Rubber composition and crosslinked rubber product
By using a rubber composition containing ring-opening copolymers of cyclooctadiene and norbornene compounds and inorganic materials, the problems of insufficient resistance to damage and cracking of existing rubber crosslinks have been solved, resulting in a high-strength and high-durability rubber crosslink suitable for applications such as tires and shock-absorbing rubber.
Patent Information
- Application Number
- CN202380028679.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-05
AI Technical Summary
In existing technologies, the resistance to damage and cracking of rubber crosslinks is insufficient, making it difficult to meet the requirements of applications such as tires.
A rubber composition comprising inorganic materials and ring-opening copolymers, the ring-opening copolymers being composed of cyclooctadiene and norbornene compounds, is copolymerized using a Ziegler-Natta catalyst to form a rubber crosslinker with excellent resistance to damage and cracking.
It achieves high tensile strength, tear strength, and excellent resistance to damage and cracking in rubber crosslinks, making it suitable for applications such as tires, belts, and shock-absorbing rubber.
Smart Images

Figure BDA0005049834170000021 
Figure BDA0005049834170000031 
Figure BDA0005049834170000271
Abstract
Description
Technical Field
[0001] The present invention relates to a rubber composition and a rubber cross-linked product capable of forming a rubber cross-linked product having excellent fracture resistance and chipping resistance. Background Art
[0002] Generally, cyclopentene and norbornene compounds are known to be 6、 The metathesis ring-opening polymerization is carried out in the presence of a so-called Ziegler-Natta catalyst composed of a transition metal compound of Group 6 of the periodic table such as MoCl5 and an organic metal activator such as triisobutylaluminum, diethylaluminum chloride, and tetrabutyltin, thereby forming an unsaturated linear ring-opening copolymer. In addition, a method for improving the affinity of a polymer for inorganic particles by introducing a functional group containing a heteroatom at the end of a polymer chain is known.
[0003] For example, Patent Document 1 discloses a composition for a material having a damage resistance property, which comprises an inorganic material and a ring-opening copolymer, wherein the ring-opening copolymer comprises a structural unit derived from a monocyclic cyclic olefin and a structural unit derived from a norbornene compound. According to the technology of Patent Document 1, a rubber cross-linked product having excellent damage resistance and chipping resistance and suitable for use in tire applications, etc., can be provided. However, a rubber cross-linked product having even better damage resistance and chipping resistance is required.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: Japanese Patent Application Publication No. 2020-15832. Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a rubber composition capable of providing a rubber cross-linked product having excellent fracture resistance and chipping resistance, and a rubber cross-linked product obtained by cross-linking such a rubber composition.
[0009] Solutions for solving problems
[0010] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that a rubber cross-linked product obtained by using a rubber composition comprising an inorganic material and a ring-opening copolymer, wherein the ring-opening copolymer comprises a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound, exhibits excellent fracture resistance and chipping resistance, thereby completing the present invention.
[0011] That is, according to the present invention, there is provided a rubber composition comprising an inorganic material and a ring-opening copolymer comprising a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound.
[0012] The inorganic material is preferably a carbon material or silicon dioxide.
[0013] The norbornene compound is preferably a norbornene compound represented by the following general formula (1).
[0014] [Chemical formula 1]
[0015]
[0016] (Where R 1 ~R 4 represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom, and R 2 and R 3 can bond to each other to form a ring structure, and m is 0 or 1).
[0017] Preferably, the above R 1 ~R 4 It is a hydrogen atom, a chain hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom.
[0018] The weight average molecular weight of the ring-opening polymer is preferably 50,000 to 1,000,000.
[0019] The glass transition temperature of the ring-opening polymer is preferably -80 to 10°C.
[0020] The rubber composition of the present invention may further contain a rubber other than the above-mentioned ring-opening copolymer.
[0021] Furthermore, according to the present invention, there is provided a cross-linked rubber obtained by cross-linking the rubber composition.
[0022] Effects of the Invention
[0023] According to the present invention, there can be provided a rubber composition capable of forming a rubber cross-linked product having excellent fracture resistance and chipping resistance, and a rubber cross-linked product obtained by cross-linking such a rubber composition. DETAILED DESCRIPTION
[0024] <Rubber composition>
[0025] The rubber composition of the present invention comprises an inorganic material and a ring-opening copolymer, wherein the ring-opening copolymer comprises a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound. The rubber composition is a composition capable of obtaining a rubber cross-linked product having excellent fracture resistance, preferably a composition capable of forming a rubber cross-linked product having a tensile strength and a tear strength within the preferred numerical range described below.
[0026] The ring-opening copolymer contained in the rubber composition of the present invention contains a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound.
[0027] Examples of the cyclooctadiene in the present invention include 1,3-cyclooctadiene, 1,4-cyclooctadiene, and 1,5-cyclooctadiene, and 1,5-cyclooctadiene is particularly preferred.
[0028] The norbornene compound in the present invention is a compound having a norbornene ring structure, and is preferably a norbornene compound represented by the following general formula (1).
[0029] [Chemical formula 2]
[0030]
[0031] In the formula, R 1 ~R 4 represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom, and R 2 and R 3 They can bond to each other to form a ring structure, and m is 0 or 1.
[0032] Specific examples of the norbornene compound represented by the general formula (1) include the following compounds.
[0033] 2-norbornene, 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-hexyl-2-norbornene, 5-decyl-2-norbornene, 5-cyclohexyl-2-norbornene, 5-cyclopentyl-2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene, 5-propenyl-2-norbornene, 5-cyclohexenyl-2-norbornene, 5-cyclopentenyl-2-norbornene, 5-phenyl-2-norbornene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene (also known as 1,4-methylene-1,4,4a,9a-tetrahydro-9H-fluorene), tetracyclo[10.2.1.0 2,11 .0 4,9]pentadeca-4,6,8,13-tetraene (also known as 1,4-methylene-1,4,4a,9,9a,10-hexahydroanthracene), dicyclopentadiene, methyldicyclopentadiene, and dihydrodicyclopentadiene (tricyclo[5.2.1.0 2,6 ] dec-8-ene) and other unsubstituted or hydrocarbon-substituted bicyclo[2.2.1]hept-2-enes;
[0034] Four rings [6.2.1.1 3,6 .0 2,7 ]Dodec-4-ene, 9-methyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-ethyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclohexyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclopentyltetracyclo[6.2.1.1 3,6 .0 2,7 ]Dodec-4-ene, 9-methylenetetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-ethylenetetracyclo[6.2.1.1 3,6 .0 2,7 ]Dodec-4-ene, 9-vinyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-propenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclohexenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclopentenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, and 9-phenyltetracyclo[6.2.1.1 3,6 .0 2 ,7 ] unsubstituted or hydrocarbon-substituted tetracyclic rings such as dodec-4-ene [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;
[0035] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group, such as methyl 5-norbornene-2-carboxylate, ethyl 5-norbornene-2-carboxylate, methyl 2-methyl-5-norbornene-2-carboxylate, and ethyl 2-methyl-5-norbornene-2-carboxylate;
[0036] Four rings [6.2.1.13,6 .0 2,7 ] methyl dodec-9-ene-4-carboxylate and 4-methyltetracyclo[6.2.1.1 3,6 .0 2 ,7 ] tetracyclic [6.2.1.1] having an alkoxycarbonyl group, such as methyl dodec-9-ene-4-carboxylate 3,6 .0 2,7 ] Dodeca-4-enes;
[0037] Bicyclo[2.2.1]hept-2-enes having a hydroxycarbonyl group or anhydride group, such as 5-norbornene-2-carboxylic acid, 5-norbornene-2,3-dicarboxylic acid, and 5-norbornene-2,3-dicarboxylic anhydride;
[0038] Four rings [6.2.1.1 3,6 .0 2,7 ]Dodec-9-ene-4-carboxylic acid, tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene-4,5-dicarboxylic acid and tetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having a hydroxycarbonyl group or anhydride group such as dodec-9-ene-4,5-dicarboxylic anhydride 3,6 .0 2,7 ] Dodeca-4-enes;
[0039] Bicyclo[2.2.1]hept-2-enes having a hydroxyl group, such as 5-hydroxy-2-norbornene, 5-hydroxymethyl-2-norbornene, 5,6-bis(hydroxymethyl)-2-norbornene, 5,5-bis(hydroxymethyl)-2-norbornene, 5-(2-hydroxyethoxycarbonyl)-2-norbornene, and 5-methyl-5-(2-hydroxyethoxycarbonyl)-2-norbornene;
[0040] Four rings [6.2.1.1 3,6 .0 2,7 ] dodec-9-ene-4-methanol and tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodeca-9-en-4-ol and other tetracyclic rings having a hydroxyl group [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;
[0041] Bicyclo[2.2.1]hept-2-enes having a hydrogen carbonyl group such as 5-norbornene-2-carboxaldehyde;
[0042] Four rings [6.2.1.1 3,6 .0 2,7] dodec-9-ene-4-carboxaldehyde and other tetracyclic [6.2.1.1 3,6 .0 2 ,7 ] Dodeca-4-enes;
[0043] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group and a hydroxycarbonyl group, such as 3-methoxycarbonyl-5-norbornene-2-carboxylic acid;
[0044] Bicyclo[2.2.1]hept-2-enes having a carbonyloxy group, such as 5-norbornene-2-yl acetate, 2-methyl-5-norbornene-2-yl acetate, 5-norbornene-2-yl acrylate, and 5-norbornene-2-yl methacrylate;
[0045] Acetic acid-9-tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-enyl ester, acrylic acid-9-tetracyclo[6.2.1.1 3,6 .0 2 ,7 ] dodec-4-enyl ester, and 9-tetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having a carbonyl group such as dodec-4-enyl ester 3,6 .0 2,7 ] Dodeca-4-enes;
[0046] Bicyclo[2.2.1]hept-2-enes having a functional group containing a nitrogen atom, such as 5-norbornene-2-carbonitrile, 5-norbornene-2-carboxamide, and 5-norbornene-2,3-dicarboximide;
[0047] Four rings [6.2.1.1 3,6 .0 2,7 ]Dodec-9-ene-4-carbonitrile, tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene-4-carboxamide, and tetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having a functional group containing a nitrogen atom such as dodec-9-ene-4,5-dicarboximide 3,6 .0 2,7 ] Dodeca-4-enes;
[0048] Bicyclo[2.2.1]hept-2-enes having a halogen atom such as 5-chloro-2-norbornene;
[0049] 9-Chlorotetracyclic [6.2.1.1 3,6 .02,7 ] tetracyclic rings having halogen atoms such as dodec-4-ene [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;
[0050] Bicyclo[2.2.1]hept-2-enes having a functional group containing a silicon atom, such as 5-trimethoxy-2-norbornene and 5-triethoxy-2-norbornene;
[0051] 4-Trimethoxysilyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene, 4-triethoxysilyltetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic rings having a functional group containing a silicon atom such as dodec-9-ene [6.2.1.1 3,6 .0 2,7 ]Dodec-4-enes.
