Highly functionalized stable alkoxysilyl polydienes and polydiene copolymers

By using a blend of monohydrogenoxysilyl and dihydrogenoxysilyl functionalized polydiene copolymers in tire tread manufacturing, the problem of limited performance of vulcanized rubber in the prior art is solved, and the problem of achieving the achievement of the following methods Higher functionalization and improved vulcanized rubber properties reduce alcohol production.

CN118900883APending Publication Date: 2024-11-05BRIDGESTONE AMERICAS TIRE OPERATIONS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027174.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-17
Filing Date
2023-02-17
Publication Date
2024-11-05

Smart Images

  • Figure BDA0005039948830000111
    Figure BDA0005039948830000111
  • Figure BDA0005039948830000112
    Figure BDA0005039948830000112
  • Figure BDA0005039948830000151
    Figure BDA0005039948830000151
Patent Text Reader

Abstract

A polymer composition, the polymer composition comprising a plurality of functionalized polymers wherein the plurality of functionalized polymers comprise a monohydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer and a dihydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer, and wherein the plurality of functionalized polymers comprise at least one of a monohydrocarbyloxysilyl functionalized polydiene and a dihydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer. The polymer composition has an aged Mooney (ML1 + 4 at100 DEG C) of from about 40 to about 105, where greater than 60 mol% of the polymer in the polymer composition is functionalized, and where the plurality of including from about 15 mol% to about 70 mol% of the plurality of functionalized polymers are monohydrocarbyloxysilyl functionalized polydienes and / or polydiene copolymers, wherein the remainder comprises a dialkoxysilyl functionalized polydiene and / or a polydiene copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention are directed to hydrocarbyloxysilyl functionalized polydienes and polydiene copolymers characterized by high functionality and long term stability against deleterious Mooney growth. According to embodiments of the present invention, the hydrocarbyloxysilyl functionalized polydienes and polydiene copolymers include blends of monohydrocarbyloxysilyl functionalized polydienes and polydiene copolymers and dihydrocarbyloxysilyl functionalized polydienes and polydiene copolymers. Background Art

[0002] In the manufacture of tires, particularly tire treads, it is known to employ modified polymers, such as those including terminal functionalizations. It has been observed that rubber vulcanizates prepared with these modified polymers exhibit reduced hysteresis losses and show reduced Payne effect, which is the loss of mechanical energy caused by filler depolymerization.

[0003] Polymer modification is usually achieved by reacting a living polymer material with a compound that can impart functional groups to the ends of the polymer chain. For example, U.S. Pat. No. 6,369,167 teaches the preparation of diene polymers (such as random copolymers of butadiene and styrene) by anionic polymerization techniques, which are then terminated with imine-containing hydrocarbyloxysilane compounds. The end-capping compound (also known as a terminal modifier) ​​is employed in an amount of 0.25 to 3 moles per mole of the organolithium compound used to initiate anionic polymerization.

[0004] Similar terminal modifiers are disclosed in U.S. Pat. No. 7,683,151, which teaches the use of 0.3 molar equivalents or more based on apparent active sites. After the modification reaction, the patent teaches the addition of a condensation promoter (e.g., tin carboxylate) to achieve condensation of the hydrocarbyloxysilane residues at the polymer chain ends (which produces polymer coupling). After completion, the resulting modified polymer has a Mooney viscosity (ML) of 10 to 150. 1+4 @100℃).

[0005] Hydrocarbyloxysilane residues have been found to cause an increase in aged Mooney viscosity, which is believed to be caused by coupling between functional polymers in the presence of water. It is believed that when water hydrolyzes the hydrocarbyloxysilane substituent to form a siloxy substituent, the siloxy substituent of the corresponding polymer then undergoes condensation to achieve coupling, and this coupling is initiated. U.S. Patent No. 6,255,404 teaches that the polymer modified by treating it with an alkyl alkoxysilane (e.g., octyl triethoxysilane) stabilizes the hydrocarbyloxysilane end group to remedy this Mooney viscosity increase. Alkyl alkoxy silane can be added in an amount of 1 to 20 moles per mole of initiator, although when present in an amount higher than the equivalent of the alkoxysilane functionality, due to the plasticizing effect of the alkyl alkoxy silane (i.e., excessive alkyl alkoxy silane acts as an oil), a reduction in polymer viscosity is observed. Summary of the invention

[0006] One or more embodiments of the present invention provide a polymer composition comprising a plurality of functionalized polymers, wherein the plurality comprises a monohydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer and a dihydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer, the polymer composition having an aged Mooney (ML) of about 40 to about 105. 1+4 @100°C), wherein greater than 60 mol% of the polymers in the polymer composition are functionalized, and wherein the plurality comprising from about 15 mol% to about 70 mol% of the plurality of functionalized polymers are monohydrocarbyloxysilyl functionalized polydienes and / or polydiene copolymers, wherein the balance comprises dihydrocarbyloxysilyl functionalized polydienes and / or polydiene copolymers.

[0007] Other embodiments of the present invention provide a method for preparing a polymer composition, which includes (i) providing a reactive polydiene or polydiene copolymer; (ii) reacting a portion of the reactive polydiene or polydiene copolymer with a first end-capping agent, which is a trihydrocarbyloxysilyl compound; (iii) reacting a portion of the reactive polydiene or polydiene copolymer with a second end-capping agent, which is a dihydrocarbyloxysilyl compound, thereby forming a functionalized dihydrocarbyloxysilyl polydiene and / or polydiene copolymer, wherein the monohydrocarbyloxysilyl polydiene and the dihydrocarbyloxysilyl polydiene and / or polydiene copolymer form a blend; and (iv) separating the blend.

[0008] Still other embodiments of the present invention provide a vulcanizable rubber composition comprising (i) a polymer composition comprising a plurality of functionalized polymers, wherein the plurality comprises a monohydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer and a dihydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer, the polymer composition having an aged Mooney (ML) of about 40 to about 105. 1+4 @100°C), wherein greater than 60 mol% of the polymers in the polymer composition are functionalized, and wherein the plurality of functionalized polymers, including from about 15 mol% to about 70 mol%, are mono-hydrocarbyloxysilyl-functionalized polydienes and / or polydiene copolymers, with the balance comprising di-hydrocarbyloxysilyl-functionalized polydienes and / or polydiene copolymers; (ii) a filler; and (iii) a curing agent.

[0009] Still other embodiments of the present invention provide a vulcanized rubber prepared by vulcanizing a vulcanizable rubber composition, the vulcanizable rubber composition comprising (i) a polymer composition comprising a plurality of functionalized polymers, wherein the plurality comprises a monohydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer and a dihydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymer, the polymer composition having an aged Mooney (ML) of about 40 to about 105. 1+4 @100°C), wherein greater than 60 mol% of the polymers in the polymer composition are functionalized, and wherein the plurality of functionalized polymers, including from about 15 mol% to about 70 mol%, are mono-hydrocarbyloxysilyl-functionalized polydienes and / or polydiene copolymers, with the balance comprising di-hydrocarbyloxysilyl-functionalized polydienes and / or polydiene copolymers; (ii) a filler; and (iii) a curing agent. DETAILED DESCRIPTION

[0010] Embodiments of the present invention are based at least in part on the discovery of a process for producing highly functionalized polydiene or polydiene copolymer blend compositions, which compositions are characterized by favorable processability. According to embodiments of the present invention, the blend comprises a blend of monohydrocarbyloxysilyl functionalized polydiene and polydiene copolymers and dihydrocarbyloxysilyl functionalized polydiene and polydiene copolymers. Although prior art expectations stabilize hydrocarbyloxysilyl functionalized polydienes (e.g., treating them with stabilizers), it has been observed that the degree of functionalization (i.e., the molar percentage of the polymer with hydrocarbyloxysilyl functionality) is proportional to the amount of the required stabilizer (e.g., the use of octyltriethoxysilane), and from the viewpoint of polymer processing, the compromise between functionalization and stabilization is conducive to reducing the level of functionalization. However, at lower levels of functionalization, the potential benefits to vulcanized rubber performance are sacrificed. Therefore, the present invention advantageously provides higher functionalization (and therefore improved vulcanized rubber performance), while maintaining desired polymer properties. In fact, it has advantageously been found that the advantageous results of the present invention can be achieved in the absence of post-functionalization stabilization.

[0011] Preparation of polymer blends

[0012] In one or more embodiments, blends of monohydrocarbyloxysilyl functionalized polydienes and polydiene copolymers and dihydrocarbyloxysilyl functionalized polydienes and polydiene copolymers are prepared by: (i) anionically synthesizing reactive polydienes and / or polydiene copolymers, (ii) reacting a portion of the reactive polydienes and / or polydiene copolymers with a dihydrocarbyloxysilyl functionalizing agent to form functionalized monohydrocarbyloxysilyl polydiene and / or polydiene copolymers, (iii) reacting a portion of the reactive polydiene and / or polydiene copolymers with a trihydrocarbyloxysilyl functionalizing agent to form functionalized dihydrocarbyloxysilyl polydiene and / or polydiene copolymers, wherein the monohydrocarbyloxysilyl polydienes and dihydrocarbyloxysilyl polydiene and / or polydiene copolymers form a blend, and (iv) separating the blend.

[0013] Anionic synthesis of reactive polydiene

[0014] In one or more embodiments, reactive polydiene and polydiene copolymers are prepared by anionic polymerization of diene monomers, optionally together with monomers copolymerizable therewith. In one or more embodiments, polymerization comprises anionic polymerization of conjugated diene monomers (e.g., butadiene) and vinyl aromatic monomers (e.g., styrene) in solution to provide a polymerization mixture comprising polydiene polymers and copolymers having reactive polymer chain ends.

[0015] It is generally known to prepare polymers by using anionic polymerization techniques. The key mechanistic features of anionic polymerization have been described in books (e.g., Hsieh, HL; Quirk, RP Anionic Polymerization: Principles and Practical Applications; Marcel Dekker: New York, 1996) and review articles (e.g., Hadjichristidis, N.; Pitsikalis, M.; Pispas, S.; Iatrou, H.; Chem. Rev. 2001, 101 (12), 3747-3792 (Hadjichristidis, N., Pitsikalis, M., Pispas, S., Iatrou, H., "Chemical Reviews", 2001, Vol. 101, No. 12, pp. 3747-3792)). Anionic initiators can advantageously produce polymers with reactive chain ends (e.g., living polymers) that can react with additional monomers for further chain growth or with certain functionalizing agents to produce functionalized polymers prior to quenching. Polymers with reactive polymer chain ends may be referred to simply as reactive polymers. As will be appreciated by those skilled in the art, these reactive polymers include reactive chain ends believed to be ionic, at which a reaction of a functionalizing agent and the reactive chain end of the polymer may occur, thereby imparting functionality or functional groups to the polymer chain ends or which may couple multiple polymers together.

[0016] Monomers that can be anionically polymerized to form these polymers include conjugated diene monomers, which can optionally be copolymerized with other monomers such as vinyl-substituted aromatic monomers. Examples of conjugated diene monomers include 1,3-butadiene, isoprene, 1,3-pentadiene, 1,3-hexadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene and 2,4-hexadiene. A mixture of two or more conjugated dienes can also be used in copolymerization. Examples of monomers that can be copolymerized with conjugated diene monomers include vinyl-substituted aromatic compounds, such as styrene, p-methylstyrene, α-methylstyrene and vinylnaphthalene.

[0017] The practice of the present invention is not limited by the selection of any particular anionic initiator. Exemplary anionic initiators include organolithium compounds. In one or more embodiments, the organolithium compound may contain heteroatoms. In these or other embodiments, the organolithium compound may contain one or more heterocyclic groups. Types of organolithium compounds include alkyl lithium compounds, aryl lithium compounds, and cycloalkyl lithium compounds. Specific examples of organolithium compounds include ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, n-pentyl lithium, isopentyl lithium, and phenyl lithium. Other useful initiators include alkyl tin lithium compounds, such as trialkyl tin lithium. Still other anionic initiators include organosodium compounds, such as phenyl sodium and 2,4,6-trimethylphenyl sodium.

[0018] Anionic polymerization can be carried out in polar solvents, non-polar solvents and mixtures thereof. In one or more embodiments, a solvent can be used as a carrier to dissolve or suspend the initiator, thereby facilitating the delivery of the initiator to the polymerization system.

[0019] In one or more embodiments, suitable solvents include those organic compounds that do not polymerize or incorporate into the growing polymer chain during the polymerization of monomers in the presence of a catalyst. In one or more embodiments, these organic substances are liquid at ambient temperature and pressure. In one or more embodiments, these organic solvents are inert to the catalyst. Exemplary organic solvents include hydrocarbons with low or relatively low boiling points, such as aromatic hydrocarbons, aliphatic hydrocarbons and alicyclic hydrocarbons. Non-limiting examples of aromatic hydrocarbons include benzene, toluene, xylene, ethylbenzene, diethylbenzene and trimethylbenzene. Non-limiting examples of aliphatic hydrocarbons include n-pentane, n-hexane, n-heptane, n-octane, n-nonane, n-decane, isopentane, isohexane, isopentane, isooctane, 2,2-dimethylbutane, petroleum ether, kerosene and white spirit. Moreover, non-limiting examples of alicyclic hydrocarbons include cyclopentane, cyclohexane, methylcyclopentane and methylcyclohexane. A mixture of the above hydrocarbons can also be used. Usually, low boiling hydrocarbon solvents are separated from polymers when polymerization is completed. Other examples of organic solvents include high molecular weight, high boiling hydrocarbons such as paraffin oil, aromatic oils or other hydrocarbon oils commonly used to extend polymers. Since these hydrocarbons are non-volatile, they generally do not need to be separated and remain incorporated into the polymer.

