 20 to 150° C., more preferably 60 to 110° C., until the product reaches a theoretical NCO group content (mass %) by a one-step method or a multi-step method. When the polyol (A) and the polyisocyanate (B) are reacted, a catalyst can be used in combination as needed. Examples of the catalyst include metal salts such as dibutyltin laurate, dioctyltin laurate, stannous octoate, lead octoate, tetra-n-butyl titanate, and organometallic derivatives; organic amines such as triethylamine; diazabicycloundecene-based catalysts; and the like.
[0048] The polyol (A) and the polyisocyanate (B) are preferably reacted in the absence of a solvent such as an organic solvent, that is, in the absence of a solvent. By reacting the polyol (A) and the polyisocyanate (B) in the absence of a solvent such as an organic solvent, a solvent-free urethane prepolymer (C) can be obtained.
[0049] (Trimethylolpropane adduct of toluene diisocyanate (D))
[0050] The urethane prepolymer composition of the present embodiment contains a trimethylolpropane adduct (D) of toluene diisocyanate (hereinafter also referred to as "TDI adduct (D)"). By containing the TDI adduct (D), a urethane prepolymer composition useful as a one-component moisture-curing adhesive that can form an adhesive layer (cured material layer) having improved heat resistance can be obtained. Furthermore, by containing the TDI adduct (D), a urethane prepolymer composition that can form a cured material layer having excellent heat resistance as well as excellent flexibility and solvent resistance can be obtained.
[0051] In the urethane prepolymer composition, the content of the TDI adduct (D) is 0.2 to 25 parts by mass, preferably 0.3 to 20 parts by mass, more preferably 0.5 to 18 parts by mass, and particularly preferably 1.0 to 15 parts by mass, relative to 100 parts by mass of the urethane prepolymer (C). By setting the content of the TDI adduct (D) within the above range, a urethane prepolymer composition capable of forming a cured layer having excellent flexibility, heat resistance, and solvent resistance can be obtained. If the content of the TDI adduct (D) is less than 0.2 parts by mass relative to 100 parts by mass of the prepolymer (C), a cured layer showing sufficient heat resistance and solvent resistance cannot be formed. On the other hand, if the content of the TDI adduct (D) exceeds 25 parts by mass relative to 100 parts by mass of the prepolymer (C), the flexibility of the formed cured layer decreases, and the storage stability of the urethane prepolymer composition decreases.
[0052] The isocyanate group (NCO group) content (hereinafter also referred to as "total NCO group content") based on the total of the prepolymer (C) and the TDI adduct (D) is 1.0 to 6.0% by mass, preferably 1.1 to 5.0% by mass, and more preferably 1.2 to 4.0% by mass. By making the total NCO group content within the above range, a urethane prepolymer composition having excellent storage stability and capable of forming a cured layer having excellent flexibility, heat resistance, and solvent resistance can be prepared. If the total NCO group content is less than 1.0% by mass, the heat resistance of the cured layer formed is reduced. On the other hand, if the total NCO group content exceeds 6.0% by mass, the softness of the cured layer formed becomes insufficient.
[0053] <Moisture curing adhesive>
[0054] One embodiment of the moisture-curable adhesive of the present invention contains the above-mentioned urethane prepolymer composition. The moisture-curable adhesive of this embodiment is suitable as a one-component adhesive for producing synthetic artificial leather and is particularly suitable as a one-component adhesive for producing various laminates.
[0055] The moisture-curable adhesive of the present embodiment may be mixed with various additives such as appropriate amounts of thermoplastic resins, tackifying resins, catalysts, pigments, antioxidants, ultraviolet absorbers, surfactants, flame retardants, fillers, and foaming agents as needed. Among them, the moisture-curable adhesive of the present embodiment is preferably substantially composed of the aforementioned urethane prepolymer composition. The moisture-curable adhesive of the present embodiment is suitable as an adhesive for synthetic leather.
[0056] The adhesive of this embodiment can facilitate the bonding of adherends by applying it to the surface of the adherend. Examples of adherends other than the substrate layer for synthetic leather include metal and non-metal (polycarbonate, glass, etc.) substrates.
[0057] <Laminated body>
[0058] One embodiment of the laminate of the present invention comprises: a film-like or sheet-like substrate; and a cured product layer formed by a cured product of the aforementioned moisture-curable adhesive disposed on the substrate. That is, the laminate of the present embodiment comprises: a cured product layer (adhesive layer) formed by curing a coating film formed by applying the aforementioned moisture-curable adhesive, etc., using moisture. As the substrate, in addition to the epidermis layer and substrate layer for synthetic leather, optical films, optical plates, flexible printed circuit boards, glass substrates, and substrates on which ITO is vapor-deposited, etc., can also be cited.