[0052] As the norbornene compound represented by the general formula (1), a compound represented by the general formula (1) wherein m is 0 is preferred. In the general formula (1), R 1 ~R 4 Can be the same or different.
[0053] Among the norbornene compounds represented by the general formula (1), R in the general formula (1) is particularly preferred from the viewpoint of being able to form a rubber cross-linked product exhibiting more excellent fracture resistance and chipping resistance. 1 ~R 4 is a hydrogen atom, a chain hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom. In this case, R 1 ~R 4 There is no particular limitation as long as the groups are not mutually bonded and do not form a ring, and they may be the same or different. 1 ~R 4 , preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. In this case, the compound represented by the general formula wherein m is 0 is preferred.
[0054] As R in the above general formula (1) 1 ~R 4 Specific examples of norbornene compounds which are substituents containing a hydrogen atom, a chain hydrocarbon group having 1 to 20 carbon atoms, or a halogen atom, a silicon atom, an oxygen atom, or a nitrogen atom include the following compounds:
[0055] Bicyclo[2.2.1]hept-2-enes which are unsubstituted or have a chain hydrocarbon substituent, such as 2-norbornene, 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-hexyl-2-norbornene, 5-decyl-2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene and 5-propenyl-2-norbornene;
[0056] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group, such as methyl 5-norbornene-2-carboxylate, ethyl 5-norbornene-2-carboxylate, methyl 2-methyl-5-norbornene-2-carboxylate, and ethyl 2-methyl-5-norbornene-2-carboxylate;
[0057] Bicyclo[2.2.1]hept-2-enes having a hydroxycarbonyl group, such as 5-norbornene-2-carboxylic acid and 5-norbornene-2,3-dicarboxylic acid;
[0058] Bicyclo[2.2.1]hept-2-enes having a hydroxyl group, such as 5-hydroxy-2-norbornene, 5-hydroxymethyl-2-norbornene, 5,6-bis(hydroxymethyl)-2-norbornene, 5,5-bis(hydroxymethyl)-2-norbornene, 5-(2-hydroxyethoxycarbonyl)-2-norbornene, and 5-methyl-5-(2-hydroxyethoxycarbonyl)-2-norbornene;
[0059] Bicyclo[2.2.1]hept-2-enes having a hydrogen carbonyl group such as 5-norbornene-2-carboxaldehyde;
[0060] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group and a hydroxycarbonyl group, such as 3-methoxycarbonyl-5-norbornene-2-carboxylic acid;
[0061] Bicyclo[2.2.1]hept-2-enes having a carbonyloxy group, such as 5-norbornene-2-yl acetate, 2-methyl-5-norbornene-2-yl acetate, 5-norbornene-2-yl acrylate, and 5-norbornene-2-yl methacrylate;
[0062] Bicyclo[2.2.1]hept-2-enes having a functional group containing a nitrogen atom, such as 5-norbornene-2-carbonitrile and 5-norbornene-2-carboxamide;
[0063] Bicyclo[2.2.1]hept-2-enes having a halogen atom such as 5-chloro-2-norbornene;
[0064] Bicyclo[2.2.1]hept-2-enes having a functional group containing a silicon atom, such as 5-trimethoxy-2-norbornene and 5-triethoxy-2-norbornene;
[0065] As R in the above general formula (1)1 ~R 4 The norbornene compound is a hydrogen atom, a chain hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom, preferably a bicyclo[2.2.1]hept-2-ene which is unsubstituted or has a hydrocarbon substituent, and more preferably 2-norbornene, 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-ethylidene-2-norbornene, and 5-vinyl-2-norbornene. From the viewpoint of more easily obtaining the effects of the present invention, 2-norbornene, 5-methyl-2-norbornene, and 5-ethyl-2-norbornene are further preferred.
[0066] In addition, when using R 2 and R 3 In the case of the norbornene compound represented by the general formula (1) above, as specific examples of the ring structure, preferably cyclopentane ring, cyclopentene ring, cyclohexane ring, cyclohexene ring, benzene ring, etc. can form a polycyclic structure and can also have a substituent. Among these, cyclopentane ring, cyclopentene ring, benzene ring are particularly preferred, and compounds having a cyclopentene ring alone or a polycyclic structure having a cyclopentane ring and a benzene ring are particularly preferred. In addition, in addition to R forming the ring structure 2 , R 3 In addition, R 1 , R 4 They may be the same or different, and are preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. In this case, compounds represented by the general formula wherein m is 0 are also preferred.
[0067] As R 2 and R 3 The compounds that are bonded to each other to form a ring are preferably unsubstituted or hydrocarbon-substituted bicyclo[2.2.1]hept-2-enes, particularly preferably dicyclopentadiene, methyldicyclopentadiene, dihydrodicyclopentadiene, 1,4-methylene-1,4,4a,9a-tetrahydro-9H-fluorene, and 1,4-methylene-1,4,4a,9,9a,10-hexahydroanthracene, and more preferably dicyclopentadiene and 1,4-methylene-1,4,4a,9a-tetrahydro-9H-fluorene.
[0068] The norbornene compound in the present invention may be used alone or in combination of two or more.
[0069] The content ratio of the structural unit derived from cyclooctadiene in the ring-opening copolymer contained in the rubber composition of the present invention relative to the total repeating structural units is preferably 10 to 75% by weight, more preferably 20 to 65% by weight, further preferably 30 to 55% by weight, and particularly preferably 35 to 50% by weight. If the content ratio of the structural unit derived from cyclooctadiene is within the above range, a rubber cross-linked product showing more excellent fracture resistance and chipping resistance can be formed.
[0070] The content ratio of the structural unit derived from the norbornene compound in the ring-opening copolymer contained in the rubber composition of the present invention relative to the total repeating structural units is preferably 25 to 90% by weight, more preferably 35 to 80% by weight, further preferably 45 to 70% by weight, and particularly preferably 50 to 65% by weight. If the content ratio of the structural unit derived from the norbornene compound is within the above range, a rubber cross-linked product showing more excellent fracture resistance and chipping resistance can be formed.
[0071] In addition, the ring-opening copolymer in the present invention can be a ring-opening copolymer obtained by copolymerizing cyclooctadiene and norbornene compounds, and other monomers copolymerizable with them. As such other monomers, monocyclic cyclic olefins other than cyclooctadiene and polycyclic cyclic olefins having aromatic rings can be exemplified. As monocyclic cyclic olefins other than cyclooctadiene, there is no particular limitation as long as it is an olefin having only one cyclic structure, and examples thereof include cyclic monoolefins such as cyclopropene, cyclobutene, cyclopentene, methylcyclopentene, cyclohexene, methylcyclohexene, cycloheptene, and cyclooctene; cyclic dienes such as cyclohexadiene, methylcyclohexadiene, and methylcyclooctadiene, etc. As polycyclic cyclic olefins having aromatic rings, phenylcyclooctene, 5-phenyl-1,5-cyclooctadiene, and phenylcyclopentene can be cited. The content ratio of the structural units derived from other monomers in the ring-opening copolymer of the present invention relative to all repeating structural units is preferably 40% by weight or less, more preferably 30% by weight or less. The ring-opening copolymer of the present invention is particularly preferably a ring-opening copolymer that substantially contains no structural units derived from other monomers.
[0072] The weight average molecular weight (Mw) of the ring-opening copolymer in the present invention is preferably 50,000 to 1,000,000, more preferably 50,000 to 700,000, further preferably 100,000 to 5,000,000, and particularly preferably 150,000 to 300,000, as a value of the weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography. By setting the weight average molecular weight (Mw) to the above range, it is possible to achieve good production and handling, and the obtained cross-linked rubber can exhibit more excellent damage resistance and chipping resistance. When the weight average molecular weight is too low, especially when the weight average molecular weight is 50,000 or less, the damage resistance and chipping resistance of the obtained cross-linked rubber deteriorate. When the weight average molecular weight is too high, especially when the weight average molecular weight is 1,000,000 or more, the processability of the obtained cross-linked rubber is poor, and production and handling become difficult. The ratio (Mw / Mn) of the polystyrene-equivalent weight average molecular weight (Mw) to the number average molecular weight (Mn) of the ring-opening copolymer in the present invention measured by gel permeation chromatography is preferably 1.0 to 5.0, more preferably 1.5 to 3.0.