[0020] Anionic polymerization can be carried out in the presence of a randomizer (which may also be referred to as a polar coordinating agent) or a vinyl modifier. As will be appreciated by those skilled in the art, these compounds, which can play a dual role, can help randomize the comonomers that run through the polymer chain and / or change the ethylene content of the mer units derived from the diene. Compounds suitable for use as randomizers include those having oxygen or nitrogen heteroatoms and non-bonded electron pairs. Examples include linear and cyclic oligomeric oxalyl alkanes, dialkyl ethers of mono- and oligomeric alkylene glycols (also known as glycol dimethyl ethers), "crown" ethers, tertiary amines, linear THF oligomers, and the like. Linear and cyclic oligomeric oxalyl alkanes are described in U.S. Patent Nos. 4,429,091 and 9,868,795, which are incorporated herein by reference. Specific examples of compounds that can be used as randomizers include 2,2-bis(2'-tetrahydrofuranyl)propane, 1,2-dimethoxyethane, N,N,N',N'-tetramethylethylenediamine (TMEDA), tetrahydrofuran (THF), 1,2-dipiperidylethane, dipiperidylmethane, hexamethylphosphoramide, N-N'dimethylpiperazine, diazabicyclooctane, dimethyl ether, diethyl ether, tri-n-butylamine, and mixtures thereof. In other embodiments, potassium alkoxides can be used to randomize styrene distribution.

[0021] The amount of randomizer to be employed may depend on various factors, such as the desired microstructure of the polymer, the ratio of monomer to comonomer, the polymerization temperature, and the nature of the specific randomizer employed. In one or more embodiments, the amount of randomizer employed may range from 0.01 mole to 100 moles per mole of anionic initiator.

[0022] The anionic initiator and the randomizer can be introduced into the polymerization system by various methods. In one or more embodiments, the anionic initiator and the randomizer can be added to the monomers to be polymerized separately by stepwise or simultaneous addition.

[0023] As mentioned above, in the presence of an effective amount of an initiator, a conjugated diene monomer is polymerized with a monomer that can copolymerize with the conjugated diene monomer to produce a reactive polymer. The introduction of the initiator, the conjugated diene monomer, the comonomer, and the solvent forms a polymerization mixture in which a reactive polymer is formed. The polymerization in a solvent produces a polymerization mixture in which the polymer product is dissolved or suspended in the solvent. The polymerization mixture can be referred to as a polymer glue.

[0024] The amount of initiator to be used may depend on the interaction of various factors, such as the type of initiator used, the purity of the composition, the polymerization temperature, the polymerization rate and the required conversion, the required molecular weight and many other factors. In one or more embodiments, the amount of the initiator used may be expressed as the number of millimoles of initiator per unit weight of monomer. In one or more embodiments, the initiator loading per 100 grams of monomer may vary from about 0.05 mmol to about 50 mmol, from about 0.1 mmol to about 25 mmol in other embodiments, from about 0.2 mmol to about 2.5 mmol in still other embodiments, and from about 0.4 mmol to about 0.7 mmol in other embodiments.

[0025] In one or more embodiments, the polymerization can be carried out in any conventional polymerization vessel known in the art. For example, the polymerization can be carried out in a conventional stirred tank reactor. In one or more embodiments, all ingredients for the polymerization can be combined in a single container (e.g., a conventional stirred tank reactor), and all steps of the polymerization process can be carried out in the container. In other embodiments, two or more ingredients can be pre-combined in one container and then transferred to another container, where the polymerization of the monomer (or at least a large part thereof) can be carried out. Since various embodiments of the present invention include the use of multiple reactors or reaction zones, the container (e.g., a tank reactor) in which the polymerization is carried out can be referred to as the first container or the first reaction zone.

[0026] Polymerization can be carried out by batch method, continuous method or semi-continuous method.In semi-continuous method, monomer is loaded intermittently as needed to replace polymerized monomer.In one or more embodiments, the heat of polymerization can be removed by the external cooling carried out by the reactor jacket via thermal control, by internal cooling (by using the reflux condenser connected to the reactor to evaporate and condense the monomer) or the combination of two methods.In addition, conditions can be controlled to polymerize at about 0.1 atmospheric pressure to about 50 atmospheric pressures, at about 0.5 atmospheric pressure to about 20 atmospheric pressures in other embodiments, and at about 1 atmospheric pressure to about 10 atmospheric pressures in other embodiments.In one or more embodiments, the pressure that can be polymerized includes those pressures that ensure that the major part of monomer is liquid phase.In these or other embodiments, the polymerization mixture can be maintained under oxygen-free conditions.

[0027] Polymerization temperature

[0028] In one or more embodiments, the conditions under which the polymerization is carried out may be controlled to maintain the peak polymerization temperature of the polymerization mixture above 30° C., in other embodiments above 50° C., and in other embodiments above 70° C. In these or other embodiments, the conditions under which the polymerization is carried out may be controlled to maintain the peak polymerization temperature of the polymerization mixture below 120° C., in other embodiments below 110° C., and in other embodiments below 100° C. In one or more embodiments, the conditions under which the polymerization is carried out may be controlled to maintain the temperature of the polymerization mixture in the range of about −10° C. to about 200° C., in other embodiments from about 0° C. to about 150° C., and in other embodiments from about 20° C. to about 110° C.

[0029] Polymer properties before modification

[0030] Reactive polymers can be characterized by their molecular weight, which can include number average molecular weight (Mn), weight average molecular weight (Mw) and peak molecular weight (Mp). As will be appreciated by those skilled in the art, molecular weight can be determined using gel permeation chromatography (GPC) using appropriate calibration standards and equipped with appropriate detectors such as refractive index and / or UV detectors. For the purposes of this specification, unless otherwise stated, GPC measurements employ polystyrene standards and polystyrene Mark Houwink constants. The coupling percentage can also be determined by GPC by measuring the area under the base peak (A) and the total area under the GPC curve (B). The coupling percentage is then calculated as follows: coupling percentage = (BA) / A x 100%.

[0031] According to embodiments of the present invention, given that it has been observed that the functionalizing agents of the present invention result in less coupling, particularly coupling of three or more chains together, the molecular weight of the base polymer can be increased while remaining within the desired rheological properties (e.g., Mooney viscosity).

[0032] In one or more embodiments, the reactive polymer has an Mp greater than 160 kg / mol, in other embodiments greater than 180 kg / mol, in other embodiments greater than 200 kg / mol, in other embodiments greater than 215 kg / mol, in other embodiments greater than 230 kg / mol, in other embodiments greater than 240 kg / mol, in other embodiments greater than 250 kg / mol, in other embodiments greater than 260 kg / mol, and in other embodiments greater than 270 kg / mol, which may also be referred to as a base Mp. In these or other embodiments, the reactive polymer has an Mp less than 370 kg / mol, in other embodiments less than 360 kg / mol, in other embodiments less than 350 kg / mol, in other embodiments less than 330 kg / mol, in other embodiments less than 310 kg / mol, in other embodiments less than 280 kg / mol, and in other embodiments less than 250 kg / mol. In one or more embodiments, the reactive polymer has an Mp of about 160 kg / mol to about 280 kg / mol, in other embodiments about 170 kg / mol to about 260 kg / mol, in other embodiments about 200 kg / mol to about 370 kg / mol, in other embodiments about 215 kg / mol to about 360 kg / mol, in other embodiments about 230 kg / mol to about 350 kg / mol, and in other embodiments about 180 kg / mol to about 250 kg / mol.

[0033] In one or more embodiments, the reactive polymer has an Mn greater than 130 kg / mol, in other embodiments greater than 140 kg / mol, in other embodiments greater than 150 kg / mol, in other embodiments greater than 170 kg / mol, in other embodiments greater than 200 kg / mol, in other embodiments greater than 210 kg / mol, in other embodiments greater than 220 kg / mol, and in other embodiments greater than 230 kg / mol, which may also be referred to as a base Mn. In these or other embodiments, the reactive polymer has an Mn less than 350 kg / mol, in other embodiments less than 340 kg / mol, in other embodiments less than 330 kg / mol, in other embodiments less than 320 kg / mol, in other embodiments less than 300 kg / mol, in other embodiments less than 280 kg / mol, and in other embodiments less than 260 kg / mol. In one or more embodiments, the reactive polymer has an Mn of about 130 to about 300 kg / mol, in other embodiments about 140 kg / mol to about 280 kg / mol, in other embodiments about 170 kg / mol to about 350 kg / mol, in other embodiments about 200 kg / mol to about 340 kg / mol, in other embodiments about 210 kg / mol to about 330 kg / mol, and in other embodiments about 150 kg / mol to about 260 kg / mol.

[0034] In one or more embodiments, the reactive polymer has an Mw greater than 180 kg / mol, greater than 190 kg / mol in other embodiments, greater than 200 kg / mol in other embodiments, greater than 230 kg / mol in other embodiments, greater than 245 kg / mol in other embodiments, greater than 260 kg / mol in other embodiments, greater than 275 kg / mol in other embodiments, and greater than 285 kg / mol in other embodiments, which may also be referred to as a base Mw. In these or other embodiments, the reactive polymer has an Mw less than 650 kg / mol, less than 600 kg / mol in other embodiments, less than 550 kg / mol, less than 500 kg / mol in other embodiments, and less than about 450 kg / mol in other embodiments. In one or more embodiments, the reactive polymer has an Mw of about 180 kg / mol to about 650 kg / mol, in other embodiments about 190 kg / mol to about 600 kg / mol, in other embodiments about 200 kg / mol to about 550 kg / mol, in other embodiments about 230 kg / mol to about 500 kg / mol, in other embodiments about 250 kg / mol to about 500 kg / mol, and in other embodiments about 200 kg / mol to about 400 kg / mol.

[0035] Reactive polymers according to aspects of the present invention may be characterized by vinyl content, which may be described as the number of unsaturated groups in the 1,2-microstructure relative to the total unsaturated groups within the polymer chain. As will be appreciated by the skilled person, the vinyl content may be determined by FTIR analysis. In one or more embodiments, the reactive polymer comprises greater than 10%, greater than 20% in other embodiments, and greater than 35% vinyl in other embodiments. In these or other embodiments, the reactive polymer comprises less than 80%, less than 60% in other embodiments, and less than 46% in other embodiments. In one or more embodiments, the reactive polymer comprises from about 10% to about 80%, from about 20% to about 60% in other embodiments, and from about 35% to about 46% vinyl in other embodiments.

[0036] The reactive polymer produced according to aspects of the present invention can be characterized by a combined styrene content, which refers to the weight percent of the vinyl aromatic monomer (e.g., styrene) incorporated into the polydiene copolymer. As understood by those skilled in the art, combined styrene can be determined with reference to the relative weight of the vinyl aromatic monomer included in the polymerization mixture relative to the diene monomer. In one or more embodiments, the reactive polymer comprises less than 20 weight %, less than 25 weight %, and less than 30 weight % of the combined styrene content in other embodiments. In one or more embodiments, the reactive polymer comprises less than 60 weight %, less than 55 weight %, and less than 50 weight % of the combined styrene content in other embodiments. In one or more embodiments, the reactive polymer comprises about 20 weight % to about 60 weight %, about 25 weight % to about 55 weight % in other embodiments, and about 30 weight % to about 50 weight % of the combined styrene content in other embodiments.

[0037] Reactive polymers can be characterized by a relatively high active (also referred to as reactive) end group content, which represents the mole % of the polymer having reactive chain ends capable of reacting with the functionalizing agent. In one or more embodiments, greater than 60%, in other embodiments greater than 70%, in other embodiments greater than 80%, in other embodiments greater than 85%, in other embodiments greater than 90%, in other embodiments greater than 95%, and in other embodiments greater than 99% of the polymer in the polymerization mixture contains active or reactive chain ends.

[0038] It has been advantageously discovered that the techniques of one or more embodiments of the present invention provide polymer blends characterized as defined herein over a wide range of microstructures and comonomer contents.

[0039] Polymer modification

[0040] As mentioned above, the reactive polymer undergoes modification, which may also be referred to as functionalization, to provide a blend of mono-hydrocarbyloxysilyl functionalized polydiene and di-hydrocarbyloxysilyl functionalized polydiene and polydiene copolymers. That is, the reactive end of the polymer is modified by introducing a functionalizing agent into the polymeric mixture, which may also be referred to as functionalized. It is believed that the polymer chain end reacts with a functionalizing agent (which may also be referred to as a modifier) ​​to provide a residue of the functionalizing agent at the end of the polymer chain. In particular, it is believed that a considerable portion of the functionalization reaction occurs on the silicon atom, thereby replacing the hydrocarbyl groups on the di-hydrocarbyloxy group or tri-hydrocarbyloxy group of the functionalizing agent. Therefore, the reaction between the polymer and the functionalizing agent produces a polymer composition comprising one or more polymer chains, which contain terminal groups derived from the functionalizing agent. It should be understood that the reaction between the functionalizing agent and the reactive polymer may also result in polymer coupling. In either case, the polymer bearing the chain end functional groups and the polymer coupled to the residue of a functionalizing agent will be referred to as a modified polymer or a functionalized polymer unless otherwise indicated.

[0041] In one or more embodiments, polymer compositions contain terminal functional groups greater than 10mol%, greater than 30mol%, greater than 35mol%, and greater than 40mol% of polymer chains in other embodiments. In these or other embodiments, polymer compositions contain terminal functional groups less than 95mol%, less than 90mol%, and less than 85mol% of polymer chains in other embodiments. In one or more embodiments, polymer compositions contain terminal functional groups from about 10mol% to about 95mol%, from about 30mol% to about 90mol%, and from about 35mol% to about 85mol% of polymer chains in other embodiments.

[0042] Functionalizing agent

[0043] According to the practice of the present invention, at least two different functionalizing agents are used. These functionalizing agents can be referred to as the first functionalizing agent and the second functionalizing agent, respectively. As described above, the first functionalizing agent is a trihydrocarbyloxysilane, and the second functionalizing agent is a dihydrocarbyloxysilane.

[0044] In one or more embodiments, the trihydrocarbyloxysilyl functionalizing agent, which may also be referred to as a trihydrocarbyloxysilane or a trihydrocarbyloxysilane (or as a corresponding alkoxy compound such as a trialkoxysilane), may be defined by the formula:

[0045]

[0046] Where R 1is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and A is selected from the group consisting of an imine group, a carboxylate group, a cyclic tertiary amine group, a non-cyclic tertiary amine group, a pyridine group, a silazane group, an epoxy group, an isocyanate group, a cyano group, a carboxylic anhydride group and a hydrocarbon sulfide group.