[0059] The moisture-curable adhesive is applied to the substrate by a known method such as comma coating, knife coating, roll coating, etc. to form a coating film, and then the formed coating film is moisture-cured to form a cured product layer, thereby obtaining a laminate.
[0060] <Synthetic leather>
[0061] One embodiment of the synthetic leather of the present invention comprises: an epidermis layer; a cured product layer formed of a cured product of the moisture-curing adhesive disposed on the epidermis layer; and a base material layer such as a base fabric disposed on the cured product layer. As the base fabric constituting the base material layer, for example, woven fabrics including twill, plain weave, etc., raised fabrics obtained by mechanically raising the cotton grey fabric of the woven fabric, rayon fabric, nylon fabric, polyester fabric, Kvela fabric, non-woven fabric (polyester, nylon, various latexes), various films, sheets, etc. can be cited. In addition, as the epidermis layer, those formed by coatings for epidermis layer formation such as solvent-based polyurethane, water-based polyurethane, TPU, etc. can be cited.
[0062] The synthetic artificial leather can be manufactured, for example, as follows. First, a coating for forming an epidermis layer is applied to release paper using known methods such as comma coating, knife coating, roller coating, gravure coating, die coating, and spraying. The applied coating is suitably dried to form an epidermis layer, and then the moisture-curing adhesive is applied to the formed epidermis layer using known methods such as comma coating, knife coating, and roller coating. After the applied moisture-curing adhesive is pressure-bonded to the substrate layer at 75 to 155° C., it is aged under prescribed conditions as required. Then, it is peeled off from the release paper, thereby obtaining the target synthetic artificial leather. The synthetic artificial leather of the present embodiment is suitable as a material for constituting shoes, clothing, bags, furniture, vehicle interior materials (e.g., dashboards, doors, consoles, seats), and the like.
[0063] Example
[0064] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. It should be noted that "parts" and "%" in Examples and Comparative Examples are based on mass unless otherwise specified.
[0065] <Manufacturing of prepolymer>
[0066] (Production Example 1)
[0067] In a glass reaction container equipped with a stirrer, a thermometer, and a gas inlet, 10 parts of isophthalic acid polyester polyol (Mn: 2000), 90 parts by mass of polytetramethylene glycol 2000 (PTMG2000) (Mn: 2000, manufactured by Mitsubishi Chemical Corporation), and 16.3 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added. As the isophthalic acid polyester polyol, a polyester polyol formed by isophthalic acid and 1,4-butanediol (1,4-BD) was used. In addition, the molar ratio (NCO group / OH group) of the NCO group of MDI to the OH group of the polyol (isophthalic acid polyester polyol and PTMG2000) was set to 1.3. After heating and decompression, a dehydration treatment was performed, and nitrogen was sealed. Stirring and reacting at an internal temperature of 100°C for 120 minutes to obtain a prepolymer (C-1). The obtained prepolymer (C-1) had a viscosity at 100°C of 95 dPa·s and an NCO group content of 1.08%.
[0068] (Production Examples 2 to 14)
[0069] Prepolymers (C-2) to (C-14) were obtained in the same manner as in the above-mentioned Production Example 1 except that the formulations shown in Tables 1-1 and 1-2 were used. The properties of the obtained prepolymers are shown in Tables 1-1 and 1-2. It should be noted that the meanings of the abbreviations in Tables 1-1 and 1-2 are shown below. In addition, the "polycarbonate polyol" in Tables 1-1 and 1-2 is a polycarbonate diol based on 1,6-hexanediol (trade name "ETERNACOLL UH-200", manufactured by Ube Industries, Ltd.).
[0070] 1,4-BD: 1,4-Butanediol
[0071] IPA: Isophthalic acid
[0072] PTMG2000: Polytetramethylene glycol 2000
[0073] AA: Adipic acid
[0074] 1,6-HD: 1,6-Hexanediol
[0075] ·TPA: terephthalic acid
[0076] ·NPG: Neopentyl Glycol
[0077] Table 1-1 (Unit in the middle section: copies)
[0078]
[0079] Table 1-2 (Unit in the middle section: copies)
[0080]
[0081] <Production of prepolymer composition>
[0082] (Example 1)
[0083] 0.67 parts of TDI adduct (trade name "Takenate D-103H", manufactured by Mitsui Chemicals, Inc., NCO group content: 13.0%, solid content: 75%) were added to 100 parts of the prepolymer (C-1) obtained in Production Example 1 (in terms of non-volatile components). The amount of TDI adduct (non-volatile components) was 0.3 parts per 100 parts of the non-volatile components of the prepolymer (C-1). The mixture was heated and decompressed while being stirred to obtain a prepolymer composition. The total NCO group content of the obtained prepolymer composition was 1.13%.