[0073] The cis / trans ratio of the ring-opening copolymer in the present invention is preferably 95 / 5 to 5 / 95, more preferably 90 / 10 to 10 / 90, further preferably 85 / 15 to 15 / 85, and particularly preferably 60 / 40 to 20 / 80. The above cis / trans ratio refers to the content ratio (cis / trans ratio) of the cis structure and the trans structure of the double bond present in the repeating unit constituting the ring-opening copolymer in the present invention. By making the cis / trans ratio within the above range, the rubber cross-linked product of the present invention obtained using the ring-opening copolymer can show more excellent damage resistance and chipping resistance. In the case where the cis ratio is too high, as described later, the rubber composition containing a carbon material as an inorganic material can form a rubber cross-linked product having excellent wear resistance in addition to damage resistance and chipping resistance, but sometimes has poor handling stability.
[0074] The glass transition temperature (Tg) of the ring-opening copolymer in the present invention is preferably -80 to 10°C, more preferably -65 to -10°C, and further preferably -50 to -10°C. By setting the glass transition temperature (Tg) to the above range, the rubber cross-linked product of the present invention obtained by using the ring-opening copolymer can show more excellent damage resistance and chipping resistance. When the glass transition temperature is too low, the characteristics such as damage resistance and chipping resistance may be lost. When the glass transition temperature is too high, the processability may be greatly deteriorated and the characteristics such as elongation may be lost. In addition, the glass transition temperature of the ring-opening copolymer can be controlled by, for example, adjusting the type and amount of the norbornene compound used.
[0075] In addition, the ring-opening copolymer in the present invention may have a modified group at the polymer chain terminal. The ring-opening copolymer in the present invention may further improve its affinity for inorganic materials by having such a terminal modified group, thereby sometimes improving the dispersibility of the inorganic material in the rubber cross-linked product when the inorganic material is added, and as a result, sometimes further improving the damage resistance and crack resistance when the rubber cross-linked product is made. The modified group introduced into the polymer chain terminal is not particularly limited, but preferably contains an atom selected from the group consisting of atoms of the 15th group of the periodic table, atoms of the 16th group of the periodic table, and silicon atoms.
[0076] As the modifying group for forming the terminal modifying group, from the viewpoint of being able to improve the affinity for inorganic materials and thereby being able to further improve the fracture resistance and chipping resistance when the rubber cross-linked product is prepared, a modifying group containing an atom selected from the group consisting of a nitrogen atom, an oxygen atom, a phosphorus atom, a sulfur atom and a silicon atom is more preferred, and a modifying group containing an atom selected from the group consisting of a nitrogen atom, an oxygen atom and a silicon atom is particularly preferred.
[0077] As the modified group containing nitrogen atoms, amino, pyridyl, imino, amide, nitro, carbamate bond or hydrocarbon groups containing any of these groups can be exemplified. As the modified group containing oxygen atoms, hydroxyl, carboxylic acid, ether, ester, carbonyl, aldehyde, epoxy or hydrocarbon groups containing any of these groups can be exemplified. As the modified group containing silicon atoms, alkylsilyl, oxysilyl or hydrocarbon groups containing any of these groups can be exemplified. As the modified group containing phosphorus atoms, phosphate, phosphine or hydrocarbon groups containing any of these groups can be exemplified. As the modified group containing sulfur atoms, sulfonyl, mercapto, thioether or hydrocarbon groups containing any of these groups can be exemplified. In addition, as the modified group, it can also be a modified group containing a plurality of the above groups. Among these, from the viewpoint of further improving the damage resistance and chipping resistance when preparing a cross-linked rubber, specific examples of particularly preferred modifying groups include amino, pyridyl, imino, amide, hydroxyl, carboxylic acid, aldehyde, epoxy, oxysilyl, or a hydrocarbon group containing any of these groups, and from the viewpoint of affinity for silica, oxysilyl is particularly preferred. In addition, oxysilyl refers to a group having a silicon-oxygen bond.
[0078] As specific examples of oxysilyl groups, alkoxysilyl groups, aryloxysilyl groups, acyloxysilyl groups, alkylsiloxysilyl groups, or arylsiloxysilyl groups can be cited. In addition, hydroxysilyl groups formed by hydrolyzing alkoxysilyl groups, aryloxysilyl groups, or acyloxysilyl groups can be cited. Among these, alkoxysilyl groups are preferred from the viewpoint of affinity to inorganic materials.
[0079] The alkoxysilyl group is a group in which one or more alkoxy groups are bonded to a silicon atom. Specific examples thereof include trimethoxysilyl, (dimethoxy)(methyl)silyl, (methoxy)(dimethyl)silyl, (methoxy)(dichloro)silyl, triethoxysilyl, (diethoxy)(methyl)silyl, (ethoxy)(dimethyl)silyl, (dimethoxy)(ethoxy)silyl, (methoxy)(diethoxy)silyl, tripropoxysilyl, and tris(trimethylsiloxy)silyl.
[0080] The introduction ratio of the modified group in the polymer chain terminal of the ring-opening copolymer is not particularly limited, and is preferably 10% or more, more preferably 20% or more, further preferably 30% or more, and particularly preferably 40% or more, in terms of the percentage of the number of ring-opening copolymer chain terminals into which the modified group is introduced / the total number of ring-opening copolymer chain terminals. The higher the introduction ratio of the terminal modified group, the higher the affinity with the inorganic material, and thus the more excellent the low heat generation property, which is preferred. In addition, there is no particular limitation on the method for determining the introduction ratio of the modified group introduced into the polymer chain terminal. When exemplifying the case of introducing an oxysilyl group as the terminal modified group, it can be determined according to the method described by 1 The molecular weight was determined by using the peak area ratio corresponding to the oxysilyl group determined by H-NMR spectroscopy and the number average molecular weight determined by gel permeation chromatography.
[0081] The Mooney viscosity (ML1+4100°C) of the ring-opening copolymer in the present invention is preferably 20 to 150, more preferably 22 to 120, and even more preferably 25 to 90. When the Mooney viscosity is within the above range, kneading at room temperature and high temperature can be facilitated, thereby improving processability.
[0082] The method for producing the ring-opening copolymer in the present invention is not particularly limited, and examples thereof include a method of copolymerizing cyclooctadiene and a norbornene compound in the presence of a ring-opening polymerization catalyst.
[0083] The ring-opening polymerization catalyst may be any catalyst capable of ring-opening copolymerization of cyclooctadiene and a norbornene compound, and a ruthenium carbene complex or a so-called Ziegler-Natta catalyst is particularly preferred.
[0084] Specific examples of ruthenium carbene complexes include bis(tricyclohexylphosphine)benzylidene ruthenium dichloride, bis(triphenylphosphine)-3,3-diphenylpropenylene ruthenium dichloride, bis(tricyclohexylphosphine)tert-butylvinylene ruthenium dichloride, dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium, bis(1,3-diisopropylimidazolin-2-ylidene)benzylidene ruthenium dichloride, bis(1,3-dicyclohexylphosphine)tert-butylvinylene ruthenium dichloride, dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium, (1,3-di-mesitylene imidazolin-2-ylidene)(tricyclohexylphosphine)benzylidene ruthenium dichloride, (1,3-di-mesitylene imidazolin-2-ylidene)(tricyclohexylphosphine)benzylidene ruthenium dichloride, (1,3-di-mesitylene imidazolidin-2-ylidene)(tricyclohexylphosphine)benzylidene ruthenium dichloride, bis(tricyclohexylphosphine)ethoxymethylene ruthenium dichloride, (1,3-di-mesitylene imidazolidin-2-ylidene)(tricyclohexylphosphine)ethoxymethylene ruthenium dichloride.
[0085] Ziegler-Natta catalysts are mixed catalysts of transition metal compounds of Group 6 of the periodic table and organoaluminum compounds. Specific examples of transition metal compounds of Group 6 of the periodic table include molybdenum compounds such as molybdenum pentachloride, molybdenum oxytetrachloride, (phenylimide) molybdenum tetrachloride, tri-dodecylammonium molybdate, methyltrioctylammonium molybdate, tridecylammonium molybdate, trioctylammonium molybdate, and tetraphenylammonium molybdate; and tungsten compounds such as tungsten hexachloride, tungsten tetrachloride, (phenylimide) tungsten tetrachloride, mono(catechol) tungsten tetrachloride, bis(3,5-di-tert-butyl)catechol dichloride, bis(2-chloroethyl ether) tungsten tetrachloride, and tetraphenoxy tungsten oxide.