[0047] In one or more embodiments, the dihydrocarbyloxysilyl functionalizing agent, which may also be referred to as a dihydrocarbyloxysilane or a dihydrocarbyloxysilane (or as a corresponding alkoxy compound such as a dialkoxysilane), may be defined by the formula:

[0048]

[0049] Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and A is selected from the group consisting of an imine group, a carboxylate group, a cyclic tertiary amine group, a non-cyclic tertiary amine group, a pyridine group, a silazane group, an epoxy group, an isocyanate group, a cyano group, a carboxylic anhydride group and a hydrocarbon sulfide group.

[0050] In one or more embodiments, the hydrocarbyl group includes but is not limited to an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an aryl group, an allyl group, an aralkyl group, an alkaryl group or an alkynyl group. The hydrocarbyl group also includes a substituted hydrocarbyl group, and the substituted hydrocarbyl group refers to a hydrocarbyl group in which one or more hydrogen atoms have been replaced with a substituent (such as a hydrocarbyl group). In one or more embodiments, these groups may include 1 (or the suitable minimum carbon atom number of the group formed) to about 20 carbon atoms. These groups may or may not contain heteroatoms. Suitable heteroatoms include but are not limited to nitrogen atoms, boron atoms, oxygen atoms, silicon atoms, sulfur atoms, tin atoms and phosphorus atoms. In one or more embodiments, cycloalkyl groups, cycloalkenyl groups and aryl groups are non-heterocyclic groups. In these or other embodiments, the substituents of the substituted hydrocarbyl groups are non-heterocyclic groups.

[0051] In one or more embodiments, the alkylene group includes but is not limited to an alkylene group, a cycloalkylene group, an alkenylene group, a cycloalkenylene group, an alkynylene group, a cycloalkynylene group or an arylene group. The alkylene group also includes a substituted alkylene group, and the substituted alkylene group refers to an alkylene group in which one or more hydrogen atoms have been replaced by a substituent (such as an alkyl group). In one or more embodiments, these groups may include 1 (or the suitable minimum carbon atom number of the group formed) to about 20 carbon atoms. These groups may or may not contain heteroatoms. Suitable heteroatoms include but are not limited to nitrogen atoms, boron atoms, oxygen atoms, silicon atoms, sulfur atoms, tin atoms and phosphorus atoms. In one or more embodiments, cycloalkylene groups, cycloalkenylene groups and arylene groups are non-heterocyclic groups. In these or other embodiments, the substituents forming the substituted alkylene groups are non-heterocyclic groups.

[0052] Examples of imine-containing trihydrocarbyloxysilanes include, but are not limited to, N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine, N-(1-methylethylidene)-3-(triethoxysilyl)-1-propylamine, N-ethylidene-3-(triethoxysilyl)-1-propylamine, N-(1-methylpropylidene)-3-(triethoxysilyl)-1-propylamine, N-(4-N,N-dimethylaminobenzylidene)-3-(triethoxymethyl)-1-propylamine, The compounds include N-(1-methylbutylene)-3-(trimethoxysilyl)-1-propylamine, N-(1,3-dimethylbutylene)-3-(trimethoxysilyl)-1-propylamine, N-(1-methylethylidene)-3-(trimethoxysilyl)-1-propylamine, N-ethylidene-3-(trimethoxysilyl)-1-propylamine, N-(1-methylpropylidene)-3-(trimethoxysilyl)-1-propylamine and N-(4-N,N-dimethylaminobenzylidene)-3-(trimethoxysilyl)-1-propylamine.

[0053] Examples of imine-containing dihydrocarbyloxysilanes include, but are not limited to, N-(1,3-dimethylbutylene)-3-(methyldiethoxysilyl)-1-propylamine, N-(1-methylethylidene)-3-(methyldiethoxysilyl)-1-propylamine, N-ethylidene-3-(methyldiethoxysilyl)-1-propylamine, N-(1-methylpropylene)-3-(methyldiethoxysilyl)-1-propylamine, N-(4-N,N-dimethylaminobenzylidene)-3-(methyldiethoxysilyl)-1-propylamine, N-(cyclohexylene)-3-(methyldiethoxysilyl)-1-propylamine, The compounds include N-(1-methylbutylene)-3-(ethyldimethoxysilyl)-1-propylamine, N-(1,3-dimethylbutylene)-3-(ethyldimethoxysilyl)-1-propylamine, N-(1-methylethylidene)-3-(ethyldimethoxysilyl)-1-propylamine, N-ethylidene-3-(ethyldimethoxysilyl)-1-propylamine, N-(1-methylpropylidene)-3-(ethyldimethoxysilyl)-1-propylamine, N-(4-N,N-dimethylaminobenzylidene)-3-(ethyldimethoxysilyl)-1-propylamine and N-(cyclohexylene)-3-(ethyldiethoxysilyl)-1-propylamine.

[0054] Examples of the trihydrocarbyloxysilane compound containing a carboxylate group include, but are not limited to, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-methacryloxypropyltriisopropoxysilane.

[0055] Examples of the dihydrocarbyloxysilane compound containing a carboxylate group include, but are not limited to, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, and 3-methacryloxypropylmethyldiisopropoxysilane.

[0056] Examples of trihydrocarbyloxysilane compounds containing a cyclic tertiary amine group include, but are not limited to, 3-(1-hexamethyleneimino)propyltriethoxysilane, 3-(1-hexamethyleneimino)propyltrimethoxysilane, (1-hexamethyleneimino)methyltriethoxysilane, (1-hexamethyleneimino)methyltrimethoxysilane, 2-(1-hexamethyleneimino)ethyltriethoxysilane, 3-(1-hexamethyleneimino)ethyltrimethoxysilane, 3-(1-pyrrolidinyl)propyltrimethoxysilane, 3-(1-pyrrolidinyl)propyltriethoxysilane, 3-(1-heptamethyleneimino)propyltriethoxysilane, 3-(1-dodecamethyleneimino)propyltriethoxysilane, and 3-[10-(triethoxysilyl)decyl]-4-oxazoline.

[0057] Examples of dihydrocarbyloxysilane compounds containing a cyclic tertiary amine group include, but are not limited to, 3-(1-hexamethyleneimino)propylmethyldiethoxysilane, 3-(1-hexamethyleneimino)propylmethyldimethoxysilane, (1-hexamethyleneimino)propylmethyldiethoxysilane, (1-hexamethyleneimino)methylmethyldimethoxysilane, 2-(1-hexamethyleneimino)ethylmethyldiethoxysilane, 3-(1-hexamethyleneimino)propylmethyldimethoxysilane, (1-hexamethyleneimino)propylmethyldiethoxysilane, (1-hexamethyleneimino)methylmethyldimethoxysilane, )ethylmethyldimethoxysilane, 3-(1-pyrrolidinyl)propylmethyldimethoxysilane, 3-(1-pyrrolidinyl)propylmethyldiethoxysilane, 3-(1-heptamethyleneimino)propylmethyldiethoxysilane, 3-(1-dodecamethyleneimino)propylmethyldiethoxysilane, 3-[10-(methyldiethoxysilyl)decyl]-4-oxazoline and 3-(1-hexamethyleneimino)propyldiethoxyethylsilane.

[0058] Examples of trihydrocarbyloxysilane compounds containing a non-cyclic tertiary amine group include, but are not limited to, 3-dimethylaminopropyltriethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 3-diethylaminopropyltriethoxysilane and 2-dimethylaminoethyltriethoxysilane, 2-dimethylaminoethyltrimethoxysilane.

[0059] Examples of dihydrocarbyloxysilane compounds containing a non-cyclic tertiary amine group include, but are not limited to, 3-dimethylaminopropyldiethoxysilane, 3-diethylaminopropyldiethoxymethylsilane,

[0060] 3-Dimethylaminopropyldimethoxymethylsilane, 3-diethylaminopropyldimethoxymethylsilane and 3-dibutylaminopropyltriethoxysilane.

[0061] Examples of the trihydrocarbyloxysilane compound containing a pyridine group include, but are not limited to, 2-trimethoxysilylethylpyridine.

[0062] Examples of the dihydrocarbyloxysilane compound containing a pyridine group include, but are not limited to, 2-methyldimethoxysilylethylpyridine.

[0063] Examples of trihydrocarbyloxysilane compounds containing a silazane group include, but are not limited to, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, and N,N-bis(trimethylsilyl)aminoethyltriethoxysilane.

[0064] Examples of dihydrocarbyloxysilane compounds containing a silazane group include, but are not limited to, 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silacyclopentane, N,N-bis(trimethylsilyl)-aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldimethoxysilane, and N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane.

[0065] Examples of the trihydrocarbyloxysilane compound containing an isocyanato group include, but are not limited to, 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-isocyanatopropyltriisopropoxysilane.

[0066] Examples of the dihydrocarbyloxysilane compound containing an isocyanate group include, but are not limited to, 3-isocyanatepropyldimethoxysilane, 3-isocyanatepropyldiethoxysilane, 3-isocyanatepropylmethyldiethoxysilane, and 3-isocyanatepropyldiisopropoxymethylsilane.

[0067] Examples of the trihydrocarbyloxysilane compound containing a cyano group include, but are not limited to, 2-cyanoethyltriethoxysilane, 3-cyanopropyltriethoxysilane, and 2-cyanoethylpropyltriethoxysilane.

[0068] Examples of the dihydrocarbyloxysilane compound containing a cyano group include, but are not limited to, 2-cyanoethyldiethoxymethylsilane, 2-cyanoethylpropyldiethoxymethylsilane, and 3-cyanopropyldiethoxymethylsilane.

[0069] Examples of the trihydrocarbyloxysilane compound containing a carboxylic anhydride group include, but are not limited to, 3-trimethoxysilylpropylsuccinic anhydride and 3-triethoxysilylpropylsuccinic anhydride.

[0070] Examples of the dihydrocarbyloxysilane compound containing a carboxylic anhydride group include, but are not limited to, 3-dimethoxymethylsilylpropylsuccinic anhydride, 3-diethoxymethylsilylpropylsuccinic anhydride, and 3-diethoxyethylsilylpropylsuccinic anhydride.

[0071] Examples of the trihydrocarbyloxysilane compound containing an epoxy group include, but are not limited to, 2-glycidyloxyethyltrimethoxysilane, 2-glycidyloxyethyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

[0072] Examples of the dihydrocarbyloxysilane compound containing an epoxy group include, but are not limited to, (2-glycidyloxyethyl)methyldimethoxysilane, (3-glycidyloxypropyl)-methyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyl(methyl)dimethoxysilane.

[0073] In one or more specific embodiments, the first functionalizing agent is an imine-containing trihydrocarbyloxysilane functionalizing agent defined by the formula

[0074]

[0075] Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and each R 3 are independently hydrocarbyl groups.

[0076] In one or more of these specific embodiments, the imine-containing hydrocarbyloxysilane includes N-(1-methylpropylene)-3-(triethoxysilyl)-1-propylamine and / or N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine.

[0077] In these embodiments, the second functionalizing agent is a glycidyloxy-containing dihydrocarbyloxysilane agent defined by the formula

[0078]

[0079] Where R 1 is a hydrocarbylene group, and each R 2 are independently hydrocarbyl groups.

[0080] In one or more of these specific embodiments, the glycidyloxy-containing dialkoxysilane includes 3-(glycidyloxypropyl)dimethoxymethylsilane, 3-(glycidyloxypropyl)diethoxymethylsilane, 3-(glycidyloxybutyl)dimethoxymethylsilane and / or 3-(glycidyloxybutyl)diethoxymethylsilane.

[0081] The amount of functionalizing agent used

[0082] The total amount of functionalizing agent (i.e., first and second functionalizing agents) employed in the practice of the present invention can be described relative to the lithium or metal cation associated with the initiator. In one or more embodiments, the total amount of functionalizing agent introduced into the polymerization mixture is greater than 0.70 moles of functionalizing agent per mole of lithium in the initiator, in other embodiments greater than 0.75 moles of functionalizing agent per mole of lithium in the initiator, in other embodiments greater than 0.80 moles of functionalizing agent per mole of lithium in the initiator, in other embodiments greater than 0.85 moles of functionalizing agent per mole of lithium in the initiator, and in other embodiments greater than 0.90 moles of functionalizing agent per mole of lithium in the initiator. In these or other embodiments, less than 0.99 moles of total functionalizing agent per mole of lithium, in other embodiments less than 0.97 moles of total functionalizing agent per mole of lithium, and in other embodiments less than 0.95 moles of total functionalizing agent per mole of lithium is introduced into the polymerization mixture. In one or more embodiments, about 0.7 moles of total functionalizing agent / mole lithium to about 1.0 moles of total functionalizing agent / mole lithium, in other embodiments about 0.75 moles of total functionalizing agent / mole lithium to about 0.99 moles of total functionalizing agent / mole lithium, and in other embodiments about 0.80 moles of total functionalizing agent / mole lithium to about 0.97 moles of total functionalizing agent / mole lithium are introduced into the polymerization mixture. Those skilled in the art understand that these loadings are equal to the amount of functionalizing agent employed relative to the number of moles of active or reactive polymer (i.e., the number of moles of functionalizing agent).

[0083] In one or more embodiments, the amount of functionalizing agent employed can be described with reference to the first functionalizing agent and the second functionalizing agent relative to the lithium or metal cation (or the number of moles of reactive or living polymer) associated with the initiator. In one or more embodiments, the amount of the first functionalizing agent (i.e., the amine-containing trihydrocarbyloxysilane) introduced into the polymerization mixture is greater than 0.15 moles of the first functionalizing agent per mole of lithium in the initiator, in other embodiments greater than 0.20 moles of the first functionalizing agent per mole of lithium in the initiator, in other embodiments greater than 0.23 moles of the first functionalizing agent per mole of lithium in the initiator, and in other embodiments greater than 0.27 moles of the first functionalizing agent per mole of lithium in the initiator. In these or other embodiments, less than 0.50 moles of the first functionalizing agent per mole of lithium, in other embodiments less than 0.45 moles of the first functionalizing agent per mole of lithium, in other embodiments less than 0.40 moles of the first functionalizing agent per mole of lithium, and in other embodiments less than 0.35 moles of the first functionalizing agent per mole of lithium are introduced into the polymerization mixture. In one or more embodiments, from about 0.15 moles of the first functionalizing agent per mole of lithium to about 0.50 moles of the first functionalizing agent per mole of lithium, in other embodiments from about 0.20 moles of the first functionalizing agent per mole of lithium to about 0.40 moles of the first functionalizing agent per mole of lithium, and in other embodiments from about 0.23 moles of the first functionalizing agent per mole of lithium to about 0.35 moles of the first functionalizing agent per mole of lithium are introduced into the polymerization mixture.

