Nitride semiconductor substrate and method for manufacturing nitride semiconductor substrate

By forming a high-quality Group III nitride semiconductor layer on the support substrate, the problem of poor crystallinity of the GaN epitaxial layer on the GaN support substrate is solved, and production of GaN substrates with high frequency characteristics and high thickness is achieved, reducing production costs.

CN118900941APending Publication Date: 2024-11-05SHIN ETSU HANDOTAI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280083343.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2022-11-08
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art has failed to effectively improve the crystallinity of the GaN epitaxial layer on the GaN support substrate, resulting in warping and dislocation problems, and limiting the thickness and quality of the GaN substrate.

Method used

By forming a Group III nitride semiconductor layer containing GaN on the support substrate, using the composite substrate structure and planarization layer, the crystallinity of the (0002) growth surface of GaN reaches less than 550 angle seconds, reducing warpage and dislocation, and forming High-quality Group III nitride semiconductor layer.

Benefits of technology

The high crystallinity and low dislocation density of the GaN epitaxial layer are achieved, which extends the thickness and growth time of the substrate, reduces production costs, and avoids wafer rupture and warping problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900941A_ABST
    Figure CN118900941A_ABST
Patent Text Reader

Abstract

Provided is a nitride semiconductor substrate in which a group III nitride semiconductor layer containing GaN is formed on a support substrate, the nitride semiconductor substrate being characterized in that the support substrate comprises: a composite substrate in which a plurality of layers are laminated, the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer laminated to the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer; and a group III nitride semiconductor seed layer which is bonded on the composite substrate with a planarization layer interposed therebetween and which contains at least GaN. The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed layer, and the crystallinity of the (0002) growth surface of GaN in the group III nitride semiconductor seed layer is 550 seconds of arc or less in XRD half-width. As a result, it is possible to provide a nitride semiconductor including a group III nitride semiconductor layer having little warpage, little dislocation occurrence, and good crystallinity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nitride semiconductor substrate and a method for manufacturing the nitride semiconductor substrate. Background Art

[0002] MOCVD, one of the semiconductor thin film manufacturing methods, is excellent in terms of large diameter and mass production, and can form a homogeneous thin film crystal, so it is widely used. Nitride semiconductors represented by GaN are expected to be the next generation of semiconductor materials that surpass the limitations of Si materials.

[0003] GaN can be used to manufacture devices that can operate at high frequencies due to its high saturation electron velocity, and can operate at high output power due to its large dielectric breakdown electric field. In addition, it can be expected to be lighter, smaller, and have lower power consumption.

[0004] In recent years, due to the increase in communication speed represented by 5G and the demand for higher output power accompanying this increase in speed, GaN HEMTs that can operate at high frequencies and high output powers have attracted attention.

[0005] As a substrate used in GaN epitaxial wafers for making GaN devices, silicon single crystal substrates are the cheapest and are conducive to large diameters. In addition, SiC substrates are also used because of their high thermal conductivity and good heat dissipation. However, these substrates are prone to cracks due to stress during the cooling process after epitaxial film formation due to the difference in thermal expansion coefficient from GaN. In addition, due to the application of strong stress, wafer breakage sometimes occurs during the device process. In addition, thicker GaN films cannot be formed, and even if complex stress relief layers are formed in the epitaxial layer, the maximum thickness without cracks is about 5μm.

[0006] Since the GaN substrate has the same (or very similar) thermal expansion coefficient as the GaN epitaxial growth layer, it is not easy to cause the above-mentioned cracking problem and the problem of wafer breakage caused by warping. In addition, since the lattice constant difference between the GaN substrate and the epitaxially grown GaN layer is extremely small, the problem of dislocation or deterioration of crystallinity caused by the lattice constant difference can be solved.

[0007] However, independent GaN substrates are not only difficult to manufacture, but also expensive and cannot produce substrates with larger diameters, so they are not suitable for mass production.

[0008] Therefore, a large-diameter substrate for GaN epitaxy (hereinafter referred to as a GaN support substrate or simply a growth substrate) has been developed, which has a large diameter and a thermal expansion coefficient close to that of GaN. A conventional GaN support substrate is composed of a support structure, a planarization layer stacked on one surface of the support structure, and a single crystal silicon layer stacked on the planarization layer, wherein the support structure includes a polycrystalline ceramic core, a first adhesive layer, a conductive layer, a second adhesive layer, and a barrier layer. In addition, sometimes there is a case where the conductive layer is not formed or is formed only on one side. Alternatively, there is a case where a conductive layer is formed on the back side of the barrier layer.

[0009] By using the GaN support substrate, a GaN epitaxial substrate can be produced, which has a large diameter and a thick epitaxial film without cracks. In addition, since the difference in thermal expansion coefficient with GaN is extremely small, it is not easy to warp during GaN growth or cooling, so that the warping of the substrate after film formation can be controlled to be small, and there is no need to set a complex stress relaxation layer in the epitaxial growth layer, so the epitaxial film formation time is shortened, which can significantly reduce the cost required for epitaxial growth.