[0086] Specific examples of the organoaluminum compound contained in the Ziegler-Natta catalyst include: diethylaluminum ethoxide, diethylaluminum isopropoxide, diisobutylaluminum butoxide, diisobutylaluminum hexoxide, (2-trichloroethoxy)diethylaluminum, (2-tribromoethoxy)diethylaluminum, (1,3-dichloro-2-propoxy)diethylaluminum, (1,1,1,3,3,3-hexafluoro-2-propoxy)diethylaluminum, (1,1,1-trichloro-2-methyl-2-propoxy)diethylaluminum, (2,6-diisopropylphenoxy)diethylaluminum, di(2-trichloroethoxy)ethylaluminum, di(2-tribromoethoxy)ethylaluminum, di(1,3-dichloro-2-propoxy)ethylaluminum, di (1,1,1,3,3,3-hexafluoro-2-propoxy)ethylaluminum, di(1,1,1-trichloro-2-methyl-2-propoxy)ethylaluminum, bis(2,6-diisopropylphenoxy)ethylaluminum, ethoxyethyl(chloro)aluminum, isopropoxyethyl(chloro)aluminum, butoxyethyl(chloro)aluminum, (2-trichloroethoxy)ethyl(chloro)aluminum, (2-tribromoethoxy)ethyl(chloro)aluminum, (1,3-dichloro-2-propoxy)ethyl(bromo)aluminum, (1,1,1,3,3,3-hexafluoro-2-propoxy)ethyl(chloro)aluminum, (1,1,1-trichloro-2-methyl-2-propoxy)ethyl(chloro)aluminum, (2,6-diisopropylphenoxy)ethyl(chloro)aluminum, and the like.
[0087] The ring-opening polymerization catalyst may be used alone or in combination of two or more.
[0088] The amount of the ring-opening polymerization catalyst used is generally in the range of 1:500 to 1:2,000,000, preferably 1:700 to 1:1,500,000, more preferably 1:1,000 to 1:1,000,000 in terms of molar ratio of (ring-opening polymerization catalyst:monomer used in copolymerization).
[0089] The polymerization reaction can be carried out in the absence of a solvent or in a solution. In the case of copolymerization in a solution, the solvent used is not particularly limited as long as it is inactive in the polymerization reaction and can dissolve the cyclooctadiene, norbornene compound, polymerization catalyst, etc. used in the copolymerization. It is preferred to use a hydrocarbon solvent or a halogen solvent. As a hydrocarbon solvent, for example: aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene; aliphatic hydrocarbons such as hexane, n-heptane, n-octane; alicyclic hydrocarbons such as cyclohexane, cyclopentane, methylcyclohexane, etc. In addition, as a halogen solvent, for example: halogenated alkanes such as dichloromethane and chloroform; aromatic halides such as chlorobenzene and dichlorobenzene, etc. These solvents can be used alone or in combination of two or more.
[0090] When cyclooctadiene and a norbornene compound are subjected to ring-opening copolymerization, an olefin compound or a diene compound may be added as a molecular weight regulator in the polymerization reaction system in order to adjust the molecular weight of the obtained ring-opening copolymer as necessary.
[0091] The olefin compound is not particularly limited as long as it is an organic compound having an olefinic unsaturated bond, and examples thereof include: α-olefins such as 1-butene, 1-pentene, 1-hexene, and 1-octene; styrenes such as styrene and vinyltoluene; halogen-containing vinyl compounds such as allyl chloride; vinyl ethers such as ethyl vinyl ether and isobutyl vinyl ether; amine-containing vinyl compounds such as allylamine, N,N-dimethylallylamine, and N,N-diethylallylamine; disubstituted olefins such as 2-butene and 3-hexene, and the like.
[0092] Examples of the diene compound include non-conjugated dienes such as 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,6-heptadiene, 2-methyl-1,4-pentadiene, and 2,5-dimethyl-1,5-hexadiene.
[0093] The amount of the olefin compound and the diene compound used as the molecular weight modifier may be appropriately selected depending on the molecular weight of the ring-opening copolymer to be produced, and is generally in the range of 1 / 100 to 1 / 100000, preferably 1 / 200 to 1 / 50000, more preferably 1 / 500 to 1 / 10000 in terms of molar ratio relative to the monomers used in the copolymerization.
[0094] In addition, when the ring-opening copolymer of the present invention has a modified group at the polymer chain end, it is preferred to use an ethylenically unsaturated hydrocarbon compound containing a modified group as a molecular weight modifier instead of the above-mentioned olefin compound or diene compound. By using such an ethylenically unsaturated hydrocarbon compound containing a modified group, the modified group can be preferably introduced into the polymer chain end of the ring-opening copolymer obtained by copolymerization.
[0095] The modified group-containing ethylenically unsaturated hydrocarbon compound is not particularly limited as long as it has a modified group and one ethylenically unsaturated carbon-carbon double bond having metathesis reactivity. For example, when it is desired to introduce an oxysilyl group at the polymer chain end of a ring-opening copolymer, it is sufficient to allow the presence of an oxysilyl-containing ethylenically unsaturated hydrocarbon in the polymerization reaction system.
[0096] Examples of such oxysilyl-containing ethylenically unsaturated hydrocarbons include alkoxysilane compounds such as vinyl (trimethoxy) silane, vinyl (triethoxy) silane, allyl (trimethoxy) silane, allyl (methoxy) (dimethyl) silane, allyl (triethoxy) silane, allyl (ethoxy) (dimethyl) silane, styryl (trimethoxy) silane, styryl (triethoxy) silane, styryl ethyl (triethoxy) silane, allyl (triethoxysilyl methyl) ether, and allyl (triethoxysilyl methyl) (ethyl) amine; and vinyl Aryloxysilane compounds such as vinyl(triphenyloxy)silane, allyl(triphenyloxy)silane, allyl(phenoxy)(dimethyl)silane; acyloxysilane compounds such as vinyl(triacetoxy)silane, allyl(triacetoxy)silane, allyl(diacetoxy)methylsilane, allyl(acetoxy)(dimethyl)silane; alkylsiloxysilane compounds such as allyltri(trimethylsiloxy)silane; arylsiloxysilane compounds such as allyltri(triphenylsiloxy)silane; polysiloxane compounds such as 1-allylheptamethyltrisiloxane, 1-allylnonamethyltetrasiloxane, 1-allylnonamethylcyclopentasiloxane, 1-allylundecamethylcyclohexasiloxane, etc.
[0097] In addition, examples of the modified groups introduced into both ends (both ends) of the polymer chain of the ring-opening copolymer include alkoxysilane compounds such as bis(trimethoxysilyl)ethylene, bis(triethoxysilyl)ethylene, 2-butene-1,4-bis(trimethoxysilane), 2-butene-1,4-bis(triethoxysilane), 1,4-bis(trimethoxysilylmethoxy)-2-butene; 2-butene-1,4-bis(triphenoxysilane), etc. Aryloxysilane compounds; acyloxysilane compounds such as 2-butene-1,4-bis(triacetoxysilane); alkylsiloxysilane compounds such as 2-butene-1,4-bis[tri(trimethylsiloxy)silane]; arylsiloxysilane compounds such as 2-butene-1,4-bis[tri(triphenylsiloxy)silane]; polysiloxane compounds such as 2-butene-1,4-bis(heptamethyltrisiloxane) and 2-butene-1,4-bis(undecamethylcyclohexasiloxane), etc.
[0098] The ethylenically unsaturated hydrocarbon compound containing a modifying group, such as the ethylenically unsaturated hydrocarbon compound containing an oxygen-containing silyl group, not only plays a role in introducing a modifying group into the polymer chain terminal of the ring-opening copolymer, but also plays a role as a molecular weight regulator. Therefore, the amount of the ethylenically unsaturated hydrocarbon compound containing a modifying group can be appropriately selected according to the molecular weight of the ring-opening copolymer to be produced. The molar ratio relative to the monomer used in the copolymerization is usually 1 / 100 to 1 / 100000, preferably 1 / 200 to 1 / 50000, and more preferably 1 / 500 to 1 / 10000.
[0099] The polymerization reaction temperature is not particularly limited, but is preferably -100°C or higher, more preferably -50°C or higher, further preferably 0°C or higher, and particularly preferably 20°C or higher. In addition, the upper limit of the polymerization reaction temperature is not particularly limited, but is preferably less than 120°C, more preferably less than 100°C, further preferably less than 90°C, and particularly preferably less than 80°C. The polymerization reaction time is also not particularly limited, but is preferably 1 minute to 72 hours, and more preferably 10 minutes to 20 hours.
[0100] The ring-opening copolymer obtained by the polymerization reaction can be added with antioxidants such as phenol stabilizers, phosphorus stabilizers, and sulfur stabilizers as desired. The amount of antioxidant added can be appropriately determined according to its type, etc. Furthermore, extender oil can be added as needed. In the case of obtaining the ring-opening copolymer in the form of a polymerization solution, in order to recover the ring-opening copolymer from the polymerization solution, a known recovery method can be used, for example, the following method can be used: after separating the solvent by steam stripping, the solid is filtered and separated, and then dried to obtain a solid ring-opening copolymer; a method of directly devolatilizing the solvent by a biaxial heating dryer, etc. to obtain a solid ring-opening copolymer; after separating the solvent by reprecipitation with a poor solvent, the solid is filtered and separated, and then dried to obtain a solid ring-opening copolymer, etc.