[0084] In conjunction with the above, the amount of the second functionalizing agent (e.g., a dihydrocarbyloxysilane containing glycidyloxy groups) may also be described with reference to the lithium or metal cation associated with the initiator. In one or more embodiments, the amount of the second functionalizing agent (e.g., a dihydrocarbyloxysilane containing glycidyloxy groups) introduced into the polymerization mixture is greater than 0.40 moles of the second functionalizing agent / mole of lithium in the initiator, in other embodiments greater than 0.45 moles of the second functionalizing agent / mole of lithium in the initiator, in other embodiments greater than 0.50 moles of the second functionalizing agent / mole of lithium in the initiator, and in other embodiments greater than 0.55 moles of the second functionalizing agent / mole of lithium in the initiator. In these or other embodiments, less than 0.80 moles of the first functionalizing agent / mole of lithium, in other embodiments less than 0.75 moles of the first functionalizing agent / mole of lithium, in other embodiments less than 0.70 moles of the first functionalizing agent / mole of lithium, and in other embodiments less than 0.65 moles of the first functionalizing agent / mole of lithium are introduced into the polymerization mixture. In one or more embodiments, from about 0.40 moles of the first functionalizing agent per mole of lithium to about 0.80 moles of the first functionalizing agent per mole of lithium, in other embodiments from about 0.50 moles of the first functionalizing agent per mole of lithium to about 0.70 moles of the first functionalizing agent per mole of lithium, and in other embodiments from about 0.55 moles of the first functionalizing agent per mole of lithium to about 0.65 moles of the first functionalizing agent per mole of lithium are introduced into the polymerization mixture.

[0085] The amount of the corresponding functionalizing agent can also be described relative to the molar percentage of each functionalizing agent relative to the total functionalizing agent used. In one or more embodiments, about 45 mol % to about 75 mol %, about 50 mol % to about 70 mol % in other embodiments, and about 55 mol % to about 65 mol % in other embodiments of the total functionalizing agent used are the first functionalizing agent (i.e., trihydrocarbyloxysilane containing amine). Correspondingly, about 25 mol % to about 55 mol %, about 30 mol % to about 50 mol % in other embodiments, and about 35 mol % to about 45 mol % in other embodiments of the total functionalizing agent used are the second functionalizing agent (e.g., dihydrocarbyloxysilane containing glycidyloxy). Due to the corresponding amount of the functionalizing agent used, the molar percentage of the total functionalized polymer will have the same (or generally the same) molar percentage.

[0086] Functionalization reaction

[0087] In one or more embodiments, the first functionalizing agent and the second functionalizing agent can be introduced into the reactive polymer sequentially or simultaneously. If sequential, they can be introduced in any order. For example, in one or more embodiments, the second functionalizing agent (e.g., a dihydrocarbyloxysilane containing a glycidyloxy group) is first introduced, followed by the first functionalizing agent (i.e., a trihydrocarbyloxysilane containing an amine). In other embodiments, the first functionalizing agent is first introduced, followed by the second functionalizing agent. In either case, it is believed that the reaction between the reactive polymer and the functionalizing agent (i.e., the first functionalizing agent or the second functionalizing agent) is primarily carried out at the hydrocarbyloxy substituent of the functionalizing agent.

[0088] In one or more embodiments, the reaction between the functionalizing agent and the reactive polymer can be carried out at a temperature of about 10°C to about 150°C, and in other embodiments at a temperature of about 20°C to about 100°C. The time required to complete the reaction between the functionalizing agent and the reactive polymer depends on various factors, such as the type and amount of catalyst or initiator used to prepare the reactive polymer, the type and amount of the functionalizing agent, and the temperature at which the functionalization reaction is carried out. In one or more embodiments, the reaction between the functionalizing agent and the reactive polymer can be carried out for about 10 to 60 minutes.

[0089] In one or more embodiments, the first functionalizing agent and the second functionalizing agent are introduced into a polymer cement (i.e., a polymeric mixture) while the polymer is dissolved or suspended in a solvent. As will be appreciated by those skilled in the art, the solution may be referred to as a polymer cement. In one or more embodiments, the properties of the polymer cement (such as its concentration) will be the same or similar to the properties of the cement prior to functionalization.

[0090] In one or more embodiments, modification of the polymer (i.e., introduction of the functionalizing agent into the polymer cement) is performed in the same vessel in which the polymerization is performed. In other embodiments, modification of the polymer is performed outside of the reaction vessel in which the polymerization is performed. For example, the first functionalizing agent and the second functionalizing agent can be introduced into the polymerization mixture (i.e., the polymer cement) in a downstream vessel or a downstream delivery conduit.

[0091] According to one or more embodiments, as a result of the functionalization reaction, greater than 60 mol%, in other embodiments greater than 70 mol%, in other embodiments greater than 80 mol%, in other embodiments greater than 85 mol%, in other embodiments greater than 90 mol%, and in other embodiments greater than 95 mol% of the polymer chains in the polymer composition contain terminal functional groups (e.g., dihydrocarbyloxysilyl terminal groups or trihydrocarbyloxysilyl terminal groups). In one or more embodiments, about 60 mol% to about 100 mol%, in other embodiments about 70 mol% to about 99 mol%, in other embodiments about 80 mol% to about 98 mol%, and in other embodiments about 90 mol% to about 97 mol% of the polymer chains in the polymer composition contain terminal functional groups.

[0092] Polymer stabilization

[0093] As mentioned above, after modification, the modified polymer can be stabilized. In one or more embodiments, stabilizers known in the art can be used. For example, stabilizers can include alkyl hydrocarbyloxy silanes (e.g., alkyl alkoxy silanes) as disclosed in U.S. Patent No. 6,255,404, which is incorporated herein by reference. Exemplary alkyl alkoxy silanes include octyl triethoxy silane. In other embodiments, stabilizers can include long chain alcohols as disclosed in U.S. Patent No. 6,279,632, which is incorporated herein by reference. Exemplary long chain alcohols include sorbitan stearate or sorbitan monooleate. In other embodiments, stabilized polymers can be treated with alkyl alkoxy silanes, followed by treatment with silanes (such as methyl trichlorosilane) containing hydrolyzable groups that form acidic substances when hydrolyzed, as disclosed in U.S. Patent No. 9,546,237, which is incorporated herein by reference.

[0094] In one or more embodiments, the modified polymer (i.e., a blend of a mono-hydrocarbyloxysilyl-functionalized polydiene and a di-hydrocarbyloxysilyl-functionalized polydiene and a polydiene copolymer) can optionally be stabilized. That is, the modified polymer can be stabilized by introducing an alkyloxysilane into a polymeric mixture comprising the modified polymer. It is believed that the alkyloxysilane reacts with a terminal functional group (e.g., at a hydrocarbyloxy substituent). It is also believed that the reaction between the chain end functional group and the alkyloxysilane is carried out when two molecules are introduced or after aging of the composition. The reaction between the alkyloxysilane and the terminal group produces a polymer composition comprising one or more polymer chains, which comprises a di-hydrocarbyloxysilane derived from an imine-containing and a terminal group subsequently reacted with the alkyloxysilane.

[0095] In one or more embodiments, the stabilizer is a hydrocarbyl hydrocarbyloxysilane (ie, stabilizer), which can be defined by Formula I:

[0096]

[0097] Where R 2 is a hydrocarbon group, R 3 , R 4 and R 5 Each is independently a hydrocarbyl group or a hydrocarbyloxy group. In a specific embodiment, R 3 , R 4 and R 5 is a hydrocarbon group. In other embodiments, R 3 and R 4 is a hydrocarbon group, and R 5 In other embodiments, R 3 is a hydrocarbon group, and R 4 and R 5 In certain embodiments, R 3 , R 4 and R 5 All are alkoxy groups.

[0098] In one or more embodiments, the hydrocarbyl group of the hydrocarbyl hydrocarbyloxysilane includes, but is not limited to, an alkyl group, a cycloalkyl group, a substituted cycloalkyl group, an alkenyl group, a cycloalkenyl group, a substituted cycloalkenyl group, an aryl group, an allyl group, a substituted aryl group, an aralkyl group, an alkaryl group, or an alkynyl group. The substituted hydrocarbyl group includes a hydrocarbyl group in which one or more hydrogen atoms have been replaced by a substituent group such as an alkyl group. In one or more embodiments, the hydrocarbyl group may include one (or the appropriate minimum number of carbon atoms forming the group) to 20 carbon atoms. These hydrocarbyl groups may contain heteroatoms such as, but not limited to, nitrogen, boron, oxygen, silicon, sulfur, and phosphorus atoms.

[0099] In one or more embodiments, the hydrocarbyl hydrocarbyloxysilane hydrocarbyloxy group includes but is not limited to: alkoxy group, cycloalkoxy group, substituted cycloalkoxy group, olefinoxy group, cycloolefinoxy group, substituted cycloolefinoxy group, aryloxy group, allyloxy group, substituted aryloxy group, aralkyloxy group, alkaryloxy group or alkynyloxy group. The substituted hydrocarbyloxy group includes a hydrocarbyloxy group in which one or more hydrogen atoms attached to a carbon atom have been replaced by a substituent (such as an alkyl group). In one or more embodiments, the hydrocarbyloxy group may include one (or the minimum number of carbon atoms suitable to form the group) to 20 carbon atoms. The hydrocarbyloxy group may contain heteroatoms, such as, but not limited to, nitrogen atoms, boron atoms, oxygen atoms, silicon atoms, sulfur atoms and phosphorus atoms.

[0100] In one or more embodiments, types of hydrocarbylhydrocarbyloxysilanes include trihydrocarbylhydrocarbyloxysilanes, dihydrocarbyldihydrocarbyloxysilanes, hydrocarbyltrihydrocarbyloxysilanes, and tetrahydrocarbyloxysilanes.

[0101] Specific examples of the hydrocarbyltrihydrocarbyloxysilane include methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, phenyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, phenyltriethoxysilane, octyltriethoxysilane, decyltriethoxysilane, methyltriphenoxysilane, ethyltriphenoxysilane, propyltriphenoxysilane, octyltriphenoxysilane, phenyltriphenoxysilane, decyltriphenoxysilane, silane, methyldiethoxymethoxysilane, ethyldiethoxymethoxysilane, propyldiethoxymethoxysilane, phenyldiethoxymethoxysilane, octyldiethoxymethoxysilane, decyldiethoxymethoxysilane, methyldiphenoxymethoxysilane, ethyldiphenoxymethoxysilane, propyldiphenoxymethoxysilane, phenyldiphenoxymethoxysilane, octyldiphenoxymethoxysilane, decyldiphenoxymethoxysilane, methyldimethoxyethoxysilane, ethyldimethoxyethoxysilane, propyldiphenoxymethoxysilane, phenyldiphenoxymethoxysilane, octyldiphenoxymethoxysilane, decyldiphenoxymethoxysilane, Dimethoxyethoxysilane, phenyl dimethoxyethoxysilane, octyl dimethoxyethoxysilane, decyl dimethoxyethoxysilane, methyl diphenoxyethoxysilane, ethyl diphenoxyethoxysilane, propyl diphenoxyethoxysilane, phenyl diphenoxyethoxysilane, octyl diphenoxyethoxysilane, decyl diphenoxyethoxysilane, methyl dimethoxyphenoxysilane, ethyl dimethoxyphenoxysilane, propyl dimethoxyphenoxysilane, phenyl dimethoxyphenoxysilane, octyl dimethoxyphenoxysilane, Phenoxysilane, decyl dimethoxy phenoxy silane, methyl diethoxy phenoxy silane, ethyl diethoxy phenoxy silane, propyl diethoxy phenoxy silane, phenyl diethoxy phenoxy silane, octyl diethoxy phenoxy silane, decyl diethoxy phenoxy silane, methyl methoxyethoxy phenoxy silane, ethyl methoxyethoxy phenoxy silane, propyl methoxyethoxy phenoxy silane, phenyl methoxyethoxy phenoxy silane, octyl methoxyethoxy phenoxy silane and decyl methoxyethoxy phenoxy silane.

[0102] In one or more embodiments, the stabilizer is added to the polymer cement after providing sufficient time to allow the reaction between the reactive polymer and the functionalizing agent to complete. In one or more embodiments, the stabilizer is introduced to the polymer cement after 30 minutes, in other embodiments after 15 minutes, and in other embodiments after 10 minutes from the time the functionalizing agent is introduced into the polymer cement.

[0103] The amount of stabilizer (i.e., hydrocarbyl hydrocarbyloxysilane) employed in the practice of the present invention can be described relative to the number of moles of lithium associated with the initiator. In one or more embodiments, greater than 0.5 moles of stabilizer per mole of lithium in the initiator, in other embodiments greater than 1.0 moles of stabilizer per mole of lithium in the initiator, in other embodiments greater than 2.0 moles of stabilizer per mole of lithium in the initiator, and in other embodiments greater than 3.0 moles of stabilizer per mole of lithium in the initiator are introduced into the polymerization mixture. In these or other embodiments, less than 8.0 moles of stabilizer per mole of lithium, in other embodiments less than 7.0 moles of stabilizer per mole of lithium, in other embodiments less than 6.0 moles of stabilizer per mole of lithium, in other embodiments less than 5.0 moles of stabilizer per mole of lithium, in other embodiments less than 4.5 moles of stabilizer per mole of lithium, in other embodiments less than 4.0 moles of stabilizer per mole of lithium, and in other embodiments less than 3.5 moles of stabilizer per mole of lithium are introduced into the polymerization mixture. In one or more embodiments, from about 1.0 mole stabilizer / mole lithium to about 7.0 mole stabilizer / mole lithium, in other embodiments from about 2.0 mole stabilizer / mole lithium to about 6.0 mole stabilizer / mole lithium, and in other embodiments from about 3.0 mole stabilizer / mole lithium to about 5.0 mole stabilizer / mole lithium are introduced into the polymerization mixture. In one or more embodiments, no stabilizer (e.g., hydrocarbyl hydrocarbyloxy silane) is employed.