[0010] Furthermore, since most of the GaN support substrate is made of ceramic, the substrate itself is very hard and is not easily plastically deformed, and wafer cracking that occurs when a nitride semiconductor is grown on a silicon single crystal substrate with a large diameter does not occur.

[0011] Patent Document 1 discloses a technique for bonding a substrate (GaN support substrate) having a thermal expansion coefficient close to that of GaN.

[0012] Although the GaN support substrate is not prone to warping during growth due to differences in thermal expansion coefficients, the surface layer is composed of a silicon layer, which is prone to lattice constant differences with the GaN layer and crystal defects (dislocations). As a result, the crystallinity of the GaN epitaxial layer formed on the GaN support substrate does not change much from that when a silicon single crystal substrate is used as a support substrate.

[0013] Patent Document 2 describes a method of exfoliating a sapphire substrate and a GaN layer by irradiating with pulsed laser beams.

[0014] Patent Document 3 describes a method of peeling off a semiconductor thin film by laser beam processing or the like, and then bonding the thin film to another substrate.

[0015] Prior art literature

[0016] Patent Literature

[0017] Patent Document 1: Japanese Patent Application No. 2019-523994

[0018] Patent Document 2: Japanese Patent Application Publication No. 2013-21225

[0019] Patent Document 3: Japanese Patent Application Publication No. 2010-161355 Summary of the invention

[0020] 1. Technical issues to be resolved

[0021] However, Patent Documents 1 to 3 do not describe or suggest a measure for improving the crystallinity of a GaN epitaxial layer formed on a GaN supporting substrate.

[0022] The present invention is made to solve the above-mentioned problems, and an object of the present invention is to provide a nitride semiconductor substrate and a method for manufacturing the same, wherein the nitride semiconductor substrate includes a Group III nitride semiconductor layer with little warping, little dislocation and good crystallinity.

[0023] (II) Technical solution

[0024] In order to solve the above problems, the present invention provides a nitride semiconductor substrate, which is a nitride semiconductor substrate having a group III nitride semiconductor layer containing GaN formed on a supporting substrate, characterized in that:

[0025] The supporting substrate comprises:

[0026] A composite substrate, which is formed by stacking a plurality of layers, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer stacked on the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer; and,

[0027] A group III nitride semiconductor seed layer, which is bonded to the composite substrate via a planarization layer and contains at least GaN;

[0028] The III-nitride semiconductor layer is formed on the III-nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the III-nitride semiconductor seed crystal layer is less than 550 arc seconds (arcsec) in terms of XRD half-peak width.

[0029] If a nitride semiconductor substrate is formed by forming a Group III nitride semiconductor layer on a Group III nitride semiconductor seed layer in which the crystallinity of the (0002) growth plane of the GaN seed crystal is less than 550 arc seconds in terms of XRD half-peak width, then a substrate having a Group III nitride semiconductor layer with extremely small dislocation density and good crystallinity can be made, thereby improving the characteristics of the device.

[0030] In addition, in the case of the nitride semiconductor substrate of the present invention, by including a supporting substrate, and the supporting substrate including a composite substrate in which a plurality of layers are stacked, the warping of the group III nitride semiconductor layer during epitaxial growth caused by the difference in thermal expansion coefficient can be reduced, and a group III nitride semiconductor layer having no cracks and a large thickness can be provided. Therefore, the group III nitride semiconductor layer can be finally peeled off from the supporting substrate and used as an independent substrate.

[0031] Furthermore, the present invention provides a nitride semiconductor substrate, wherein a Group III nitride semiconductor layer including GaN is formed on a support substrate, wherein:

[0032] The supporting substrate comprises:

[0033] A composite substrate, which is stacked with a plurality of layers, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a barrier layer bonded to the entire first adhesive layer, a second adhesive layer bonded to the back side of the barrier layer, and a conductive layer bonded to the back side of the second adhesive layer; and,

[0034] A group III nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer bonded only to a surface of the composite substrate and comprising at least GaN;

[0035] The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

[0036] If a nitride semiconductor substrate is formed by forming a Group III nitride semiconductor layer on a Group III nitride semiconductor seed layer in which the crystallinity of the (0002) growth plane of the GaN seed crystal is less than 550 arc seconds in terms of XRD half-peak width, then a substrate having a Group III nitride semiconductor layer with extremely small dislocation density and good crystallinity can be made, thereby improving the characteristics of the device.

[0037] In addition, if such a nitride semiconductor substrate includes a supporting substrate, and the supporting substrate includes a composite substrate in which a plurality of layers are stacked, the warping of the III-nitride semiconductor layer during epitaxial growth caused by the difference in thermal expansion coefficient can be reduced, so that a III-nitride semiconductor layer having no cracks and a large thickness can be obtained. Therefore, the III-nitride semiconductor layer can be finally peeled off from the supporting substrate and used as an independent substrate.