[0101] In addition, the rubber composition of the present invention may also contain a rubber other than the above-mentioned ring-opening copolymer as a rubber component. In addition, the rubber component in the present invention refers to the above-mentioned ring-opening copolymer and a rubber other than the above-mentioned ring-opening copolymer. Examples of rubbers other than the above-mentioned ring-opening copolymer include natural rubber (NR), polyisoprene rubber (IR), emulsion-polymerized SBR (styrene-butadiene copolymer rubber), solution-polymerized random SBR (bonded styrene 5 to 50% by weight, 1,2-bond content of butadiene part 10 to 80%), high trans SBR (trans bond content of butadiene part 70 to 95%), low cis BR (polybutadiene rubber), high cis BR, high trans BR (trans bond content of butadiene part 70 to 95%). 95%), ethylene-propylene-diene rubber (EPDM), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, emulsion polymerization styrene-acrylonitrile-butadiene copolymer rubber, acrylonitrile-butadiene copolymer rubber, high vinyl SBR-low vinyl SBR block copolymer rubber, polyisoprene-SBR block copolymer rubber, polystyrene-polybutadiene-polystyrene block copolymer, acrylic rubber, epichlorohydrin rubber, fluororubber, silicone rubber, ethylene-propylene rubber, polyurethane rubber, etc. NR, BR, IR, EPDM, SBR are particularly preferred, and solution polymerization random SBR is particularly preferred. These silicas can be used alone or in combination of two or more.
[0102] The rubber other than the above-mentioned ring-opening copolymer in the present invention may have a modified group at the polymer terminal. In addition, as the modified group that can be present at the polymer terminal of the rubber other than the above-mentioned ring-opening copolymer, the same modified group as the modified group that can be present at the polymer terminal of the above-mentioned ring-opening copolymer can be cited, and the same modified group as the preferred modified group that can be present at the polymer terminal of the above-mentioned ring-opening copolymer is preferred.
[0103] The rubber composition of the present invention contains an inorganic material that functions as a filler. As the inorganic material contained in the rubber composition of the present invention, a carbon material or silica is preferred. As the carbon material, carbon black is preferred. The rubber composition containing a carbon material as an inorganic material can form a rubber cross-linked product that is not only excellent in damage resistance and crack resistance, but also excellent in wear resistance and handling stability. In addition, the rubber composition containing silica as an inorganic material can form a rubber cross-linked product that is not only excellent in damage resistance and crack resistance, but also excellent in wet grip and low heat generation.
[0104] Examples of carbon black used as an inorganic material contained in the rubber composition of the present invention include furnace black, acetylene black, thermal black, channel black, graphite, etc. Among them, furnace black is preferred, and specific examples thereof include SAF, ISAF, ISAF-HS, ISAF-LS, IISAF-HS, HAF, HAF-HS, HAF-LS, FEF, etc. These carbon blacks can be used alone or in combination of two or more.
[0105] The nitrogen adsorption specific surface area (N2SA) of carbon black is preferably 5 to 200 m 2 / g, more preferably 70 to 120 m 2 / g, and the adsorption amount of dibutyl phthalate (DBP) is preferably 5 to 300 ml / 100 g, more preferably 80 to 160 ml / 100 g.
[0106] As the silica used as the inorganic material contained in the rubber composition of the present invention, for example, dry-process silica, wet-process silica, colloidal silica, and precipitated silica disclosed in Japanese Patent Publication No. 62-62838 can be cited. Among these, wet-process silica with hydrous silicic acid as the main component is preferred. In addition, a carbon-silica dual-phase filler in which silica is supported on the surface of carbon black can also be used. These silicas can be used alone or in combination of two or more.
[0107] The nitrogen adsorption specific surface area of silicon dioxide (measured by the BET method according to ASTM D3037-81) is preferably 50 to 400 m 2 / g, more preferably 100 to 220 m 2 / g. In addition, the pH of silica is preferably less than pH 7, and more preferably pH 5 to 6.9. When it is within this range, the affinity between the ring-opening copolymer and silica is particularly good.
[0108] When silica is used as an inorganic material, it is preferred to further add a silane coupling agent to the rubber composition of the present invention in order to further improve the affinity between the ring-opening copolymer and silica. As the silane coupling agent, for example, vinyl triethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl trimethoxysilane, bis(3-(triethoxysilyl)propyl)tetrasulfide, bis(3-(triethoxysilyl)propyl)disulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyl tetrasulfide, γ-trimethoxysilylpropylbenzothiazolyl tetrasulfide and other tetrasulfides described in Japanese Patent Laid-Open No. 6-248116 can be cited. Tetrasulfides are particularly preferred. These silane coupling agents can be used alone or in combination of two or more. The amount of the silane coupling agent added is preferably 0.1 to 30 parts by weight, more preferably 1 to 15 parts by weight, based on 100 parts by weight of the inorganic material.
[0109] The content of the inorganic material in the present invention is preferably 10 to 150 parts by weight, more preferably 20 to 120 parts by weight, further preferably 40 to 100 parts by weight, and particularly preferably 40 to 60 parts by weight, based on 100 parts by weight of the rubber material.
[0110] In addition to the above-mentioned ingredients, the rubber composition of the present invention may further contain required amounts of crosslinking agents, crosslinking accelerators, crosslinking activators, fillers other than inorganic materials, antioxidants, activators, processing oils, plasticizers, flow aids and other additives according to conventional methods.
[0111] As the crosslinking agent, sulfur such as powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur can be cited; sulfur halides such as sulfur monochloride and sulfur dichloride; organic peroxides such as diisopropylbenzene peroxide and di-tert-butyl peroxide; quinone dioximes such as p-quinone dioxime and p,p′-dibenzoylquinone dioxime; organic polyamine compounds such as triethylenetetramine, hexamethylenediamine carbamate, and 4,4′-methylenebis(o-chloroaniline); alkylphenol-formaldehyde resins having hydroxymethyl groups, etc. Among these, sulfur is preferred, and powdered sulfur is more preferred. These crosslinking agents can be used alone or in combination of two or more. The amount of the crosslinking agent added is preferably 0.1 to 15 parts by weight, and more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition.
[0112] Examples of the crosslinking accelerator include: sulfonamide-based crosslinking accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N′-diisopropyl-2-benzothiazole sulfenamide; guanidine-based crosslinking accelerators such as 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, and 1-o-tolylbiguanide; diethyl Thiourea crosslinking accelerators such as thiourea; thiazole crosslinking accelerators such as 2-mercaptobenzothiazole, dibenzothiazole disulfide, and 2-mercaptobenzothiazole zinc salt; thiuram crosslinking accelerators such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide; dithiocarbamic acid crosslinking accelerators such as sodium dimethyldithiocarbamate and zinc diethyldithiocarbamate; xanthogenic acid crosslinking accelerators such as sodium isopropyl xanthogenate, zinc isopropyl xanthogenate, and zinc butyl xanthogenate. It is particularly preferred to include a sulfonamide crosslinking accelerator, and it is particularly preferred to include N-tert-butyl-2-benzothiazole sulfonamide. These crosslinking accelerators can be used alone or in combination of two or more. The amount of the crosslinking accelerator added is preferably 0.1 to 15 parts by weight, and more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition.
[0113] As the crosslinking activator, for example, higher fatty acids such as stearic acid, zinc oxide, etc. can be used. The amount of the crosslinking activator added can be appropriately selected, but the amount of the higher fatty acid added is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition, and the amount of zinc oxide added is preferably 0.05 to 10 parts by weight, more preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition.
[0114] As the processing oil, mineral oil and synthetic oil can be used. Mineral oil can generally be aromatic oil, naphthenic oil, paraffin oil, etc. As other additives, there can be mentioned: activators such as diethylene glycol, polyethylene glycol, silicone oil; fillers other than inorganic materials such as calcium carbonate, talc, clay; tackifiers such as petroleum resin, coumarone resin; wax, etc.
[0115] The rubber composition of the present invention can be obtained by kneading the components according to a conventional method. For example, after kneading the additives other than the crosslinking agent and the crosslinking accelerator with the rubber components such as the ring-opening copolymer, the rubber composition can be obtained by mixing the crosslinking agent and the crosslinking accelerator in the kneaded product. The kneading temperature of the additives other than the crosslinking agent and the crosslinking accelerator with the rubber components such as the ring-opening copolymer is preferably 20 to 200° C., more preferably 30 to 180° C., and the kneading time is preferably 30 seconds to 30 minutes. The mixing of the crosslinking agent and the crosslinking accelerator is usually carried out below 100° C., preferably below 80° C.
[0116] <Rubber cross-linked product>
[0117] The cross-linked rubber of the present invention is obtained by cross-linking the rubber composition of the present invention described above.
[0118] The rubber cross-linked product of the present invention can be manufactured as follows: using the rubber composition of the present invention, using a molding machine corresponding to the desired shape, such as an extruder, an injection molding machine, a compressor, a roller, etc., for molding, and performing a cross-linking reaction by heating to fix the shape to make a cross-linked product. In this case, cross-linking can be performed after pre-molding, or cross-linking can be performed while molding. The molding temperature is usually 10 to 200°C, preferably 25 to 120°C. The cross-linking temperature is usually 100 to 200°C, preferably 130 to 190°C, and the cross-linking time is usually 1 minute to 24 hours, preferably 2 minutes to 12 hours, and particularly preferably 3 minutes to 6 hours.
[0119] Furthermore, depending on the shape and size of the cross-linked rubber, even if the surface is cross-linked, the interior may not be sufficiently cross-linked. Therefore, further heating may be performed to perform secondary cross-linking.
[0120] As the heating method, any method generally used for crosslinking of rubber, such as press heating, steam heating, oven heating, and hot air heating, may be appropriately selected.