[0104] In other embodiments, the amount of stabilizer (i.e., hydrocarbyl hydrocarbyloxysilane) employed in the practice of the present invention may be described as a molar ratio relative to the number of moles of functionalizing agent employed. In one or more embodiments, the ratio of the number of moles of stabilizer employed to the number of moles of functionalizing agent is from about 0:1 to about 16:1, in other embodiments from about 0.5:1 to about 10:1, and in other embodiments from about 2:1 to about 8:1. In these or other embodiments, the ratio of the number of moles of stabilizer employed to the number of moles of functionalizing agent is less than 7:1, in other embodiments less than 6:1, in other embodiments less than 5.5:1, in other embodiments less than 5:1, and in other embodiments less than 4.5:1.

[0105] In one or more embodiments, the stabilization of the polymer (i.e., the introduction of the stabilizer) is carried out in the same container in which the polymerization is carried out. In these embodiments, this will include the same container in which the modification is carried out. In other embodiments, the stabilization of the polymer (i.e., the introduction of the stabilizer) is carried out outside the container in which the polymerization is carried out. Similarly, in one or more embodiments, the stabilization of the polymer is carried out outside the container in which the modification of the polymer is carried out. For example, in one or more embodiments, the stabilizer can be added to the polymerization mixture (i.e., polymer cement) in a container or a transfer line, which is downstream of the container in which the polymerization is carried out and downstream of the container in which the polymer modification is carried out. For the purposes of this specification, the container or conduit in which the stabilizer is introduced can be referred to as the second container or the second reaction zone relative to the polymerization container. In other embodiments, the stabilizer can be introduced into the polymer when the polymer is suspended or dissolved in the monomer.

[0106] As described above, one of the benefits of embodiments of the present invention is that favorable polymer properties can be achieved in the absence of a stabilizer. Thus, embodiments of the present invention prepare polymer compositions as defined herein in the absence of a stabilizer (e.g., no stabilizer is employed or included in the polymerization mixture). In one or more embodiments, less than 3 moles of stabilizer per mole of lithium in the initiator, less than 2 moles of stabilizer per mole of lithium in the initiator, less than 1 mole of stabilizer per mole of lithium in the initiator, and less than 0.5 moles of stabilizer per mole of lithium in the initiator are introduced into the polymerization mixture.

[0107] Antioxidants

[0108] In one or more embodiments, an antioxidant may be added to the polymerization mixture after the functionalizing agent is introduced into the reactive polymer, optionally after the addition of a quencher and / or antioxidant, optionally after or with a stabilizer, and optionally after recovery or isolation of the functionalized polymer. Exemplary antioxidants include 2,6-di-tert-butyl-4-methylphenol.

[0109] In one or more embodiments, processing aids and other optional additives (eg, oil) may be added to the polymer glue after the polymer is formed.

[0110] Optional quenching

[0111] In one or more embodiments, after the reaction between the reactive polymer and the functionalizing agent has been completed or ended, a quencher may be added to the polymerization mixture to deactivate any residual reactive polymer chains and catalyst or catalyst components. The quencher may include a protic compound, including but not limited to alcohols, carboxylic acids, inorganic acids, water, or mixtures thereof. The amount of quencher employed may range from 0.5 moles of quencher per mole of lithium used to initiate polymerization to 10 moles of quencher per mole of lithium used to initiate polymerization.

[0112] Condensation accelerator

[0113] In one or more embodiments, after the functionalizing agent is introduced into the reactive polymer, optionally after adding a quencher and / or an antioxidant, optionally after or with a stabilizer, and optionally after reclaiming or separating the functionalized polymer, a condensation promoter can be added to the polymerization mixture. Useful condensation promoters include tin and / or titanium carboxylates and tin and / or titanium alkoxides. A specific example is 2-ethylhexyl titanium oxide. Useful condensation catalysts and uses thereof are disclosed in U.S. Patent Publication No. 2005 / 0159554 (patent No. US 7,683,151), which is incorporated herein by reference. In other embodiments, organic acids can be used as condensation promoters. Useful types of organic acids include aliphatic, alicyclic and aromatic monocarboxylic acids, dicarboxylic acids, tricarboxylic acids and tetracarboxylic acids. Specific examples of useful organic acids include, but are not limited to, acetic acid, propionic acid, butyric acid, caproic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, cyclohexanoic acid and benzoic acid.

[0114] The amount of condensation promoter employed in the practice of the present invention can be described relative to the number of moles of lithium associated with the initiator. In one or more embodiments, the number of moles of condensation promoter per mole of lithium is greater than 1.0 mole of condensation promoter / mole of lithium in the initiator, greater than 1.5 moles of condensation promoter / mole of lithium in the initiator in other embodiments, and greater than 1.8 moles of condensation promoter / mole of lithium in the initiator in other embodiments. In these or other embodiments, less than 4.0 moles of condensation promoter / mole of lithium, less than 3.3 moles of condensation promoter / mole of lithium in other embodiments, and less than 3.0 moles of condensation promoter / mole of lithium in other embodiments are introduced into the polymerization mixture. In one or more embodiments, from about 1.0 mole of condensation promoter / mole of lithium to about 4.0 moles of condensation promoter / mole of lithium, from about 1.5 moles of condensation promoter / mole of lithium to about 3.3 moles of condensation promoter / mole of lithium in other embodiments, and from about 1.8 moles of condensation promoter / mole of lithium to about 3.0 moles of condensation promoter / mole of lithium in other embodiments are introduced into the polymerization mixture.

[0115] Polymer desolventization

[0116] As described above, after modification, optional stabilization and optional introduction of condensation promoters and / or antioxidants, the polymer product (i.e., the blend of functionalized polymers) undergoes separation from the solvent, which can be referred to as desolvation. In other words, as described above, the polymer is synthesized in an organic solvent, and during the desolvation step, the organic solvent is separated from the polymer.

[0117] In a specific embodiment, desolventizing includes hot water and / or steam condensation. For example, the polymeric mixture of the blend comprising the modified polymer can be merged with a steam or hot water stream. The heat associated with the steam or hot water stream volatilizes the solvent and any unreacted monomers. The polymer product is then dispersed in the aqueous phase in the form of, for example, polymer crumbs. The properties and size of the polymer crumbs can be controlled typically by introducing mechanical energy (for example, in the form of a mixer).

[0118] In one or more embodiments, the polymer crumb is temporarily stored in water as a crumb dispersion until a subsequent drying step, which will be described below. The crumb dispersion is typically a mixture of polymer particles or crumbs and water. The polymer particles (which may also be referred to as coagulated polymer) are typically macroscopic and have at least one dimension greater than 1 mm. The crumb dispersion can be contained in a tank, such as a conventional reaction tank, such as a continuous stirred tank reactor.

[0119] In one or more embodiments, the polymer crumbs may be further processed to remove residual solvent and dry the polymer (i.e., separate the polymer from water). In practicing the present invention, the polymer may be dried using conventional techniques, which may include one or more of filtration, pressing, and heating. After desolventization and drying, the volatile content of the dried polymer may be 2.0% or less, in other embodiments 1.0% or less, and in other embodiments 0.5% or less by weight of the polymer.

[0120] In other embodiments, the polymer product may be desolventized by using a devolatilizer, which is an extruder-type device that may be operated in conjunction with heat and / or vacuum. In other embodiments, the polymerization mixture may be directly drum dried.

[0121] Regardless of the method used to desolventize and dry the polymer, the final polymer product may be referred to as dried polymer. The dried polymer may be molded or otherwise manipulated to form a bag using conventional techniques.

[0122] Polymer properties of dried polymers

[0123] In one or more embodiments, the dried, unaged blends of the functionalized polymers of the present invention are characterized by a favorable Mooney viscosity (ML 1+4 @100°C). Specifically, in one or more embodiments, the blend of functionalized polymers has a Mooney viscosity (ML) of less than 95, in other embodiments less than 90, and in other embodiments less than 85 within 24 hours of desolventization and drying. 1+4 @100°C). In these or other embodiments, the blend of functionalized polymers has a Mooney viscosity (ML) of from about 35 to about 120, in other embodiments from about 55 to about 95, in other embodiments from about 60 to about 90, and in other embodiments from about 65 to about 85 within 24 hours of desolventizing and drying. 1+4 @100°C). For the purpose of this specification, the dry, unaged Mooney viscosity (ML 1+4 @100°C) can be called the Mooney viscosity of the package.

[0124] Polymer properties of aged polymers

[0125] As noted above, the functionalized polymer blends of the present invention are characterized by favorable aged Mooney viscosities (ML 1+4 @100°C). Specifically, in one or more embodiments, the blend of functionalized polymers has a Mooney viscosity (ML) of less than 120, in other embodiments less than 105, and in other embodiments less than 95 when aged for two years after desolvation and drying. 1+4 @100°C). In one or more embodiments, the blend of functionalized polymers has a Mooney viscosity (ML) of from about 40 to about 105, in other embodiments from about 50 to about 100, and in other embodiments from about 60 to about 95 when aged for two years after desolvation and drying. 1+4 @100°C). For the purposes of this specification, and particularly with respect to Mooney viscosity at two years of aging, accelerated aging may be conducted at 100°C for two days, instead of two years of room temperature aging. In other words, for the purposes of this specification, the two aging methods are treated equally with respect to the viscosity obtained.

[0126] It should be understood that the polymer composition of the present invention comprises a variety of functionalized polymers, including mono-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers and di-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers. The relative amounts of mono-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers and di-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers can be described as the molar percentage of mono-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers, wherein the balance is di-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers. In one or more embodiments, the polymer composition comprises about 15 mol % to about 70 mol %, in other embodiments about 20 mol % to about 65 mol %, in other embodiments about 25 mol % to about 55 mol %, and in other embodiments about 30 mol % to about 45 mol % of mono-hydrocarbyloxysilyl functionalized polydiene, wherein the balance is di-hydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers.

[0127] As mentioned above, polymer composition of the present invention is advantageously highly functionalized. The degree of functionalization can be quantitatively described as the molar percentage of functionalized polymer in the polymer composition. In one or more embodiments, greater than 50 mole %, greater than 60 mole % in other embodiments, and greater than 70 mole % of polymer is functionalized in other embodiments in the polymer composition.

[0128] Industrial Applicability

[0129] In one or more embodiments, the functionalized polydiene and polydiene copolymers of the present invention can be used to formulate vulcanizable rubber compositions, which can be used, for example, to prepare tire components. Rubber compounding techniques and additives used therein are generally disclosed in "The Compounding and Vulcanization of Rubber, in Rubber Technology" (2nd edition, 1973).

[0130] Generally speaking, these vulcanizable rubber compositions comprise a vulcanizable rubber component, a reinforcing filler and a curing agent or curing agent system. These compositions may also optionally comprise a metal activator, a resin and a processing oil, as well as the various ingredients that may be conventionally included in these vulcanizable rubber compositions.

[0131] Ingredients of the vulcanizable composition

[0132] In one or more embodiments, the stabilized functionalized polydiene or polydiene copolymer of the present invention can form all or part of the rubber component of the vulcanizable composition. That is, the rubber component can include other vulcanizable rubbers, which can also be referred to as elastomeric polymers or simply elastomers.

[0133] The rubber composition can be prepared by using the polymer of the present invention alone or in combination with other elastomers (i.e., a polymer that can be vulcanized to form a composition having rubber or elastomeric properties). Other elastomers that can be used include natural rubber and synthetic rubber. Synthetic rubber is generally derived from the polymerization of conjugated diene monomers, the copolymerization of conjugated diene monomers with other monomers (such as, vinyl-substituted aromatic monomers), or the copolymerization of ethylene with one or more alpha-olefins and optionally one or more diene monomers.

[0134] Exemplary elastomers include natural rubber, synthetic polyisoprene, polybutadiene, polyisobutylene-isoprene copolymer, chloroprene rubber, ethylene-propylene copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-isoprene-butadiene copolymer, isoprene-butadiene copolymer, ethylene-propylene-diene copolymer, polysulfide rubber, acrylic rubber, polyurethane rubber, silicone rubber, epichlorohydrin rubber and mixtures thereof. These elastomers can have a variety of macromolecular structures, including linear structures, branched structures and star structures.

[0135] The rubber composition may include fillers, such as inorganic and organic fillers. Examples of organic fillers include carbon black and starch. Examples of inorganic fillers include silicon dioxide, aluminum hydroxide, magnesium hydroxide, mica, talc (hydrated magnesium silicate) and clay (hydrated aluminum silicate). Carbon black and silicon dioxide are the most commonly used fillers in manufacturing tires. In certain embodiments, a mixture of different fillers may be advantageously used.

[0136] In one or more embodiments, the carbon black includes furnace black, channel black and lamp black. More specific examples of carbon black include super wear-resistant furnace black, medium super wear-resistant furnace black, high wear-resistant furnace black, fast extrusion furnace black, fine furnace black, semi-reinforced furnace black, medium processing channel black, difficult processing channel black, conductive channel black and acetylene black.

[0137] In certain embodiments, the surface area (EMSA) of the carbon black may be at least 20 m 2 / g, and in other embodiments is at least 35m 2 / g; surface area values ​​can be determined by ASTM D-1765 using the cetyltrimethylammonium bromide (CTAB) technique. Carbon black can be in a granular form or a non-granular flocculent form. The preferred form of carbon black can depend on the type of mixing equipment used to mix the rubber compound.

[0138] Some commercially available silicas that can be used include Hi-Sil TM 215.Hi-Sil TM 233 and Hi-Sil TM 190 (PPG Industries, Inc., Pittsburgh, PA). Other suppliers of commercially available silica include Grace Davison, Baltimore, MD, Degussa Corp, Parsippany, NJ, Rhodia Silica Systems, Cranbury, NJ, and JM Huber Corp., Edison, NJ.