[0038] Furthermore, with the nitride semiconductor substrate of the present invention including the above-mentioned support substrate, no leakage path is generated due to the conductive layer on the surface side of the support substrate, and a substrate having excellent high-frequency characteristics can be obtained.

[0039] Furthermore, the present invention provides a nitride semiconductor substrate, wherein a Group III nitride semiconductor layer including GaN is formed on a support substrate, wherein:

[0040] The supporting substrate comprises:

[0041] A composite substrate, which is formed by stacking a plurality of layers, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a conductive layer bonded to the back side of the first adhesive layer, a second adhesive layer bonded to the back side of the conductive layer, and a barrier layer bonded to the surface and side of the first adhesive layer, the side of the conductive layer, and the side and back of the second adhesive layer; and,

[0042] A group III nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer bonded only to a surface of the composite substrate and comprising at least GaN;

[0043] The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

[0044] If a nitride semiconductor substrate is formed by forming a Group III nitride semiconductor layer on a Group III nitride semiconductor seed layer in which the crystallinity of the (0002) growth plane of the GaN seed crystal is less than 550 arc seconds in terms of XRD half-peak width, then a substrate having a Group III nitride semiconductor layer with extremely small dislocation density and good crystallinity can be made, thereby improving the characteristics of the device.

[0045] In addition, if such a nitride semiconductor substrate includes a supporting substrate, and the supporting substrate includes a composite substrate in which a plurality of layers are stacked, the warping of the III-nitride semiconductor layer during epitaxial growth caused by the difference in thermal expansion coefficient can be reduced, so that a III-nitride semiconductor layer having no cracks and a large thickness can be obtained. Therefore, the III-nitride semiconductor layer can be finally peeled off from the supporting substrate and used as an independent substrate.

[0046] Furthermore, with the nitride semiconductor substrate of the present invention including the above-mentioned support substrate, no leakage path is generated due to the conductive layer on the surface side of the support substrate, and a substrate having excellent high-frequency characteristics can be obtained.

[0047] The group III nitride semiconductor layer may include one or more of AlN and AlGaN in addition to GaN.

[0048] As such, the Group III nitride semiconductor layer may include a nitride other than GaN.

[0049] The polycrystalline ceramic core preferably comprises aluminum nitride.

[0050] If the polycrystalline ceramic core contains aluminum nitride, the difference in thermal expansion coefficient can be made extremely small.

[0051] Preferably, the first adhesive layer and the second adhesive layer respectively comprise tetraethyl silicate and / or silicon oxide, and the barrier layer comprises silicon nitride.

[0052] The first adhesive layer and the second adhesive layer may contain the above-mentioned compound, for example. In addition, as long as the barrier layer contains the above-mentioned compound, it is possible to sufficiently block the movement of impurities from the inside of the composite substrate to the Group III nitride semiconductor layer.

[0053] Preferably, the first adhesive layer and the second adhesive layer each have a thickness of 50 to 200 nm, and the barrier layer has a thickness of 100 to 1500 nm.

[0054] If the thickness of the first adhesive layer and the second adhesive layer is within the above range, the upper and lower layers can be bonded with sufficient force, and warping can be more reliably suppressed. In addition, if the thickness of the barrier layer is within the above range, it is possible to sufficiently block the movement of impurities from the inside of the composite substrate to the group III nitride semiconductor layer.

[0055] Preferably, the planarization layer includes at least one selected from the group consisting of tetraethyl silicate, silicon oxide, aluminum oxide, silicon nitride, and silicon oxynitride, and has a thickness of 500 nm to 3000 nm.

[0056] If such a planarizing layer is included, warping can be more reliably suppressed, and a group III nitride semiconductor layer having better crystallinity can be included. In addition, surface irregularities can be sufficiently planarized.

[0057] The Group III nitride semiconductor seed crystal layer may be a Group III nitride semiconductor seed crystal layer having a thickness of 100 nm or more.

[0058] The Group III nitride semiconductor seed crystal layer may have a thickness of, for example, 100 nm or more.

[0059] It is preferable that the composite substrate further includes a conductive layer laminated on the entire first adhesive layer or laminated on one side of the first adhesive layer between the first adhesive layer and the second adhesive layer.

[0060] By including such a conductive layer, a nitride semiconductor substrate including a portion having conductivity can be produced.

[0061] Preferably, the conductive layer has a thickness of 50 nm to 500 nm.

[0062] When the thickness of the conductive layer is within this range, it is possible to obtain a nitride semiconductor substrate that can suppress the occurrence of warping and includes a portion having excellent conductivity.

[0063] It is preferable that the composite substrate further includes a back surface conductive layer stacked on the back surface side surface to which the Group III nitride semiconductor seed crystal layer is not bonded.

[0064] If such a back surface conductive layer is further provided, a nitride semiconductor substrate having conductivity on the back surface can be obtained.