[0121] The cross-linked rubber of the present invention thus obtained has high tensile strength and tear strength. Specifically, the tensile strength of the cross-linked rubber of the present invention measured in accordance with the tensile test specified in JIS K6251:2010 is preferably 20 MPa or more, more preferably 25 MPa or more, further preferably 30 MPa or more, and particularly preferably 35 MPa or more. In addition, the elongation of the cross-linked rubber of the present invention measured in accordance with the tensile test specified in JIS K6251:2010 is preferably 250% or more, more preferably 300% or more, further preferably 350% or more, and particularly preferably 400% or more. In addition, the tear strength of the cross-linked rubber of the present invention measured using a tensile tester specified in JIS K6252:2007 is preferably 70 N / mm or more, more preferably 75 N / mm or more, and further preferably 80 N / mm.
[0122] The cross-linked rubber of the present invention can exhibit excellent fracture resistance and chipping resistance, and is preferably used in applications such as tires, belts, and anti-vibration rubbers.
[0123] Furthermore, the cross-linked rubber obtained by cross-linking a rubber composition containing a carbon material as an inorganic material also has excellent wear resistance and handling stability, and can be preferably used for tires of large vehicles. In addition, the cross-linked rubber obtained by cross-linking a rubber composition containing silica as an inorganic material also has excellent wet grip and low heat generation properties, and can be preferably used for tires of light vehicles.
[0124] Example
[0125] The present invention will be described below based on more detailed examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" are based on weight.
[0126] In addition, various tests and evaluations were performed according to the following methods.
[0127] <Molecular weight of ring-opening copolymer>
[0128] The number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the ring-opening copolymer were measured as polystyrene conversion values by gel permeation chromatography (GPC) using tetrahydrofuran as solvent. "HLC-8320GPC" (manufactured by Tosoh Corporation) was used as a measuring device. The measurement was carried out using a column composed of four "TSKgel Super Multipore HZ-H" (manufactured by Tosoh Corporation) connected in series as a column, under the conditions of flow rate: 0.35 ml / min, sample injection volume: 10 μml, and column temperature: 40°C.
[0129] <Ratio of the structural unit derived from the norbornene compound and the structural unit derived from cyclooctadiene>
[0130] The ratio of monomer units in the ring-opening copolymer is determined by 1 The H-NMR spectrum was measured. Specifically, deuterated chloroform was used as the solvent. 1 In the H-NMR measurement, the ratio of the monomer units in the ring-opening copolymer was determined based on the integrated ratio of the signal at 5.0 to 5.5 ppm derived from the double bond and the integrated ratio of the signal at 2.3 to 3.0 ppm derived from the norbornene compound.
[0131] <Cis / trans ratio of main chain double bonds>
[0132] The cis / trans ratio of the main chain double bonds in the ring-opening copolymers is determined by 13 It was determined by C-NMR spectrum measurement.
[0133] <Introduction rate of structural units from chain transfer terminals>
[0134] The introduction rate of the structural unit from the chain transfer terminal in the ring-opening copolymer is determined by 1Specifically, the determination is made by using deuterated chloroform as solvent. 1 The ratio of the monomer units in the ring-opening copolymer to the structural units derived from the chain transfer terminals is determined by H-NMR measurement based on the integrated ratio of the signals of 5.0 to 5.5 ppm derived from the double bond, the integrated ratio of the signals of 2.3 to 3.0 ppm derived from the norbornene compound, and the integrated ratio of the signals of -0.5 to 0.5 ppm in the case of a chain transfer terminal having a silyl group, and is determined by comparison with the number average molecular weight (Mn) of the ring-opening copolymer calculated by the above-mentioned GPC.
[0135] <Glass transition temperature (Tg) of ring-opening copolymer>
[0136] The glass transition temperature (Tg) of the ring-opening copolymer was measured at a temperature increase rate of 10°C / min between -150°C and 40°C using a differential scanning calorimeter (DSC "X-DSC7000" (manufactured by Hitachi High-Technologies Corporation)).
[0137] <Tensile test>
[0138] A sheet-shaped cross-linked rubber product is produced by press-crosslinking the rubber composition, and the cross-linked rubber product is punched into a dumbbell-shaped No. 6 shape specified in JIS K6251:2010 in a direction parallel to the grain direction, thereby obtaining a dumbbell-shaped test piece. Then, the obtained dumbbell-shaped test piece is subjected to a tensile test at 23°C and 500 mm / min using a tensile testing machine (product name "TENSOMETER 10K", manufactured by Alpha Tech) in accordance with JIS K6251:2010 to measure the tensile strength and elongation. The higher the tensile strength, the better the fracture resistance.
[0139] <Tear test>
[0140] A sheet-shaped cross-linked rubber product is prepared by press-crosslinking the rubber composition, and the cross-linked rubber product is punched into a square shape without cuts specified in JIS K6252: 2007 in a direction perpendicular to the grain direction to obtain a test piece. Then, the obtained test piece is subjected to a tear test at 23°C and 500 mm / min using a tensile tester (product name "TENSOMETER 10K", manufactured by Alpha Tech) in accordance with JIS K6252: 2007 to measure the tear strength. The higher the tear strength, the better the chipping resistance.
[0141] <Resilience test>
[0142] The rubber composition was press-molded using a metal mold while being pressurized to obtain a cylindrical cross-linked rubber for a high resilience material having a diameter of 29 mm and a thickness of 12.5 mm. The obtained cylindrical cross-linked rubber for a high resilience material was then adjusted to 0° C. or 60° C. using a thermostatic bath, and immediately after being taken out, the rebound rate was measured using a Lupke type rebound tester (manufactured by Kobunsu Keiki Co., Ltd.) as a tester in accordance with JIS K6255:1996 at 23° C. and a holding force of 29 to 39 N.
[0143] <Wet Grip>
[0144] The rubber composition was press-crosslinked at 160°C for 20 minutes to prepare a test piece, and the obtained test piece was measured for tanδ at 0°C using ARES manufactured by Rheometrics under the conditions of 0.5% dynamic strain and 10 Hz. Then, the obtained measurement results were calculated as an index with the measured value of the sample of Comparative Example 6 described later as 100. The larger the index, the better the wet grip. In addition, wet grip was evaluated for Examples 11 to 20 and Comparative Examples 6 to 10.
[0145] <Low heat generation>
[0146] The rubber composition was press-crosslinked at 160°C for 20 minutes to prepare a test piece, and the obtained test piece was measured for tanδ at 60°C using ARES manufactured by Rheometrics under the conditions of dynamic strain 2.0% and 10 Hz. Then, the obtained measurement results were calculated as an index with the measured value of the sample of Comparative Example 6 described later as 100. The smaller the index, the better the low heat generation property. In addition, low heat generation property was evaluated for Examples 11 to 20 and Comparative Examples 6 to 10.
[0147] <DIN abrasion test>
[0148] The rubber composition was pressurized and molded using a metal mold to obtain a cylindrical rubber cross-linked product for high resilience material with a diameter of 16 mm and a thickness of 6 mm. Then, the obtained cylindrical rubber cross-linked product for high resilience material was tested using a DIN abrasion tester (product name "AB-6110", manufactured by Ueshima Seisakusho Co., Ltd.) as a tester, and the relative wear volume was measured according to JIS K6264-2:2005 under the conditions of test method A, additional force 10 N, friction distance 40 m, 23°C, and reference test piece D1. The smaller the relative wear volume, the better the wear resistance. In addition, DIN abrasion tests were performed on Examples 1 to 10 and Comparative Examples 1 to 5.
[0149] <Rubber hardness>
[0150] The rubber composition was press-crosslinked at 160°C for 20 minutes to prepare a test piece, and the obtained test piece was used to measure the hardness at 20°C using a type A durometer according to JIS K6253. The result obtained is expressed with the value of the standard example being 100. The larger the index of rubber hardness, the better the handling stability. In addition, the rubber hardness of Examples 1 to 10 and Comparative Examples 1 to 5 was evaluated.
[0151] [Polymerization Example 1]
[0152] (Preparation of Ring-Opening Copolymer (A))
[0153] In a nitrogen environment, 100 parts of 2-norbornene (NB) as a norbornene compound, 60 parts of 1,5-cyclooctadiene (COD), 394 parts of toluene, and 0.10 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.005 parts of (1,3-dimesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0154] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 159 parts of a ring-opening copolymer (A). The number average molecular weight (Mn) of the obtained ring-opening copolymer (A) was 126,000, the weight average molecular weight (Mw) was 273,000, the ratio of 2-norbornene structural unit / 1,5-cyclooctadiene structural unit was 63 / 37 (weight ratio), the cis / trans ratio was 46 / 54, and the glass transition temperature (Tg) was -25°C. In addition, the weight ratio of 2-norbornene structural unit / 1,5-cyclooctadiene structural unit represents the ratio of the content ratio [weight %] of each structural unit. That is, the content ratio of the structural unit derived from 2-norbornene in the ring-opening copolymer (A) was 63% by weight, and the content ratio of the structural unit derived from 1,5-cyclooctadiene was 37% by weight. Similarly, hereinafter, the weight ratio of the monomer units in the ring-opening copolymer means the ratio of the content ratio [weight %] of each monomer unit in the ring-opening copolymer.
[0155] [Polymerization Example 2]
[0156] (Preparation of Ring-Opening Copolymer (B))
[0157] In a nitrogen environment, 110 parts of dicyclopentadiene (DCPD) as a norbornene compound, 90 parts of 1,5-cyclooctadiene (COD), 800 parts of toluene and 0.11 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.010 parts of (1,3-dimesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0158] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 195 parts of a ring-opening copolymer (B). The number average molecular weight (Mn) of the obtained ring-opening copolymer (B) was 124,000, the weight average molecular weight (Mw) was 259,000, the ratio of dicyclopentadiene structural unit / 1,5-cyclooctadiene structural unit was 55 / 45 (weight ratio), the cis / trans ratio was 42 / 58, and the glass transition temperature (Tg) was -26°C.