[0139] In one or more embodiments, the silica can be characterized by its surface area, which gives a measure of its reinforcing properties. The Brunauer, Emmet and Teller ("BET") method (described in J. Am. Chem. Soc., 1939, Vol. 60, pp. 309-319) is a recognized method for determining surface area. The BET surface area of ​​silica is typically less than 450 m 2 / g. Useful ranges of surface area include about 32 to about 400 m 2 / g, about 100 to about 250m 2 / g and about 150 to about 220m 2 / g.

[0140] The pH of the silica is typically from about 5 to about 7 or slightly above 7, or in other embodiments, from about 5.5 to about 6.8.

[0141] In one or more embodiments, when silica is employed as a filler (alone or in combination with other fillers), coupling agents and / or shielding agents may be added to the rubber composition during mixing in order to enhance the interaction of the silica with the elastomer. Useful coupling agents and shielding agents are disclosed in U.S. Pat. Nos. 3,842,111; 3,873,489; 3,978,103; 3,997,581; 4,002,594; 5,580,919; 5,583,245; 5,663,396; 5,674,932; 5,684,171; 5,684,172; 5,696,197; 6,608,145; 6,667,362; 6,579,949; 6,590,017; 6,525,118; 6,342,552; and 6,683,135, which are incorporated herein by reference.

[0142] In one or more embodiments, the vulcanizable composition of the present invention may include one or more resins. As the technician will appreciate, resins may include plasticizing resins and hardening or thermosetting resins. Available plasticizing resins include hydrocarbon resins, such as alicyclic resins, aliphatic resins, aromatic resins, terpene resins and combinations thereof. Available resins may be commercially available from multiple companies under various trade names, including for example Chemfax, Dow Chemical Company, Eastman Chemical Company, Idemitsu, Neville Chemical Company, Nippon, Polysat Inc., Resinall Corp., Pinova Inc., Yasuhara Chemical Co., Ltd., Arizona Chemical and SI Group Inc. and Zeon.

[0143] In one or more embodiments, useful hydrocarbon resins may be characterized by a glass transition temperature (Tg) of about 30°C to about 160°C, in other embodiments about 35°C to about 60°C, and in other embodiments about 70°C to about 110°C. In one or more embodiments, useful hydrocarbon resins may also be characterized by a softening point above their Tg. In certain embodiments, useful hydrocarbon resins have a softening point of about 70°C to about 160°C, in other embodiments about 75°C to about 120°C, and in other embodiments about 120°C to about 160°C.

[0144] In certain embodiments, one or more alicyclic resins are used in combination with one or more of an aliphatic resin, an aromatic resin, and a terpene resin. In one or more embodiments, one or more alicyclic resins are used as the major weight component (e.g., greater than 50 wt %) relative to the total loading of the resin. For example, the resin employed comprises at least 55 wt %, in other embodiments at least 80 wt %, and in other embodiments at least 99 wt % of one or more alicyclic resins.

[0145] In one or more embodiments, the alicyclic resin includes both alicyclic homopolymer resins and alicyclic copolymer resins, including those derived from alicyclic monomers, which are optionally mixed with one or more other (non-alicyclic) monomers, wherein the majority of all monomers by weight are alicyclic. Non-limiting examples of available alicyclic resins suitably include cyclopentadiene ("CPD") homopolymer or copolymer resins, dicyclopentadiene ("DCPD") homopolymer or copolymer resins, and combinations thereof. Non-limiting examples of alicyclic copolymer resins include CPD / vinyl aromatic copolymer resins, DCPD / vinyl aromatic copolymer resins, CPD / terpene copolymer resins, DCPD / terpene copolymer resins, CPD / aliphatic copolymer resins (e.g., CPD / C5 fractional copolymer resins), DCPD / aliphatic copolymer resins (e.g., DCPD / C5 fractional copolymer resins), CPD / aromatic copolymer resins (e.g., CPD / C9 fractional copolymer resins), DCPD / aromatic copolymer resins (e.g., DCPD / C9 fractional copolymer resins), CPD / C In some embodiments, the cycloaliphatic resin may include a hydrogenated form of one of the above-mentioned cycloaliphatic resins (i.e., a hydrogenated cycloaliphatic resin). In other embodiments, the cycloaliphatic resin does not include any hydrogenated cycloaliphatic resin; in other words, the cycloaliphatic resin is not hydrogenated.

[0146] In certain embodiments, one or more aromatic resins are used in combination with one or more of an aliphatic resin, an alicyclic resin, and a terpene resin. In one or more embodiments, one or more aromatic resins are used as the major weight component (e.g., greater than 50 wt %) relative to the total loading of the resin. For example, the resin employed comprises at least 55 wt %, in other embodiments at least 80 wt %, and in other embodiments at least 99 wt % of one or more aromatic resins.

[0147] In one or more embodiments, aromatic resins include both aromatic homopolymer resins and aromatic copolymer resins, including those derived from a combination of one or more aromatic monomers and one or more other (non-aromatic) monomers, wherein the largest amount of any type of monomer is aromatic. Non-limiting examples of available aromatic resins include coumarone-indene resins and alkyl-phenol resins and vinyl aromatic homopolymer or copolymer resins, such as those derived from one or more of the following monomers: alpha-methylstyrene, styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-(tert-butyl)styrene, methoxystyrene, chlorostyrene, hydroxystyrene, vinyl mesitylene, divinylbenzene, vinylnaphthalene, or any vinyl aromatic monomer obtained from a C9 fraction or a C8-C10 fraction. Non-limiting examples of vinyl aromatic copolymer resins include vinyl aromatic / terpene copolymer resins (e.g., limonene / styrene copolymer resins), vinyl aromatic / C5 fraction resins (e.g., C5 fraction / styrene copolymer resins), vinyl aromatic / aliphatic copolymer resins (e.g., CPD / styrene copolymer resins and DCPD / styrene copolymer resins). Non-limiting examples of alkyl-phenol resins include alkylphenol-acetylene resins, such as p-tert-butylphenol-acetylene resins, alkylphenol-formaldehyde resins (such as those with a low degree of polymerization). In certain embodiments, the aromatic resin may include a hydrogenated form of one of the above aromatic resins (i.e., a hydrogenated aromatic resin). In other embodiments, the aromatic resin does not include any hydrogenated aromatic resins; in other words, the aromatic resin is not hydrogenated.

[0148] In certain embodiments, one or more aliphatic resins are used in combination with one or more of alicyclic resins, aromatic resins, and terpene resins. In one or more embodiments, one or more aliphatic resins are used as the major weight component (e.g., greater than 50 wt %) relative to the total loading of the resin. For example, the resin employed comprises at least 55 wt %, in other embodiments at least 80 wt %, and in other embodiments at least 99 wt % of one or more aliphatic resins.

[0149] In one or more embodiments, aliphatic resins include both aliphatic homopolymer resins and aliphatic copolymer resins, including those resins derived from a combination of one or more aliphatic monomers and one or more other (non-aliphatic) monomers, wherein the largest amount of any type of monomer is aliphatic. Non-limiting examples of available aliphatic resins include homopolymer or copolymer resins of C5 fractions, C5 fractions / C9 fractions copolymer resins, C5 fractions / vinyl aromatic copolymer resins (e.g., C5 fractions / styrene copolymer resins), C5 fractions / alicyclic copolymer resins, C5 fractions / C9 fractions / alicyclic copolymer resins, and combinations thereof. Non-limiting examples of alicyclic monomers include, but are not limited to, cyclopentadiene ("CPD") and dicyclopentadiene ("DCPD"). In certain embodiments, aliphatic resins may include a hydrogenated form of one of the above-mentioned aliphatic resins (i.e., hydrogenated aliphatic resins). In other embodiments, aliphatic resins do not include any hydrogenated aliphatic resins; in other words, in such embodiments, aliphatic resins are not hydrogenated.

[0150] In one or more embodiments, the terpene resin includes both terpene homopolymer resins and terpene copolymer resins, including those resins derived from a combination of one or more terpene monomers and one or more other (non-terpene) monomers, wherein the largest amount of any type of monomer is a terpene. Non-limiting examples of usable terpene resins include α-pinene resins, β-pinene resins, limonene resins (e.g., L-limonene, D-limonene, dipentene that is a racemic mixture of L-isomers and D-isomers), β-phellandrene, δ-3-carene, δ-2-carene, pinene-limonene copolymer resins, terpene-phenol resins, aromatic modified terpene resins, and combinations thereof. In certain embodiments, the terpene resin may include a hydrogenated form of one of the above-mentioned terpene resins (i.e., a hydrogenated terpene resin). In other embodiments, the terpene resin does not include any hydrogenated terpene resins; in other words, in such embodiments, the terpene resin is not hydrogenated.

[0151] In one or more embodiments, the vulcanizable compositions of the present invention include a process oil, which may also be referred to as an extender oil. In one or more embodiments, the vulcanizable compositions are free or substantially free of process oil.

[0152] In a particular embodiment, the oil used includes those that are commonly used as extender oils. Available oils or extenders that can be used include but are not limited to aromatic oils, paraffin oils, naphthenic oils, vegetable oils except castor oil, low PCA oils (including MES, TDAE and SRAE) and heavy naphthenic oils. Suitable low PCA oils also include oils from various plant sources, such as oils that can be harvested from vegetables, nuts and seeds. Non-limiting examples include but are not limited to soybean oil or soybean oil, sunflower seed oil, safflower oil, corn oil, linseed oil, cottonseed oil, rapeseed oil, cashew nut oil, sesame oil, camellia oil, jojoba oil, macadamia oil, coconut oil and palm oil. As generally understood in the art, oil refers to those compounds with relative viscosity compared to other components (such as resins) of the vulcanizable composition.

[0153] In one or more embodiments, the oil includes those hydrocarbon compounds having greater than 15 carbon atoms per molecule, greater than 20 carbon atoms in other embodiments, greater than 25 carbon atoms in other embodiments, greater than 30 carbon atoms in other embodiments, greater than 35 carbon atoms in other embodiments, and greater than 40 carbon atoms in other embodiments. In these or other embodiments, the oil includes those hydrocarbon compounds having less than 250 carbon atoms per molecule, less than 200 carbon atoms in other embodiments, less than 150 carbon atoms in other embodiments, less than 120 carbon atoms in other embodiments, less than 100 carbon atoms in other embodiments, less than 90 carbon atoms in other embodiments, less than 80 carbon atoms in other embodiments, less than 70 carbon atoms in other embodiments, less than 60 carbon atoms in other embodiments, and less than 50 carbon atoms in other embodiments. In one or more embodiments, the oils include those hydrocarbon compounds having from about 15 to about 250, in other embodiments from about 20 to about 200, in other embodiments from about 25 to about 100 carbon atoms per molecule, in other embodiments from about 25 to about 70 carbon atoms per molecule, in other embodiments from about 25 to about 70 carbon atoms per molecule, in other embodiments from about 25 to about 60 carbon atoms per molecule, and in other embodiments from about 25 to about 40 carbon atoms per molecule.

[0154] In one or more embodiments, the oil includes those compounds having a dynamic viscosity at 25°C greater than 5 mPa·s, in other embodiments greater than 10 mPa·s, in other embodiments greater than 15 mPa·s, in other embodiments greater than 20 mPa·s, in other embodiments greater than 25 mPa·s, and in other embodiments greater than 30 mPa·s, in other embodiments greater than 35 mPa·s, and in other embodiments greater than 40 mPa·s. In these or other embodiments, the oil includes those compounds having a dynamic viscosity at 25°C less than 3000 mPa·s, in other embodiments less than 2500 mPa·s, in other embodiments less than 2000 mPa·s, in other embodiments less than 1500 mPa·s, in other embodiments less than 1000 mPa·s, in other embodiments less than 750 mPa·s, in other embodiments less than 500 mPa·s, in other embodiments less than 250 mPa·s, in other embodiments less than 100 mPa·s, and in other embodiments less than 75 mPa·s. In one or more embodiments, the oils include those compounds having a dynamic viscosity at 25°C of about 5 mPa·s to 3000 mPa·s, in other embodiments about 15 mPa·s to about 2000 mPa·s, in other embodiments about 20 mPa·s to about 1500 mPa·s, in other embodiments about 25 mPa·s to about 1000 mPa·s, in other embodiments about 30 mPa·s to about 750 mPa·s, in other embodiments about 35 mPa·s to about 500 mPa·s, and in other embodiments about 50 mPa·s to about 250 mPa·s.

[0155] Many kinds of rubber curing agents (also referred to as vulcanizing agents) can be used, including sulfur-based or peroxide-based curing systems. Curing agents are described in the following documents: Kirk-Othmer, Encyclopedia of Chemical Technology, Vol. 20, pp. 365-468, (3rd edition 1982), especially Vulcanization Agents and Auxiliary Materials, pp. 390-402, and AY Coran, Vulcanization, Encyclopedia of Polymer Science and Engineering, (2nd edition 1989)), which are incorporated herein by reference. Vulcanizing agents can be used alone or in combination.

[0156] Other ingredients commonly used in rubber compounding may also be added to the rubber composition. These ingredients include accelerators, accelerator activators, oils, plasticizers, waxes, scorch inhibitors, processing aids, zinc oxide, tackifying resins, reinforcing resins, fatty acids (such as stearic acid), peptizers, and antidegradants (such as antioxidants and antiozonants). In a particular embodiment, the oil employed includes those oils commonly used as extender oils, which are described above.

[0157] Ingredient Amount

[0158] As mentioned above, vulcanizable compositions comprise vulcanizable rubber component.In one or more embodiments, based on the gross weight of composition, vulcanizable compositions comprise and be greater than 20 weight %, in other embodiments, be greater than 30 weight %, and in other embodiments, be greater than 40 weight % vulcanizable rubber component (it can be referred to as rubber component) of weight %.In these or other embodiments, based on the gross weight of vulcanizable compositions, vulcanizable compositions comprise and be less than 90 weight %, in other embodiments, be less than 70 weight %, and in other embodiments, be less than 60 weight % of rubber component.In one or more embodiments, based on the gross weight of vulcanizable compositions, vulcanizable compositions comprise and be less than 20 weight %, in other embodiments, be less than 70 weight %, and in other embodiments, be less than 60 weight % of rubber component.