[0065] In addition, the present invention provides a method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that the method comprises the following steps:

[0066] Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer;

[0067] Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width;

[0068] Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer;

[0069] Step (4), wherein a composite substrate formed by stacking a plurality of layers is prepared as a composite substrate different from the initial composite substrate, and a planarization layer is stacked on the composite substrate, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer stacked on the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer;

[0070] Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate;

[0071] Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate;

[0072] Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and

[0073] Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

[0074] In such a method for manufacturing a nitride semiconductor substrate, since a group III nitride semiconductor layer including GaN is epitaxially grown on a group III nitride semiconductor seed layer including GaN and having a crystallinity of 550 arc seconds or less in terms of XRD half-peak width of the GaN (0002) growth plane, a group III nitride semiconductor layer having a low dislocation density, i.e., good crystallinity, without lattice mismatch between the seed layer and the group III nitride semiconductor layer as an epitaxial growth layer, can be formed. Furthermore, by repeatedly performing this method, a group III nitride semiconductor layer with fewer dislocations can be formed.

[0075] In addition, the III-nitride semiconductor layer formed by this method can be stacked thicker due to the small number of dislocations. Furthermore, by using a support substrate including a composite substrate stacked with a plurality of layers as a support substrate, the warping of the III-nitride semiconductor layer during growth caused by the difference in thermal expansion coefficient can be reduced, and a III-nitride semiconductor layer having a large thickness and no cracks can be formed. Therefore, the III-nitride semiconductor layer can be finally peeled off from the support substrate and used as an independent substrate.

[0076] In addition, when the above-mentioned initial supporting substrate is used as a growth substrate, since the initial supporting substrate is peeled off from the bonding substrate by splitting the silicon single crystal thin film, the substrate obtained by re-bonding the silicon single crystal to the surface of the peeled off initial supporting substrate can be used again as the initial supporting substrate, thereby achieving the advantage of cost reduction.

[0077] Preferably, in step (4), a substrate further including a conductive layer laminated on the entire first adhesive layer or laminated on one side of the first adhesive layer between the first adhesive layer and the second adhesive layer is prepared as the composite substrate.

[0078] In this way, a nitride semiconductor substrate including a portion having conductivity can be manufactured.

[0079] In addition, the present invention provides a method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that the method comprises the following steps:

[0080] Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer;

[0081] Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width;

[0082] Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer;

[0083] Step (4), wherein, as a composite substrate different from the initial composite substrate, a composite substrate formed by stacking a plurality of layers is prepared, and a planarization layer is stacked only on a surface of the composite substrate, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a barrier layer bonded to the entire first adhesive layer, a second adhesive layer bonded to the back surface of the barrier layer, and a conductive layer bonded to the back surface of the second adhesive layer;

[0084] Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate;

[0085] Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate;

[0086] Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and

[0087] Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

[0088] In such a method for manufacturing a nitride semiconductor substrate, since a group III nitride semiconductor layer including GaN is epitaxially grown on a group III nitride semiconductor seed layer including GaN and having a crystallinity of 550 arc seconds or less in terms of XRD half-peak width of the GaN (0002) growth plane, a group III nitride semiconductor layer having a low dislocation density, i.e., good crystallinity, without lattice mismatch between the seed layer and the group III nitride semiconductor layer as an epitaxial growth layer, can be formed. Furthermore, by repeatedly performing this method, a group III nitride semiconductor layer with fewer dislocations can be formed.

[0089] In addition, the III-nitride semiconductor layer formed by this method can be stacked thicker due to the small number of dislocations. Furthermore, by using a support substrate including a composite substrate stacked with a plurality of layers as a support substrate, the warping of the III-nitride semiconductor layer during growth caused by the difference in thermal expansion coefficient can be reduced, and a III-nitride semiconductor layer having a large thickness and no cracks can be formed. Therefore, the III-nitride semiconductor layer can be finally peeled off from the support substrate and used as an independent substrate.

[0090] In addition, when the above-mentioned initial supporting substrate is used as a growth substrate, since the initial supporting substrate is peeled off from the bonding substrate by dividing the silicon single crystal thin film, the substrate obtained by re-bonding the silicon single crystal to the surface of the peeled off initial supporting substrate can be used again as the initial supporting substrate, thereby achieving the advantage of cost reduction.

[0091] Furthermore, according to such a method for manufacturing a nitride semiconductor substrate, a leakage path caused by the conductive layer on the surface side of the support substrate is not generated, and a nitride semiconductor substrate having excellent high-frequency characteristics can be manufactured.