[0159] [Polymerization Example 3]
[0160] (Preparation of Ring-Opening Copolymer (C))
[0161] Under nitrogen environment, 41 parts of 2-norbornene (NB) as a norbornene compound, 39 parts of dicyclopentadiene (DCPD) as a norbornene compound, 75 parts of cyclooctadiene, 620 parts of toluene and 0.14 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.005 parts of (1,3-dimesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0162] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 145 parts of a ring-opening copolymer (C). The number average molecular weight (Mn) of the obtained ring-opening copolymer (C) was 133,000, the weight average molecular weight (Mw) was 268,000, the ratio of 2-norbornene structural unit / dicyclopentadiene structural unit / cyclooctadiene structural unit was 27 / 25 / 48 (weight ratio), the cis / trans ratio was 42 / 58, and the glass transition temperature (Tg) was -40°C.
[0163] [Polymerization Example 4]
[0164] (Preparation of Ring-Opening Copolymer (D))
[0165] Under nitrogen environment, 100 parts of dicyclopentadiene (DCPD) as a norbornene compound, 180 parts of 1,5-cyclooctadiene (COD), 1120 parts of toluene and 0.15 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.011 parts of (1,3-dimesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene were added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0166] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 276 parts of a ring-opening polymer (D). The number average molecular weight (Mn) of the obtained ring-opening polymer (D) was 121,000, the weight average molecular weight (Mw) was 255,000, the ratio of dicyclopentadiene structural unit / 1,5-cyclooctadiene structural unit was 36 / 64 (weight ratio), the cis / trans ratio was 37 / 63, and the glass transition temperature (Tg) was -43°C.
[0167] [Polymerization Example 5]
[0168] (Preparation of Ring-Opening Copolymer (E))
[0169] In a nitrogen atmosphere, 70 parts of tetracyclic [6.2.1.1 3,6 .0 2,7 ] dodec-4-ene (tetracyclododecene; TCD), 180 parts of 1,5-cyclooctadiene (COD), 1000 parts of toluene and 0.14 parts of 1-hexene. Next, 0.015 parts of (1,3-di-mesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene were added and the polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0170] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 242 parts of a ring-opening copolymer (E). The number average molecular weight (Mn) of the obtained ring-opening copolymer (E) was 138,000, the weight average molecular weight (Mw) was 262,000, the ratio of tetracyclododecene structural unit / 1,5-cyclooctadiene structural unit was 28 / 72 (weight ratio), the cis / trans ratio was 34 / 66, and the glass transition temperature (Tg) was -23°C.
[0171] [Polymerization Example 6]
[0172] (Preparation of Ring-Opening Copolymer (F))
[0173] Under nitrogen environment, 100 parts of dicyclopentadiene (DCPD) as a norbornene compound, 245 parts of 1,5-cyclooctadiene (COD), 1400 parts of toluene and 0.20 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.015 parts of (1,3-dimesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0174] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 340 parts of a ring-opening copolymer (F). The number average molecular weight (Mn) of the obtained ring-opening copolymer (F) was 122,000, the weight average molecular weight (Mw) was 246,000, the ratio of dicyclopentadiene structural unit / 1,5-cyclooctadiene structural unit was 29 / 71 (weight ratio), the cis / trans ratio was 35 / 65, and the glass transition temperature (Tg) was -50°C.
[0175] [Polymerization Example 7]
[0176] (Preparation of Ring-Opening Copolymer (G))
[0177] In a nitrogen environment, 100 parts of 2-norbornene (NB) as a norbornene compound, 60 parts of 1,5-cyclooctadiene (COD), 394 parts of toluene, and 0.38 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.005 parts of (1,3-dimesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0178] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 158 parts of a ring-opening copolymer (G). The number average molecular weight (Mn) of the obtained ring-opening copolymer (G) was 32,000, the weight average molecular weight (Mw) was 67,000, the ratio of 2-norbornene structural unit / 1,5-cyclooctadiene structural unit was 63 / 37 (weight ratio), the cis / trans ratio was 46 / 54, and the glass transition temperature (Tg) was -27°C.
[0179] [Polymerization Example 8]
[0180] (Preparation of Ring-Opening Copolymer (H))
[0181] Under nitrogen environment, 110 parts of dicyclopentadiene (DCPD) as a norbornene compound, 90 parts of 1,5-cyclooctadiene (COD), 800 parts of toluene and 0.43 parts of vinyl tris (trimethylsiloxy) silane were added to a glass reaction container with a stirrer. Next, 1.000 parts of (1,3-di-mesityl imidazolidin-2-ylidene) (tricyclohexylphosphine) benzal dichlororuthenium (II) dissolved in 10 parts of toluene were added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0182] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 192 parts of a ring-opening copolymer (H). The number average molecular weight (Mn) of the obtained ring-opening copolymer (H) was 133,000, the weight average molecular weight (Mw) was 264,000, the ratio of dicyclopentadiene structural unit / 1,5-cyclooctadiene structural unit was 55 / 45 (weight ratio), the cis / trans ratio was 42 / 58, and the glass transition temperature (Tg) was -25°C. 1 The introduction rate of oxysilyl groups into the chain transfer terminals identified by H-NMR was 94%, that is, the value of the percentage of the number of ring-opening copolymer chain terminals into which the modifying group was introduced / the total number of ring-opening copolymer chain terminals was 47%.
[0183] [Polymerization Example 9]
[0184] (Preparation of Ring-Opening Copolymer (I))
[0185] In a nitrogen environment, 110 parts of dicyclopentadiene (DCPD) as a norbornene compound, 90 parts of 1,5-cyclooctadiene (COD), 800 parts of toluene and 0.11 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.030 parts of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium (II) dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0186] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 194 parts of a ring-opening copolymer (I). The number average molecular weight (Mn) of the obtained ring-opening copolymer (I) was 128,000, the weight average molecular weight (Mw) was 266,000, the ratio of dicyclopentadiene structural unit / 1,5-cyclooctadiene structural unit was 54 / 46 (weight ratio), the cis / trans ratio was 20 / 80, and the glass transition temperature (Tg) was -26°C.
[0187] [Polymerization Example 10]
[0188] (Preparation of diisobutylaluminum hexyloxide / toluene solution)
[0189] In a nitrogen atmosphere, 88 parts of toluene and 7.8 parts of a 25.4 wt% triisobutylaluminum / n-hexane solution (manufactured by Tosoh Finechem Corporation) were added to a glass container containing a stirrer. The mixture was cooled to -45°C and 1.02 parts (molar equivalent relative to triisobutylaluminum) of n-hexanol was slowly added dropwise while being vigorously stirred. The mixture was then allowed to stand at room temperature while being stirred to prepare a hexyloxy diisobutylaluminum / toluene solution (2.5 wt%).
[0190] (Preparation of Ring-Opening Copolymer (J))
[0191] Next, in a nitrogen atmosphere, 17.4 parts of a 1.0 wt % tungsten hexachloride / toluene solution and 8.6 parts of a 2.5 wt % diisobutylaluminum hexoxide / toluene solution were added to a glass reaction container equipped with a stirrer and stirred for 10 minutes to obtain a catalyst solution.
[0192] Next, 110 parts of dicyclopentadiene (DCPD) as a norbornene compound, 90 parts of 1,5-cyclooctadiene (COD), 800 parts of toluene and 0.35 parts of 1-hexene were added, and polymerization was carried out at room temperature for 6 hours. After the polymerization, an excess amount of methanol was added to terminate the polymerization.
[0193] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 193 parts of a ring-opening copolymer (J). The number average molecular weight (Mn) of the obtained ring-opening copolymer (J) was 119,000, the weight average molecular weight (Mw) was 245,000, the ratio of dicyclopentadiene structural unit / 1,5-cyclooctadiene structural unit was 54 / 46 (weight ratio), the cis / trans ratio was 73 / 27, and the glass transition temperature (Tg) was -27°C.
[0194] [Polymerization Example 11]
[0195] (Preparation of Ring-Opening Copolymer (a))
[0196] In a nitrogen atmosphere, 100 parts of 2-norbornene (NB) as a norbornene compound, 100 parts of cyclopentene (CPE), 394 parts of toluene, and 0.12 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.006 parts of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0197] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 160 parts of a ring-opening copolymer (a). The number average molecular weight (Mn) of the obtained ring-opening copolymer (a) was 122,000, the weight average molecular weight (Mw) was 234,000, the ratio of 2-norbornene structural unit / cyclopentene structural unit was 62 / 38 (weight ratio), the cis / trans ratio was 17 / 83, and the glass transition temperature (Tg) was -24°C.
[0198] [Polymerization Example 12]
[0199] (Preparation of Ring-Opening Copolymer (b))
[0200] In a nitrogen atmosphere, 45 parts of dicyclopentadiene (DCPD) as a norbornene compound, 55 parts of cyclopentene (CPE), 233 parts of toluene, and 0.08 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.011 parts of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium (II) dissolved in 6 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 3 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0201] The polymerization solution was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 62 parts of a ring-opening copolymer (b). The obtained ring-opening copolymer (b) had a number average molecular weight (Mn) of 119,000, a weight average molecular weight (Mw) of 238,000, a ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn) of 2.00, a ratio of dicyclopentadiene (DCPD) structural unit / cyclopentene structural unit of 55 / 45 (weight ratio), a cis / trans ratio of 17 / 83, and a glass transition temperature (Tg) of -25°C.