[0159] In one or more embodiments, the rubber component of the vulcanizable composition of the present invention comprises greater than 10% by weight, greater than 30% by weight in other embodiments, and greater than 50% by weight of the functionalized polymer of the present invention in other embodiments, wherein the balance comprises other vulcanizable rubbers. In these or other embodiments, the rubber component of the vulcanizable composition of the present invention comprises less than 100% by weight, less than 90% by weight in other embodiments, and less than 80% by weight of the functionalized polymer of the present invention in other embodiments, wherein the balance comprises other vulcanizable rubbers. In one or more embodiments, the rubber component of the vulcanizable composition of the present invention comprises about 10% by weight to about 100% by weight, about 30% by weight to about 90% by weight in other embodiments, and about 50% by weight to about 80% by weight of the functionalized polymer of the present invention in other embodiments, wherein the balance comprises other vulcanizable rubbers.

[0160] filler

[0161] In one or more embodiments, the vulcanizable composition comprises greater than 0 parts by weight (pbw), greater than 40 pbw in other embodiments, greater than 60 pbw in other embodiments, greater than 80 pbw in other embodiments, greater than 90 pbw in other embodiments, greater than 100 pbw in other embodiments, and greater than 110 pbw of filler in other embodiments, per 100 parts by weight of rubber (phr). In these or other embodiments, the vulcanizable composition comprises less than 200 pbw, less than 160 pbw in other embodiments, less than 150 pbw in other embodiments, and less than 140 pbw of filler in other embodiments, in phr. In one or more embodiments, the vulcanizable composition comprises from about 40 pbw to about 200 pbw, from about 60 pbw to about 160 pbw in other embodiments, and from about 100 pbw to about 150 pbw of filler in other embodiments.

[0162] Carbon Black

[0163] In one or more embodiments, in every 100 parts by weight of rubber (phr), the vulcanizable composition comprises greater than 0 parts by weight (pbw), greater than 1pbw in other embodiments, greater than 2pbw in other embodiments, greater than 5pbw in other embodiments, greater than 10pbw in other embodiments, and greater than 15pbw of carbon black in other embodiments. In these or other embodiments, in phr, the vulcanizable composition comprises less than 60pbw, less than 40pbw in other embodiments, and less than 30pbw of carbon black in other embodiments. In one or more embodiments, in phr, the vulcanizable composition comprises about 1pbw to about 60pbw, about 5pbw to about 50pbw in other embodiments, and about 10pbw to about 40pbw of carbon black in other embodiments. In one or more embodiments, the vulcanizable composition does not contain or is substantially free of carbon black.

[0164] Silicon dioxide

[0165] In one or more embodiments, in every 100 parts by weight of rubber (phr), the vulcanizable composition comprises greater than 5 parts by weight (pbw), greater than 40 pbw in other embodiments, greater than 60 pbw in other embodiments, greater than 70 pbw in other embodiments, greater than 80 pbw in other embodiments, greater than 90 pbw in other embodiments, greater than 100 pbw in other embodiments, and greater than 110 pbw of silica in other embodiments. In these or other embodiments, in phr, the vulcanizable composition comprises less than 140 pbw, less than 130 pbw in other embodiments, less than 120 pbw in other embodiments, less than 120 pbw in other embodiments, and less than 100 pbw of silica in other embodiments. In one or more embodiments, in phr, the vulcanizable composition comprises about 40 pbw to about 140 pbw, about 60 pbw to about 130 pbw in other embodiments, and about 80 pbw to about 120 pbw of silica in other embodiments.

[0166] Filling ratio

[0167] In one or more embodiments, the vulcanizable composition may be characterized by the ratio of silica to other filler compounds, such as carbon black. In one or more embodiments, silica is used in excess relative to other fillers, such as carbon black. In one or more embodiments, the ratio of the amount of silica to carbon black is greater than 1:1, greater than 2:1 in other embodiments, greater than 3:1 in other embodiments, and greater than 5:1 in other embodiments, based on a weight ratio. In one or more embodiments, the weight ratio of silica to carbon black is from about 1:1 to about 30:1, from about 2.1: to about 20:1 in other embodiments, and from about 3:1 to about 10:1 in other embodiments.

[0168] Silica coupling agent

[0169] In one or more embodiments, the vulcanizable composition comprises greater than 1 part by weight (pbw), greater than 2 pbw in other embodiments, and greater than 5 pbw of silica coupling agent per 100 parts by weight of silica. In these or other embodiments, the vulcanizable composition comprises less than 20 pbw, less than 15 pbw in other embodiments, and less than 10 pbw of silica coupling agent per 100 parts by weight of silica. In one or more embodiments, the vulcanizable composition comprises from about 1 pbw to about 20 pbw of silica coupling agent per 100 parts by weight of silica, from about 2 pbw to about 15 pbw of silica coupling agent in other embodiments, and from about 5 pbw to about 10 pbw of silica coupling agent in other embodiments. In one or more embodiments, the vulcanizable composition is free of or substantially free of silica coupling agent.

[0170] Plasticizing resin

[0171] In one or more embodiments, the vulcanizable composition comprises greater than 0.1 parts by weight (pbw), greater than 0.5 pbw, greater than 1.0 pbw, greater than 1.5 pbw, greater than 15 pbw, and greater than 25 pbw of a plasticizing resin (e.g., a hydrocarbon resin) per 100 parts by weight of rubber (phr). In these or other embodiments, the vulcanizable composition comprises less than 150 pbw, less than 120 pbw, less than 90 pbw, less than 80 pbw, less than 60 pbw, less than 45 pbw, less than 15 pbw, less than 10 pbw, and less than 3.0 pbw of a plasticizing resin (e.g., a hydrocarbon resin) in phr. In one or more embodiments, the vulcanizable composition comprises from about 1 pbw to about 150 pbw, from about 0.5 pbw to about 15 pbw in other embodiments, from about 1 pbw to about 10 pbw in other embodiments, from about 1.5 pbw to about 3 pbw in other embodiments, from about 15 pbw to about 100 pbw in other embodiments, and from about 25 pbw to about 80 pbw of a plasticizing resin (e.g., a hydrocarbon resin) in other embodiments. In one or more embodiments, the vulcanizable composition is free of or substantially free of a plasticizing resin.

[0172] Processing oil / increasing oil

[0173] In one or more embodiments, the vulcanizable composition comprises greater than 0.1 parts by weight (pbw), greater than 0.5 pbw, greater than 1 pbw, greater than 1.5 pbw, and greater than 2 pbw of a process oil (e.g., naphthenic oil) per 100 parts by weight of rubber (phr). In these or other embodiments, the vulcanizable composition comprises less than 20 pbw, less than 18 pbw, less than 15 pbw, less than 12 pbw, less than 10 pbw, and less than 8 pbw, less than 5 pbw, and less than 3 pbw of a process oil in phr. In one or more embodiments, the vulcanizable composition comprises from about 0.1 pbw to about 20 pbw, from about 0.5 pbw to about 18 pbw, from about 0.5 pbw to about 15 pbw, from about 1 pbw to about 10 pbw, from about 0.5 pbw to about 18 pbw, from about 1.5 pbw to about 3.0 pbw, and from about 2 pbw to about 12 pbw of oil in phr. In one or more embodiments, the vulcanizable composition is free or substantially free of oil.

[0174] Plasticizer additives

[0175] In one or more embodiments, plasticizing resin and processing oil can be collectively referred to as plasticizing additives, plasticizing ingredients, plasticizing components or plasticizing systems. In one or more embodiments, in every 100 parts by weight of rubber (phr), the vulcanizable composition of the present invention comprises more than 0.5 parts by weight (pbw), more than 1pbw in other embodiments, and more than 1.5pbw of plasticizing additives in other embodiments. In these or other embodiments, in phr, the vulcanizable composition comprises less than 15pbw, less than 12pbw in other embodiments, less than 10pbw in other embodiments, less than 5pbw in other embodiments, and less than 3pbw of plasticizing additives in other embodiments. In one or more embodiments, in phr, the vulcanizable composition comprises about 0.5pbw to about 15pbw, about 1pbw to about 10pbw in other embodiments, and about 1.5pbw to about 3pbw of plasticizing additives in other embodiments.

[0176] Hardening resin

[0177] In one or more embodiments, the vulcanizable composition comprises less than 2 pbw, in other embodiments less than 1 pbw, and in other embodiments less than 0.5 pbw of hardening resin in phr. In one or more embodiments, the vulcanizable composition comprises from about 0.1 pbw to about 8 pbw, in other embodiments from about 0.5 pbw to about 6 pbw, and in other embodiments from about 2 pbw to about 4 pbw of hardening resin in phr. In one or more embodiments, the vulcanizable composition is free of or substantially free of hardening resin.

[0178] sulfur

[0179] In one or more embodiments, the vulcanizable composition includes sulfur as a curing agent. In one or more embodiments, in every 100 parts by weight of rubber (phr), the vulcanizable composition includes greater than 0.1 parts by weight (pbw), greater than 0.3pbw in other embodiments, and greater than 0.9pbw of sulfur in other embodiments. In these or other embodiments, in phr, the vulcanizable composition includes less than 6pbw, less than 4pbw in other embodiments, less than 3.0pbw in other embodiments, and less than 2.0pbw of sulfur in other embodiments. In one or more embodiments, in phr, the vulcanizable composition includes about 0.1pbw to about 5.0pbw, about 0.8pbw to about 2.5pbw in other embodiments, about 1pbw to about 2.0pbw in other embodiments, and about 1.0pbw to about 1.8pbw of sulfur in other embodiments.

[0180] Processing of vulcanizable compositions

[0181] In one or more embodiments, the vulcanizable composition is prepared by mixing the vulcanizable rubber with a filler to form a masterbatch, and then adding a curing agent to the masterbatch. The preparation of the masterbatch can be carried out using one or more sub-mixing steps, wherein, for example, one or more ingredients can be added to the composition in sequence after preparing an initial mixture by mixing two or more ingredients. In addition, using conventional techniques, additional ingredients such as but not limited to carbon black, additional fillers, silica, silica coupling agents, silica dispersants, process oils, processing aids (such as zinc oxide and fatty acids) and antidegradants (such as antioxidants or antiozonants) can be added to the preparation of the vulcanizable composition.

[0182] Mixing conditions

[0183] In one or more embodiments, various components of the rubber component (e.g., rubber component and filler) are introduced into a vulcanizable rubber as initial ingredients to form a rubber masterbatch, optionally with carbon black and silica fillers. Therefore, these components are subjected to high shear, high temperature mixing. In one or more embodiments, the masterbatch mixing step is mixed at a minimum temperature of more than 110°C, more than 130°C in other embodiments, and more than 150°C in other embodiments. In one or more embodiments, high shear, high temperature mixing is carried out at a temperature of about 110°C to about 170°C. In one or more embodiments, the masterbatch mixing step or one or more sub-steps of the masterbatch mixing step can be characterized by the peak temperature obtained by the composition during mixing. The peak temperature can also be referred to as the dripping temperature. In one or more embodiments, the peak temperature of the composition during the masterbatch mixing step can be at least 140°C, at least 150°C in other embodiments, and at least 160°C in other embodiments. In these or other embodiments, the peak temperature of the composition during the masterbatch mixing step may be from about 140°C to about 200°C, in other embodiments from about 150°C to about 190°C, and in other embodiments from about 160°C to about 180°C.

[0184] After the initial mixing, the composition (i.e., masterbatch) is cooled to a temperature of less than 100°C or less than 80°C in other embodiments, and a curing agent is added. In certain embodiments, mixing is continued at a temperature of about 90°C to about 110°C, or in other embodiments, mixing is continued at a temperature of about 95°C to about 105°C to prepare the final vulcanizable composition. After the masterbatch mixing step, a curing agent or curing agent system is introduced into the composition and mixing is continued to finally form a vulcanizable material composition. This mixing step may be referred to as a final mixing step, a curing mixing step, or a productive mixing step. The product obtained by this mixing step may be referred to as a vulcanizable composition.

[0185] In one or more embodiments, the final mixing step can be characterized by the peak temperature obtained by the composition during the final mixing. The skilled person will recognize that this temperature can also be referred to as the final drip temperature. In one or more embodiments, the peak temperature of the composition during the final mixing can be up to 130°C, up to 110°C in other embodiments, and up to 100°C in other embodiments. In these or other embodiments, the peak temperature of the composition during the final mixing can be from about 80°C to about 130°C, from about 90°C to about 115°C in other embodiments, and from about 95°C to about 105°C in other embodiments.

[0186] Mixing procedures and conditions particularly suitable for silica-filled tire formulations are described in U.S. Patent Nos. 5,227,425; 5,719,207; and 5,717,022 and European Patent No. 890,606, which are incorporated herein by reference. In one embodiment, an initial masterbatch is prepared by including the polymer and silica in the substantial absence of coupling agents and shielding agents.

[0187] Mixing equipment

[0188] All ingredients of the vulcanizable composition can be mixed with standard mixing equipment such as internal mixers (e.g., Banbury mixers or Brabender mixers), extruders, kneaders, and two-roll mills. Mixing can be carried out individually or in tandem. As mentioned above, the ingredients can be mixed in a single stage, or in other embodiments, in two or more stages. For example, in the first stage (i.e., mixing stage), a masterbatch is prepared, which generally comprises a rubber component and a filler. Once the masterbatch is prepared, a vulcanizing agent can be introduced and mixed into the masterbatch in the final mixing stage, which is generally carried out at a relatively low temperature to reduce the chance of premature vulcanization. Additional mixing stages can be adopted between the masterbatch mixing stage and the final mixing stage, sometimes referred to as re-refining.