[0092] In addition, the present invention provides a method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that the method comprises the following steps:

[0093] Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer;

[0094] Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width;

[0095] Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer;

[0096] Step (4), wherein, as a composite substrate different from the initial composite substrate, a composite substrate formed by stacking a plurality of layers is prepared, and a planarization layer is stacked only on a surface of the composite substrate, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a conductive layer bonded to the back surface of the first adhesive layer, a second adhesive layer bonded to the back surface of the conductive layer, and a barrier layer bonded to the surface and side surface of the first adhesive layer, the side surface of the conductive layer, and the side surface and back surface of the second adhesive layer;

[0097] Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate;

[0098] Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate;

[0099] Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and

[0100] Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

[0101] In such a method for manufacturing a nitride semiconductor substrate, since a group III nitride semiconductor layer including GaN is epitaxially grown on a group III nitride semiconductor seed layer including GaN and having a crystallinity of 550 arc seconds or less in terms of XRD half-peak width of the GaN (0002) growth plane, a group III nitride semiconductor layer having a low dislocation density, i.e., good crystallinity, without lattice mismatch between the seed layer and the group III nitride semiconductor layer as an epitaxial growth layer, can be formed. Furthermore, by repeatedly performing this method, a group III nitride semiconductor layer with fewer dislocations can be formed.

[0102] In addition, the III-nitride semiconductor layer formed by this method can be stacked thicker due to the small number of dislocations. Furthermore, by using a support substrate including a composite substrate stacked with a plurality of layers as a support substrate, the warping of the III-nitride semiconductor layer during growth caused by the difference in thermal expansion coefficient can be reduced, and a III-nitride semiconductor layer having a large thickness and no cracks can be formed. Therefore, the III-nitride semiconductor layer can be finally peeled off from the support substrate and used as an independent substrate.

[0103] In addition, when the above-mentioned initial supporting substrate is used as a growth substrate, since the initial supporting substrate is peeled off from the bonding substrate by dividing the silicon single crystal thin film, the substrate obtained by re-bonding the silicon single crystal to the surface of the peeled off initial supporting substrate can be used again as the initial supporting substrate, thereby achieving the advantage of cost reduction.

[0104] Furthermore, such a method for manufacturing a nitride semiconductor substrate can produce a nitride semiconductor substrate having excellent high frequency characteristics without generating a leakage path due to the conductive layer on the surface side of the support substrate.

[0105] The wavelength of the laser light used in step (3) is preferably 360 nm to 1100 nm.

[0106] Thereby, the separation layer can be formed reliably in the vicinity of the interface with the silicon single crystal thin film of the growth substrate or the silicon single crystal substrate.

[0107] (III) Beneficial effects

[0108] As described above, the nitride semiconductor substrate of the present invention can include a Group III nitride semiconductor layer having little warpage, little dislocation, and good crystallinity.

[0109] Furthermore, according to the method for producing a nitride semiconductor substrate of the present invention, it is possible to produce a nitride semiconductor substrate including a Group III nitride semiconductor layer having little warpage, little dislocation, and good crystallinity. BRIEF DESCRIPTION OF THE DRAWINGS

[0110] Figure 1 Schematic cross-sectional view showing an example of the nitride semiconductor substrate of the present invention.

[0111] Figure 2 This is a partial flow chart of a first embodiment of a method for manufacturing a nitride semiconductor substrate according to the present invention.

[0112] Figure 3 This is a schematic cross-sectional view of an initial support substrate used in the first embodiment of the method for producing a nitride semiconductor substrate of the present invention.

[0113] Figure 4 This is a partial flow chart of a first embodiment of a method for manufacturing a nitride semiconductor substrate according to the present invention.

[0114] Figure 5 This is a partial flow chart of a first embodiment of a method for manufacturing a nitride semiconductor substrate according to the present invention.

[0115] Figure 6 This is a partial flow chart of a first embodiment of a method for manufacturing a nitride semiconductor substrate according to the present invention.

[0116] Figure 7 This is a partial flow chart of a second embodiment of the method for manufacturing a nitride semiconductor substrate of the present invention.

[0117] Figure 8 This is a partial flow chart of a second embodiment of the method for manufacturing a nitride semiconductor substrate of the present invention.

[0118] Fig. 9 This is a partial flow chart of a second embodiment of the method for manufacturing a nitride semiconductor substrate of the present invention.

[0119] Fig.10 It is a schematic cross-sectional view showing another example of the nitride semiconductor substrate of the present invention.

[0120] Fig.11 It is a schematic cross-sectional view showing another example of the nitride semiconductor substrate of the present invention. DETAILED DESCRIPTION

[0121] As described above, there is a need to develop a nitride semiconductor substrate including a Group III nitride semiconductor layer having little warpage, little dislocation, and good crystallinity, and a method for producing the same.

[0122] The inventors of the present application have conducted in-depth research on the above-mentioned problems, and found that if it is a nitride semiconductor substrate comprising a composite substrate, a group III nitride semiconductor seed layer and a group III nitride semiconductor layer, and the group III nitride semiconductor seed layer is bonded to the composite substrate via a planarization film and the crystallinity of the (0002) growth plane of GaN is less than 550 arc seconds in terms of XRD half-peak width, and the group III nitride semiconductor layer is formed on the group III nitride semiconductor seed layer, then it is possible to have a group III nitride semiconductor layer with extremely low dislocation density and good crystallinity, and a nitride semiconductor substrate with less warping can be made, thereby completing the present invention.