[0202] [Polymerization Example 13]
[0203] (Preparation of Ring-Opening Copolymer (c))
[0204] In a nitrogen atmosphere, 41 parts of 2-norbornene (NB) as a norbornene compound, 39 parts of dicyclopentadiene (DCPD) as a norbornene compound, 100 parts of cyclopentene (CPE), 394 parts of toluene, and 0.14 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.017 parts of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0205] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 145 parts of a ring-opening copolymer (c). The number average molecular weight (Mn) of the obtained ring-opening copolymer (c) was 126,000, the weight average molecular weight (Mw) was 254,000, the ratio of 2-norbornene structural unit / dicyclopentadiene structural unit / cyclopentene structural unit was 27 / 25 / 48 (weight ratio), the cis / trans ratio was 18 / 82, and the glass transition temperature (Tg) was -40°C.
[0206] [Polymerization Example 14]
[0207] (Preparation of Ring-Opening Copolymer (d))
[0208] In a nitrogen atmosphere, 72 parts of dicyclopentadiene (DCPD) as a norbornene compound, 188 parts of cyclopentene (CPE), 1160 parts of toluene, and 0.17 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.028 parts of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium dissolved in 10 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 4 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0209] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 217 parts of a ring-opening copolymer (d). The number average molecular weight (Mn) of the obtained ring-opening copolymer (d) was 120,000, the weight average molecular weight (Mw) was 248,000, the ratio of dicyclopentadiene structural unit / cyclopentene structural unit was 36 / 64 (weight ratio), the cis / trans ratio was 17 / 83, and the glass transition temperature (Tg) was -45°C.
[0210] [Polymerization Example 15]
[0211] (Preparation of Ring-Opening Copolymer (e))
[0212] In a nitrogen atmosphere, 100 parts of tetracyclic [6.2.1.1 3,6 .0 2,7 ] 4-dodecene (tetracyclododecene; TCD), 300 parts of cyclopentene (CPE), 380 parts of toluene and 8.6 parts of 1-hexene. Then, 0.028 parts of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium dissolved in 10 parts of toluene was added, and polymerization was carried out at room temperature for 4 hours. After the polymerization, an excess of vinyl ethyl ether was added to terminate the polymerization.
[0213] The polymer solution obtained above was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 290 parts of a ring-opening copolymer (e). The number average molecular weight (Mn) of the obtained ring-opening copolymer (e) was 131,000, the weight average molecular weight (Mw) was 253,000, the ratio of tetracyclododecene structural unit / cyclopentene structural unit was 28 / 72 (weight ratio), the cis / trans ratio was 17 / 83, and the glass transition temperature (Tg) was -22°C.
[0214] [Example 1]
[0215] (Preparation of rubber composition)
[0216] 100 parts of the ring-opening polymer (A) obtained in Polymerization Example 1 were masticated in a Banbury mixer having a volume of 250 ml, and 50 parts of carbon black (trade name "SEAST 9H", manufactured by Tokai Carbon Co., Ltd.), 3 parts of zinc oxide (zinc white No. 1), 2.0 parts of stearic acid (trade name "SA-300", manufactured by Aidi Co., Ltd.) and 2.0 parts of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (trade name "NOCRAC 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd., antioxidant) were added thereto, and the rubber composition was discharged from the Banbury mixer after kneading at a starting temperature of 80°C for 4 minutes. The temperature of the rubber composition at the end of kneading was 160°C. Next, the obtained rubber composition was kneaded with 1.75 parts of sulfur and 1 part of N-cyclohexylbenzothiazole-2-sulfenamide (trade name "NOCCELER CZ-G (CZ)", manufactured by Ouchi Shinko Chemical Industry Co., Ltd., a crosslinking accelerator) using an open roll at 50°C, and then the sheet-like rubber composition was taken out. The obtained rubber composition was evaluated for tensile strength, elongation, tear strength, rebound rate, relative wear volume and rubber hardness. The results are shown in Table 1.
[0217] [Examples 2 to 10]
[0218] A rubber composition was obtained in the same manner as in Example 1 except that 100 parts of the ring-opening copolymers (B) to (J) shown in Table 1 were used instead of the ring-opening copolymer (A), and the rubber composition was evaluated in the same manner.
[0219] [Comparative Examples 1 to 5]
[0220] A rubber composition was obtained in the same manner as in Example 1 except that 100 parts of the ring-opening copolymers (a) to (e) shown in Table 1 were used instead of the ring-opening copolymer (A), and the rubber composition was evaluated in the same manner.
[0221] [Table 1]
[0222]
[0223] As shown in Table 1, the cross-linked rubbers obtained by cross-linking the rubber compositions of Examples 1 to 10 containing an inorganic material and a ring-opening copolymer containing a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound showed excellent tensile strength, elongation, tear strength and resilience compared to the case where cyclopentene was used instead of cyclooctadiene (Comparative Examples 1 to 5). In addition, the cross-linked rubbers obtained by cross-linking the rubber compositions of Examples 1 to 10 using carbon black as an inorganic material also showed excellent wear resistance and rubber hardness.
[0224] [Example 11]
[0225] (Preparation of rubber composition)
[0226] To 100 parts of the ring-opening copolymer (A) obtained in Polymerization Example 1 was added 50 parts of silica (trade name "Zeosil 1165MP", manufactured by Rhodia, nitrogen adsorption specific surface area (BET method): 163 m 2 / g) and 10 parts of processing oil (trade name "Aromax T-DAE", manufactured by Nippon Oil Corporation), 6.0 parts of silane coupling agent (bis(3-(triethoxysilyl)propyl)tetrasulfide, trade name "Si69", manufactured by Degussa), and kneading for 1.5 minutes at a starting temperature of 110°C. To the kneaded material, 25 parts of silica (trade name "Zeosil 1165MP", manufactured by Rhodia), 3 parts of zinc oxide (zinc white No. 1), 2.0 parts of stearic acid (trade name "SA-300", manufactured by Asahi Denka Kogyo Co., Ltd.) and 2.0 parts of antioxidant (N-phenyl-N′-(1,3-dimethylbutyl) p-phenylenediamine, trade name "NOCRAC 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added, kneading was carried out for 2.5 minutes, and the rubber composition was discharged from the Banbury mixer. The temperature of the rubber composition at the end of mixing was 150°C. After the rubber composition was cooled to room temperature, it was mixed again in a Banbury mixer for 3 minutes, and then the rubber composition was discharged from the Banbury mixer. Next, the obtained rubber composition was mixed with 1.5 parts of sulfur and a crosslinking accelerator (a mixture of 1.8 parts of N-tert-butyl-2-benzothiazole sulfonamide (trade name "NOCCELER NS", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) and 1.5 parts of diphenylguanidine (trade name "NOCCELER D", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)) with an open roll at 50°C, and then the sheet-like rubber composition was taken out. The obtained rubber composition was evaluated for tensile strength, elongation, tear strength, rebound rate, wet grip and low heat generation. The results are shown in Table 1.
[0227] [Examples 12 to 20]
[0228] The rubber composition was obtained in the same manner as in Example 11 except that 100 parts of the ring-opening copolymers (B) to (J) shown in Table 1 were used instead of the ring-opening copolymer (A), and the rubber composition was evaluated in the same manner.
[0229] [Comparative Examples 6 to 10]
[0230] The rubber composition was obtained in the same manner as in Example 11 except that 100 parts of the ring-opening copolymers (b) to (e) shown in Table 1 were used instead of the ring-opening copolymer (A), and the rubber composition was evaluated in the same manner.
[0231] [Table 2]
[0232]
[0233] As shown in Table 2, the cross-linked rubbers obtained by cross-linking the rubber compositions of Examples 11 to 20 containing an inorganic material and a ring-opening copolymer containing a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound showed excellent tensile strength, elongation, tear strength and rebound rate compared to the case where cyclopentene was used instead of cyclooctadiene (Comparative Examples 6 to 10). In addition, the cross-linked rubbers obtained by cross-linking the rubber compositions of Examples 11 to 20 using silica as an inorganic material also showed excellent wet grip and low heat build-up properties.
Claims
1. A rubber composition comprising an inorganic material and a ring-opening copolymer, wherein the ring-opening copolymer comprises a structural unit derived from cyclooctadiene and a structural unit derived from a norbornene compound.
2. The rubber composition according to claim 1, wherein The inorganic material is a carbon material or silicon dioxide.
3. The rubber composition according to claim 1 or 2, wherein: The norbornene compound is a norbornene compound represented by the following general formula (1): In the formula, R 1 ~R 4 represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom, and R 2 and R 3 They can bond to each other to form a ring structure, and m is 0 or 1.
4. The rubber composition according to claim 3, wherein The R 1 ~R 4 It is a hydrogen atom, a chain hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom or a nitrogen atom.
5. The rubber composition according to any one of claims 1 to 4, wherein The weight average molecular weight of the ring-opening polymer is 50,000 to 1,000,000.
6. The rubber composition according to any one of claims 1 to 5, wherein The glass transition temperature of the ring-opening polymer is -80 to 10°C. 7 . The rubber composition according to claim 1 , further comprising a rubber other than the ring-opening copolymer. 8 . A cross-linked rubber product obtained by cross-linking the rubber composition according to claim 1 .
Citation Information
Patent Citations
Rubber composition for tire
JP1994248116A
Composition for fracture-resistant material, crosslinked product for fracture-resistant material and fracture-resistant material
JP2020015832A