[0189] According to an embodiment of the present invention, the use of functionalized polymers of the present invention provides the unexpected advantage of reducing alcohol generation (as volatiles) during rubber processing; for example, less ethanol is generated as volatiles during the rubber mixing step. According to an embodiment of the present invention, the amount of alcohol (e.g., ethanol) released from the functionalized polymers of the present invention is less than 5.0 mmol ethanol / kg processed polymer, less than 4.0 mmol ethanol / kg processed polymer in other embodiments, less than 3.5 mmol ethanol / kg processed polymer in other embodiments, and less than 3.0 mmol ethanol in other embodiments, excluding any alcohol (e.g., ethanol) generated by silane coupling agents. In addition, in view of the reduced loading of stabilizers required for processing the functionalized polymers of the present invention (i.e., the amount of alkoxysilanes that must be introduced into the functionalized polymer as stabilizers), the total volatile alcohols released during polymer processing are further reduced. According to embodiments of the present invention, the total volatile alcohols generated during rubber mixing (the volatile alcohols derived from the functionalized polymer and the stabilizer) are less than 110 mmol ethanol / kg processed polymer, in other embodiments less than 95 mmol ethanol / kg processed polymer, in other embodiments less than 80 mmol ethanol / kg processed polymer, and in other embodiments less than 70 mmol ethanol / kg processed polymer, excluding any alcohols generated by the silane coupling agent (e.g., ethanol).

[0190] Tire preparation

[0191] The vulcanizable composition can be processed into tire components according to common tire manufacturing techniques (including standard rubber molding, molding and curing techniques). Typically, vulcanization is achieved by heating the vulcanizable composition in a mold; for example, it can be heated to about 140°C to about 180°C. The cured or cross-linked rubber composition may be referred to as a vulcanized rubber, which typically contains a thermosetting three-dimensional polymer network. Other ingredients (such as fillers and processing aids) may be uniformly dispersed throughout the cross-linked network. Pneumatic tires may be prepared as discussed in U.S. Patent Nos. 5,866,171, 5,876,527, 5,931,211 and 5,971,046, which are incorporated herein by reference.

[0192] As described above, the vulcanizable compositions of the present invention can be cured to prepare various tire components. These tire components include, but are not limited to, tire treads, tire sidewalls, belts, inner liners, plies, and apex rubber cores. These tire components can be included in a variety of vehicle tires (including passenger tires).

[0193] Rubber compositions prepared from the polymers of the present invention are particularly useful for forming tire components such as treads, subtreads, sidewalls, carcass barriers, bead fillers, etc. In one or more embodiments, these tread or sidewall formulations may contain from about 10% to about 100% by weight of the polymers of the present invention, in other embodiments from about 35% to about 90% by weight of the polymers of the present invention, and in other embodiments from about 50% to about 80% by weight of the polymers of the present invention, based on the total weight of rubber in the formulation.

[0194] Example

[0195] In order to demonstrate the practice of the present invention, the following examples have been prepared and tested. However, the examples should not be considered to limit the scope of the present invention. The claims will be used to define the present invention.

[0196] The samples were prepared in a 378.5 liter reactor equipped with a heating / cooling jacket and agitator blades. Specifically, the reactive polymer cement was prepared by initially charging about 90 kg of hexane, about 36 kg of about 35% by weight styrene in hexane, and about 90 kg of about 23% by weight butadiene in hexane into the reactor, then adding 0.6 kg of 3% by weight butyl lithium, followed by 0.003 kg of 2,2-di(tetrahydrofuranyl)propane and 0.018 kg of potassium tert-amyl alcohol. Specifically, the monomers and solvents were charged into the reactor at room temperature, stirred, and heated to a stabilized temperature of 33°C. External heating was then stopped, and a butyl lithium initiator was charged to form a polymerization mixture. The polymerization mixture was allowed to exotherm to a peak, which typically occurred at about 23 minutes from the start of the butyl lithium charge, and the polymerization mixture was thermostated at about 85°C using a cooling jacket. A polymer sample was removed from the polymerization mixture and introduced into a 1 liter bottle and combined with about 10 mL of isopropanol and about 10 mL of a 10% solution of butylated hydroxytoluene (BHT).

[0197] Within about 5 minutes of peak polymerization temperature, the reactor was charged with a functionalizing agent of the type and amount provided in Table 1. The polymerization mixture was continuously agitated for about 30 minutes before ethylhexanoic acid (EHA) (about 0.114 kg) was added to the reactor followed by octyltriethoxysilane (OTES), if applicable, in the amount provided in Table 1. Then, 0.252 kg of butylated hydroxytoluene (BHT) was charged followed by about 0.023 kg of isopropanol.

[0198] Functionalizing agents employed and provided in Table I include: 3-(1,3 dimethylbutylene)aminopropyltriethoxysilane (3-EOS) and (glycidoxypropyl)(methyl)diethoxysilane (G-2-EOS). At this point in the process, samples were extracted for analysis by GPC using polystyrene standards and polystyrene Mark Houwink constants for peak molecular weight (this analysis was also used to determine % coupling), and Mooney viscosity (ML 1+4 The glass transition temperature (T) was measured by differential scanning calorimetry (DSC) in the range of -120°C to 23°C at a heating rate of 10°C / min. g ). The butadiene content (1,2-microstructure) and the vinyl microstructure of the styrene content were determined by infrared. Total nitrogen analysis was performed on (3x) the coagulated samples using a Mitsubishi ChemicalAnalytech NSX-2100 elemental analysis system.

[0199] The polymer analyzed at this point in the process may be referred to as the "blend jar" (eg, blend jar Mooney). For purposes of this specification and the present invention, the blend jar Mooney and the Mooney at solvent removal are considered equivalent.

[0200] The polymerization mixture is then transferred to a water-based desolventizing process. Specifically, a tank filled with water is heated to a temperature of about 82°C. The polymerization mixture is slowly added to the tank, which causes the hexane to volatilize; the volatiles are collected in a condenser. The polymer condenses in the presence of water to form a condensed polymer dispersion. The polymer is then dehydrated by passing the polymer-water mixture through a grinder (i.e., a single screw extruder equipped with a perforated die). The dehydrated polymer is then dried in an oven at 71°C for one hour and then heated in an oven at 60°C until dry (e.g., the water content is less than about 0.5 wt %). After drying, the polymer is packaged and the Mooney viscosity (ML 1+4 @100°C) to provide Bale Raw Mooney. Samples of the bales were aged by placing them in an oven at 100°C for 48 hours. The Mooney viscosity (ML 1+4 @100℃).

[0201] The polymer Mooney viscosity was determined using a Monsanto Mooney viscometer. The ML (1+4) value was measured on a large rotor at 100°C for 4 minutes with a preheating time of 1 minute.

[0202] Table I

[0203]

[0204] Vulcanizable compositions for some polymer samples were prepared in a 300 g Brabender mixer using a three-stage mixing procedure as shown in Table II and Table III. Remilling did not include the addition of any ingredients. The masterbatch stage was mixed at 50 rpm with a starting mixer temperature of 90°C and mixed for 5 minutes or until the sample reached 160°C, whichever occurred first. The remill stage was mixed at 50 rpm with a starting mixer temperature of 90°C and mixed for 3.0 minutes or until the sample reached 160°C, whichever occurred first. The final stage was mixed at 40 rpm with a starting mixer temperature of 60°C and mixed for 2.5 minutes or until the sample reached 100°C, whichever occurred first.

[0205] Table II

[0206]

[0207]

[0208] Mooney analysis was performed on the vulcanizable composition. The samples were cured at 145°C for 33 minutes and analyzed for mechanical and dynamic properties. Mechanical properties were tested according to ASTM D412, and dynamic properties were tested using a dynamic analyzer. The results of the analysis are set forth in Table III.

[0209] Table III

[0210] Polymer samples 3 4 7 8 Compound Mooney 101.3 94.4 99.8 100.6 Tanδ at 0℃ 0.183 0.182 0.19 0.163 Tanδ at 65℃ 0.094 0.098 0.095 0.087 ΔG'(MPa) 1.53 1.38 1.53 1.02

[0211] Various modifications and alterations will become apparent to those skilled in the art without departing from the scope and spirit of this invention.This invention should not be unduly limited to the illustrative embodiments set forth herein.

Claims

1. A polymer composition, comprising: A plurality of functionalized polymers, wherein the plurality comprises monohydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers and dihydrocarbyloxysilyl functionalized polydiene and / or polydiene copolymers, the polymer composition having an aged Mooney (ML) of about 40 to about 105 1+4 @100°C), wherein greater than 60 mol% of the polymers in the polymer composition are functionalized, and wherein the plurality, including from about 15 mol% to about 70 mol% of the plurality of functionalized polymers, are monohydrocarbyloxysilyl functionalized polydienes and / or polydiene copolymers, with the balance comprising dihydrocarbyloxysilyl functionalized polydienes and / or polydiene copolymers.

2. The polymer composition of claim 1, wherein the polymer composition is formed by reacting a reactive polydiene or polydiene copolymer with a first end-capping agent defined by the formula: Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and A is selected from the group consisting of an imine group, a carboxylate group, a cyclic tertiary amine group, a non-cyclic tertiary amine group, a pyridine group, a silazane group, an epoxy group, an isocyanate group, a cyano group, a carboxylic anhydride group, and a hydrocarbon sulfide group: Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and A is selected from the group consisting of an imine group, a carboxylate group, a cyclic tertiary amine group, a non-cyclic tertiary amine group, a pyridine group, a silazane group, an epoxy group, an isocyanate group, a cyano group, a carboxylic anhydride group and a hydrocarbon sulfide group.

3. The polymer composition of claim 1, wherein the polymer composition is formed by reacting a reactive polydiene or polydiene copolymer with a first end-capping agent defined by the formula: Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and each R 3 are independently a hydrocarbyl group, Where R 1 is a hydrocarbylene group, and each R 2 are independently hydrocarbyl groups.

4. The polymer composition of any one of the preceding claims, wherein greater than 70 mol % of the polymers in the polymer composition are functionalized.

5. The polymer composition of any one of the preceding claims, wherein the polymer composition has an aged Mooney (ML) of about 50 to about 100. 1+4 @100℃).

6. A method for preparing a polymer composition, the method comprising: include: (i) providing a reactive polydiene or polydiene copolymer; (ii) reacting a portion of the reactive polydiene or polydiene copolymer with a first end-capping agent, The first end-capping agent is a trihydrocarbyloxysilyl compound; (iii) reacting a portion of the reactive polydiene or polydiene copolymer with a second end-capping agent, the second end-capping agent being a dihydrocarbyloxysilyl compound, thereby forming a functionalized dihydrocarbyloxysilyl polydiene and / or polydiene copolymer, wherein the monohydrocarbyloxysilyl polydiene and the dihydrocarbyloxysilyl polydiene and / or polydiene copolymer form a blend; and (iv) separating the blend.

7. The method according to any one of the preceding claims, wherein the first capping agent is defined by the formula: Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and A is selected from the group consisting of an imine group, a carboxylate group, a cyclic tertiary amine group, a non-cyclic tertiary amine group, a pyridine group, a silazane group, an epoxy group, an isocyanate group, a cyano group, a carboxylic anhydride group and a hydrocarbon sulfide group.

8. The method according to any one of the preceding claims, wherein the second capping agent is defined by the formula: Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and A is selected from the group consisting of an imine group, a carboxylate group, a cyclic tertiary amine group, a non-cyclic tertiary amine group, a pyridine group, a silazane group, an epoxy group, an isocyanate group, a cyano group, a carboxylic anhydride group and a hydrocarbon sulfide group.

9. The method according to any one of the preceding claims, wherein the first capping agent is defined by the formula: Where R 1 is a hydrocarbylene group, each R 2 are independently a hydrocarbon group, and each R 3 are independently hydrocarbyl groups.

10. The method according to any one of the preceding claims, wherein the second capping agent is defined by the formula: Where R 1 is a hydrocarbylene group, and each R 2 are independently hydrocarbyl groups.

11. The method according to any one of the preceding claims, wherein the reactive polydiene or polydiene copolymer is formed by anionic polymerization of 1,3-butadiene, optionally together with monomers copolymerizable therewith, to form the reactive polydiene or polydiene copolymer.

12. The method of any one of the preceding claims, wherein the step of anionic polymerizing reaches a peak polymerization temperature of about -10°C to about 200°C.

13. The method according to any one of the preceding claims, wherein the reactive polydiene forms a polymerization mixture, and wherein the polymerization mixture comprises greater than 75 mole % of the reactive polydiene or polydiene copolymer, based on the total amount of polydiene or polydiene copolymer.

14. The method of any one of the preceding claims, wherein the step of reacting the reactive polydiene or polydiene copolymer with a first end-capping agent employs from about 0.15 moles of the first end-capping agent per mole of reactive polydiene or polydiene copolymer to about 0.50 moles of the first end-capping agent per mole of reactive polydiene or polydiene copolymer, and wherein the step of reacting the reactive polydiene or polydiene copolymer with a second end-capping agent employs from about 0.4 moles of the second end-capping agent per mole of the reactive polydiene or polydiene copolymer to about 0.8 moles of the second end-capping agent per mole of the reactive polydiene or polydiene copolymer.

15. The method of any one of the preceding claims, wherein the amount of the first end-capping agent used in the method and the second end-capping agent used in the method form a total amount of end-capping agent, and wherein the total amount of end-capping agent is greater than 0.70 moles of end-capping agent per mole of reactive polydiene or polydiene copolymer.

16. The method according to any one of the preceding claims, wherein the step of reacting the reactive polydiene or polydiene copolymer with a first end-capping agent and the step of reacting the reactive polydiene or polydiene copolymer with a second end-capping agent are performed with a solvent.

17. The process according to any one of the preceding claims, further comprising the step of separating the polydiene or polydiene copolymer from the solvent.

18. The method of any one of the preceding claims, wherein the polymer composition has an aged Mooney (ML) of about 40 to about 105. 1+4 @100℃).

19. The method of any one of the preceding claims, wherein the reactive polydiene or polydiene copolymer has an Mp of about 160 kg / mol to about 280 kg / mol.

20. The process according to any one of the preceding claims, wherein the step of anionically polymerizing 1,3-butadiene, optionally together with monomers copolymerizable therewith, to form the reactive polydiene or polydiene copolymer is carried out with a lithium-containing initiator.

21. The method of any one of the preceding claims, wherein the method introduces substantially no stabilizer into the blend.

22. A vulcanizable rubber composition, comprising: (i) A polymer composition according to any one of the preceding claims; (ii) fillers; and (iii) Curing agent.

23. A vulcanizate prepared by vulcanizing a vulcanizable composition according to any one of the preceding claims.