[0123] That is, the present invention is a nitride semiconductor substrate having a group III nitride semiconductor layer containing GaN formed on a support substrate, characterized in that:

[0124] The supporting substrate comprises:

[0125] A composite substrate, which is formed by stacking a plurality of layers, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer stacked on the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer; and,

[0126] A group III nitride semiconductor seed layer, which is bonded to the composite substrate via a planarization layer and contains at least GaN;

[0127] The III-nitride semiconductor layer is formed on the III-nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the III-nitride semiconductor seed crystal layer is less than 550 arc seconds (arcsec) in terms of XRD half-peak width.

[0128] Furthermore, the present invention is a nitride semiconductor substrate in which a Group III nitride semiconductor layer containing GaN is formed on a supporting substrate, wherein:

[0129] The supporting substrate comprises:

[0130] A composite substrate, which is stacked with a plurality of layers, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a barrier layer bonded to the entire first adhesive layer, a second adhesive layer bonded to the back side of the barrier layer, and a conductive layer bonded to the back side of the second adhesive layer; and,

[0131] A group III nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer bonded only to a surface of the composite substrate and comprising at least GaN;

[0132] The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

[0133] Furthermore, the present invention is a nitride semiconductor substrate in which a Group III nitride semiconductor layer containing GaN is formed on a supporting substrate, wherein:

[0134] The supporting substrate comprises:

[0135] A composite substrate, which is formed by stacking a plurality of layers, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a conductive layer bonded to the back side of the first adhesive layer, a second adhesive layer bonded to the back side of the conductive layer, and a barrier layer bonded to the surface and side of the first adhesive layer, the side of the conductive layer, and the side and back of the second adhesive layer; and,

[0136] A group III nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer bonded only to a surface of the composite substrate and comprising at least GaN;

[0137] The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

[0138] In addition, the present invention is a method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that the method comprises the following steps:

[0139] Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer;

[0140] Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width;

[0141] Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer;

[0142] Step (4), wherein a composite substrate formed by stacking a plurality of layers is prepared as a composite substrate different from the initial composite substrate, and a planarization layer is stacked on the composite substrate, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer stacked on the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer;

[0143] Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate;

[0144] Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate;

[0145] Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and

[0146] Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

[0147] In addition, the present invention is a method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that the method comprises the following steps:

[0148] Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer;

[0149] Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width;

[0150] Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer;

[0151] Step (4), wherein, as a composite substrate different from the initial composite substrate, a composite substrate formed by stacking a plurality of layers is prepared, and a planarization layer is stacked only on a surface of the composite substrate, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a barrier layer bonded to the entire first adhesive layer, a second adhesive layer bonded to the back surface of the barrier layer, and a conductive layer bonded to the back surface of the second adhesive layer;

[0152] Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate;

[0153] Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate;

[0154] Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and

[0155] Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

[0156] In addition, the present invention is a method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that the method comprises the following steps:

[0157] Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer;

[0158] Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width;

[0159] Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer;

[0160] Step (4), wherein, as a composite substrate different from the initial composite substrate, a composite substrate formed by stacking a plurality of layers is prepared, and a planarization layer is stacked only on a surface of the composite substrate, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a conductive layer bonded to the back surface of the first adhesive layer, a second adhesive layer bonded to the back surface of the conductive layer, and a barrier layer bonded to the surface and side surface of the first adhesive layer, the side surface of the conductive layer, and the side surface and back surface of the second adhesive layer;

[0161] Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate;

[0162] Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate;

[0163] Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and

[0164] Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

[0165] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings, but the present invention is not limited thereto.

[0166] [Nitride semiconductor substrate]

[0167] Figure 1 A schematic cross-sectional view of an example of the nitride semiconductor substrate of the present invention is shown in FIG.

[0168] Figure 1 The nitride semiconductor substrate 100 shown includes a support substrate 10 and a group III nitride semiconductor layer 20 formed on the support substrate 10 .

[0169] The support substrate 10 includes a composite substrate 6 and a group III nitride semiconductor seed crystal layer 8 bonded to the composite substrate 6 via a planarization film 7 .

[0170] The composite substrate 6 is stacked with a plurality of layers, the plurality of layers including a polycrystalline ceramic core 1, a first adhesive layer 2 bonded to the entire polycrystalline ceramic core 1, a second adhesive layer 4 stacked on the entire first adhesive layer 2, and a barrier layer 5 bonded to the entire second adhesive layer 4. Figure 1 In the illustrated example, the composite substrate 6 further has a conductive layer 3 as an arbitrary layer between the first adhesive layer 2 and the second adhesive layer 4 and is laminated on the entire first adhesive layer 2 .

[0171] exist Figure 1 In the illustrated example, the group III nitride semiconductor seed crystal layer 8 is bonded to only one side of the composite substrate 6 via the planarization layer 7 .