[0084] (Examples 2 to 15, Comparative Examples 1 to 12)
[0085] Prepolymer compositions were obtained in the same manner as in Example 1 except that the formulations shown in Tables 2-1 to 2-3 were used. The total NCO group contents of the obtained prepolymer compositions are shown in Tables 2-1 to 2-3. The details of the components in Tables 2-1 to 2-3 are shown below.
[0086] · Polymeric MDI: Trade name "Lupranate M20S", manufactured by BASF INOAC Polyurethanes Ltd.
[0087] ·HDI urea ester body: Trade name "Duranate TPA-100", manufactured by Asahi Kasei Co., Ltd.
[0088] ·HDI adduct: Trade name "Duranate AE700-100", manufactured by Asahi Kasei Co., Ltd.
[0089] ·HDI biuret: Trade name "Duranate 24A-100", manufactured by Asahi Kasei Co., Ltd.
[0090] <Manufacturing of synthetic leather>
[0091] After applying a solution-type urethane resin (trade name "RESAMIN NE-8875-30M", manufactured by Dainichi Seika Industries Co., Ltd.) on release paper, it was dried at 120°C for 5 minutes to form a skin layer with a thickness of 40 μm. On the other hand, each of the manufactured prepolymer compositions (moisture-curing adhesives) was applied to another release paper and aged for 48 hours at 25°C and 60RH% to form an adhesive layer with a thickness of 100 μm. The adhesive layer peeled off from the release paper was clamped between the skin layer and the base cloth (test polyester mesh raw material). Using a sealing machine, laminated for 30 seconds at 170°C and 0.15MPa in a state where a heat source is arranged on the side of the release paper in contact with the skin layer. Afterwards, the release paper in contact with the skin layer was peeled off to obtain synthetic artificial leather.
[0092] <Evaluation>
[0093] (Softness)
[0094] An adhesive was prepared by mixing 100 parts of a polyurethane resin adhesive (trade name "RESAMIN UD-8351NT", manufactured by Dainichi Seika Industries, Ltd.) and 10 parts of an isocyanate crosslinking agent (trade name "C-50 crosslinking agent", manufactured by Dainichi Seika Industries, Ltd.). The prepared adhesive was applied to the surface layer on the release paper formed in the aforementioned "Manufacture of synthetic artificial leather" to form an adhesive layer with a film thickness of 100 μm. After pre-drying the formed adhesive layer at 80°C for 2 minutes, it was press-bonded to the substrate (woven fabric) under the condition of a laminating roller temperature of 40°C. After that, it was aged at 50°C for 48 hours to obtain a standard synthetic artificial leather for softness evaluation.
[0095] The softness of the synthetic leather was evaluated by comparing the touch of the manufactured synthetic leather and the standard synthetic leather according to the following evaluation criteria. The results are shown in Tables 2-1 to 2-3. It should be noted that "◎", "○", and "△" are recorded as passing.
[0096] ◎: Softer than standard synthetic leather.
[0097] ○: As soft as standard synthetic leather.
[0098] △: Slightly harder than standard synthetic leather.
[0099] ×: Much harder than standard synthetic leather.
[0100] (Heat resistance)
[0101] The prepolymer composition heated to 100°C is applied to release paper. After aging for more than 48 hours at 25°C and 60RH%, it is peeled off from the release paper to obtain a translucent film with a thickness of 50μm, a width of 8cm, and a length of 15cm. The obtained film is subjected to a heat resistance test at 120°C for 400 hours. Using a tensile testing device (model name "AutographAGS-100A", manufactured by Shimadzu Corporation), the breaking strength of the film before and after the heat resistance test is measured at 25°C and a tensile speed of 200mm / min, and the heat resistance is evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3. It should be noted that "◎" and "○" are recorded as qualified.
[0102] ◎: The retention rate of breaking strength is 50% or more.
[0103] ○: The retention rate of breaking strength is 25% or more and less than 50%.
[0104] ×: The retention rate of breaking strength was less than 25%, or the film was dissolved.