[0172] The group III nitride semiconductor seed crystal layer 8 contains at least GaN. The crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer 8 is 550 arc seconds or less in terms of the half-width of the XRD (X-ray Diffraction) peak.

[0173] The group III nitride semiconductor layer 20 is formed on the group III nitride semiconductor seed crystal layer 8. The group III nitride semiconductor layer 20 contains GaN.

[0174] In the nitride semiconductor substrate 100 of the present invention, the III-nitride semiconductor layer 20 is epitaxially formed on the III-nitride semiconductor seed layer 8 whose crystallinity of the (0002) growth plane of GaN of the seed crystal is 550 arc seconds or less in terms of XRD half-peak width, and thus, a dislocation density is extremely low and good crystallinity can be exhibited. As a result, in the nitride semiconductor substrate 100 of the present invention, the characteristics of the device can be improved.

[0175] In addition, the nitride semiconductor substrate 100 of the present invention includes the support substrate 10 as described above, and the support substrate 10 includes the composite substrate 6 in which a plurality of layers are stacked, so that the warping of the III-nitride semiconductor layer 8 caused by the difference in thermal expansion coefficient during epitaxial growth can be reduced, and thus the III-nitride semiconductor layer 20 having no cracks and a large thickness can be provided. Therefore, the III-nitride semiconductor layer 20 can be finally peeled off from the support substrate 10 and used as an independent substrate.

[0176] The following, Figure 1 The nitride semiconductor substrate 100 shown will be described in more detail.

[0177] The polycrystalline ceramic core 1 may include, for example, aluminum nitride. If the polycrystalline ceramic core 1 includes aluminum nitride, the difference in thermal expansion coefficient can be minimized.

[0178] Such a polycrystalline ceramic core 1 can be sintered at a high temperature of, for example, 1800° C. using a sintering aid to have a thickness of about 600 to 1150 μm. Basically, it is often formed with a thickness in accordance with the SEMI (Semiconductor Equipment and Materials International) standard for silicon substrates.

[0179] The first adhesive layer 2 and the second adhesive layer 4 may be, for example, a tetraethyl silicate (TEOS) layer or a silicon oxide (SiO2) layer, or a layer containing both. The first adhesive layer 2 and the second adhesive layer 4 are deposited by a LPCVD (Low-Pressure Chemical Vapor Deposition) process or a CVD (Chemical Vapor Deposition) process, respectively, and may have a thickness of about 50 to 200 nm.

[0180] The conductive layer 3 includes, for example, polycrystalline silicon and is deposited by an LPCVD process. The conductive layer 3 is a layer for imparting conductivity and may be doped with, for example, boron (B) or phosphorus (P). The conductive layer 3 including polycrystalline silicon may be provided as required, or may not be provided, and may be formed only on one side of the first adhesive layer 2.

[0181] Any conductive layer 3 preferably has a thickness of 50 nm to 500 nm. When the thickness of the conductive layer 3 is within this range, the nitride semiconductor substrate 100 can be formed to include a portion having excellent conductivity while suppressing the occurrence of warping.

[0182] The barrier layer 5 is made of, for example, silicon nitride, and is deposited by an LPCVD process, etc., and has a thickness of about 100 nm to 1500 nm. The barrier layer 5 is a layer that blocks impurities from the inside of a substrate such as ceramics.

[0183] The planarization layer 7 can be deposited by, for example, an LPCVD process or the like, and has a thickness of about 500 nm to 3000 nm. The planarization layer 7 is a layer deposited to planarize the upper surface. As the material of the planarization layer 7, for example, tetraethyl orthosilicate, or silicon oxide (SiO2), aluminum oxide (Al2O3), silicon nitride (Si3N4), or silicon oxynitride (Si x O y N z , where 0 < x < 1, 0 < y < 2, 0 ≤ z ≤ 0.6), and other common ceramic film materials, etc.

[0184] In the nitride semiconductor substrate 100 of the present invention, the crystallinity of the (0002) growth plane of GaN of the seeds in the group III nitride semiconductor seed layer 8 is 550 arcseconds or less in terms of the XRD full width at half maximum. More preferably, the crystallinity of the (0002) growth plane of GaN of the seeds is 300 arcseconds or less in terms of the XRD full width at half maximum. The preferred lower limit value of the XRD full width at half maximum is not particularly limited, and is, for example, 100 arcseconds.

[0185] In addition to GaN, the group III nitride semiconductor seed layer 8 may further contain one or more of AlN and AlGaN.

[0186] Furthermore, the thickness of the group III nitride semiconductor seed layer 8 can be changed according to the use, and thus is not particularly limited. For example, it can be set to 100 nm or more. The upper limit of the thickness of the group III nitride semiconductor seed layer 8 is not particularly limited, and can be set to 1000 nm, for example.

[0187] The group III nitride semiconductor layer 20 contains GaN, but in addition to GaN, it may also contain, for example, one or more of AlN and AlGaN.