[0105] (Shelf life (storage stability))
[0106] The prepared prepolymer composition was placed in a container and stored at 100°C for 8 hours with the container opened. The viscosity of the prepolymer composition before and after storage was measured, and the pot life was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3. It should be noted that "◎" and "○" are recorded as passing.
[0107] ◎: The viscosity change rate is less than 150%.
[0108] ○: The viscosity change rate is 150% or more and less than 250%.
[0109] ×: The viscosity change rate is 250% or more.
[0110] (Solvent resistance)
[0111] The prepolymer composition heated to 100°C is applied on release paper. After aging at 25°C and 60RH% for more than 48 hours, it is peeled off from the release paper to obtain a translucent film with a thickness of 50μm, a width of 5cm and a length of 5cm. The obtained film is immersed in acetone for 10 minutes and then taken out. The linear swelling ratio of the removed film is calculated (={(width of the film after immersion) / (width of the film before immersion)}×100(%)), and the solvent resistance is evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3. It should be noted that "◎" and "○" are recorded as qualified.
[0112] ◎: The linear swelling ratio of one side of the film is less than 120%.
[0113] ○: The linear swelling ratio of one side of the film is 120% or more and less than 150%.
[0114] △: The linear swelling ratio of one side of the film is 150% or more.
[0115] ×: The film was dissolved.
[0116] Table 2-
[0117]
[0118] Table 2-2
[0119]
[0120] Table 2-3
[0121]
[0122] It is known that by using the TDI adduct, the mechanical strength such as solvent resistance required for the use of synthetic artificial leather is improved compared with the case of using aliphatic polyisocyanates such as HDI. It is also known that by using the TDI adduct, the softness and pot life that cannot be obtained when using polymeric MDI are improved. It should be noted that even when the TDI adduct is used, it is known that the softness of the obtained synthetic artificial leather is poor unless the polyol (A) containing a specific amount of polyester polyol (A-1) having a structural unit derived from an aromatic dicarboxylic acid is used (Comparative Example 6).
[0123] Industrial Applicability
[0124] The urethane prepolymer composition of the present invention is useful as an adhesive for producing synthetic artificial leather and various laminates.
Claims
1. A urethane prepolymer composition comprising: a urethane prepolymer (C) which is a reactant of a polyol (A) and a polyisocyanate (B); and trimethylolpropane adduct of toluene diisocyanate (D), The polyol (A) contains 5 to 90% by mass of a polyester polyol (A-1), wherein the polyester polyol (A-1) has a structural unit derived from an aromatic dicarboxylic acid. The content of the trimethylolpropane adduct of toluene diisocyanate (D) is 0.2 to 25 parts by mass relative to 100 parts by mass of the urethane prepolymer (C). The isocyanate group content based on the total amount of the urethane prepolymer (C) and the trimethylolpropane adduct (D) of toluene diisocyanate is 1.0 to 6.0% by mass. The polyol (A) further comprises a polyester polyol (wherein, does not contain at least one other polyol (A-2) selected from the group consisting of the polyester polyol (A-1)), polyether polyol, and polycarbonate polyol, In the polyol (A), the ratio of the other polyol (A-2) is 10 to 95% by mass.
2. The urethane prepolymer composition according to claim 1, wherein The urethane prepolymer (C) does not contain a resin having a carboxyl group or an aminosulfonic acid (salt) group.
3. The urethane prepolymer composition according to claim 1 or 2, wherein In the polyol (A), the proportion of the polyester polyol (A-1) is 5 to 70% by mass. In the polyol (A), the ratio of the other polyol (A-2) is 30 to 95% by mass.
4. The urethane prepolymer composition according to any one of claims 1 to 3, wherein The molar ratio (NCO group / OH group) of the polyisocyanate (B) to the polyol (A) is 1.3 to 2.
0.
5. The urethane prepolymer composition according to any one of claims 1 to 4, wherein The melt viscosity of the urethane prepolymer (C) at 100° C. is 110 dPa·s or less. 6 . A moisture-curable adhesive comprising the urethane prepolymer composition according to claim 1 .
7. A laminate comprising: substrate; and, A cured product layer formed of a cured product of the moisture-curable adhesive according to claim 6 and provided on the substrate.
8. A synthetic leather comprising: Epidermis; a cured product layer formed of a cured product of the moisture-curable adhesive according to claim 6 and provided on the skin layer; and A base material layer is provided on the cured product layer.
Citation Information
Patent Citations
Adhesion promoter for monomer-free reactive polyurethanes
JP2003515636A
Moisture-curable hot-melt adhesive composition
JP2005075877A