[0188] The GaN in the group III nitride semiconductor layer 20 is a material epitaxially grown on the group III nitride semiconductor seed layer 8 having good crystallinity as described above, and thus can exhibit good crystallinity like the GaN of the group III nitride semiconductor seed layer 8. In addition, the group III nitride semiconductor layer 20 can have a thickness of 10 μm or more without cracks.

[0189] Although not shown, in the nitride semiconductor substrate 100 of the present invention, the composite substrate 6 may further have a back conductive layer laminated on the back side surface where the group III nitride semiconductor seed layer 8 is not bonded, instead of the conductive layer 3. The back conductive layer may contain, for example, polysilicon in the same manner as the conductive layer 3, and can be deposited by, for example, an LPCVD process or the like. In addition, the back conductive layer may have a thickness of, for example, 50 nm to 500 nm.

[0190] The nitride semiconductor substrate 100 of the present invention can be manufactured, for example, by the manufacturing method of the nitride semiconductor substrate of the present invention described below by way of example. However, the nitride semiconductor substrate 100 of the present invention can also be manufactured by a method other than the manufacturing method of the nitride semiconductor substrate of the present invention.

[0191] The nitride semiconductor substrate of the present invention can also be used Fig.10 or Fig.11 The composite substrate 10 schematically shown in FIG. 1 serves as a supporting substrate.

[0192] Fig.10 The support substrate 10 shown includes a composite substrate 6 and a III-nitride semiconductor seed layer 8, wherein the III-nitride semiconductor seed layer 8 is bonded to the composite substrate 6 via a planarization layer 7 bonded only to the surface (front side surface) of the composite substrate 6 and includes at least GaN. The composite substrate 6 is a composite substrate 6 having a plurality of layers stacked thereon, wherein the plurality of layers include a polycrystalline ceramic core 1, a first adhesive layer 2 bonded to the entire polycrystalline ceramic core 1, a barrier layer 5 bonded to the entire first adhesive layer 2, a second adhesive layer 4 bonded to the back surface of the barrier layer 5, and a conductive layer 3 bonded to the back surface of the second adhesive layer 4.

[0193] Fig.11 The support substrate 10 shown includes a composite substrate 6 and a III-nitride semiconductor seed layer 8, wherein the III-nitride semiconductor seed layer 8 is bonded to the composite substrate 6 via a planarization layer 7 bonded only to the surface (front side surface) of the composite substrate 6 and includes at least GaN. The composite substrate 6 is a composite substrate 6 having a plurality of layers stacked thereon, wherein the plurality of layers include a polycrystalline ceramic core 1, a first adhesive layer 2 bonded to the entire polycrystalline ceramic core 1, a conductive layer 3 bonded to the back side of the first adhesive layer 2, a second adhesive layer 4 bonded to the back side of the conductive layer 3, and a barrier layer 5 bonded to the surface and side of the first adhesive layer 2, the side of the conductive layer 3, and the side and back of the second adhesive layer 4.

[0194] Fig.10 and Fig.11 The layers of the composite substrate 6 shown may be the same as the layers described above.

[0195] like Fig.10 and Fig.11 The nitride semiconductor substrate 100 shown includes a support substrate 10 having a structure in which a conductive layer 3 is formed only on the back side. Figure 1 In addition to the effects described above, when a high-frequency device is manufactured, no leakage path is generated due to the conductive layer on the surface side of the support substrate 10, and a device with excellent high-frequency characteristics can be manufactured.

[0196] [Method for manufacturing nitride semiconductor substrate]

[0197] Hereinafter, as examples of the method for producing a nitride semiconductor substrate of the present invention, a first embodiment and a second embodiment will be described with reference to the drawings. However, the method for producing a nitride semiconductor substrate of the present invention is not limited to the examples described below.

[0198] (First embodiment)

[0199] Reference Figure 2 to Figure 6 A first embodiment of the method for producing a nitride semiconductor substrate according to the present invention will be described.

[0200] (Step (1): Step of Preparing an Initial Supporting Substrate as a Growth Substrate)

[0201] In step (1), in order to manufacture a Group III nitride semiconductor substrate for bonding, Figure 2 As shown in (a), an initial support substrate 30 is prepared as a growth substrate, wherein a silicon single crystal thin film is bonded to an initial composite substrate 36 via an initial planarizing layer 37 as an initial seed layer 38. The initial support substrate 30 may also be referred to as a GaN support substrate.

[0202] The initial composite substrate 36 may have, for example, Figure 3 The structure of the schematic cross-sectional view is shown in FIG. Figure 3 The initial composite substrate 36 shown is a support structure, which includes a polycrystalline ceramic core 31, a first bonding layer 32 bonded to the entire polycrystalline ceramic core 31, a conductive layer 33 bonded to the entire first bonding layer 32, a second bonding layer 34 bonded to the entire conductive layer 33, and a barrier layer 35 bonded to the entire second bonding layer 34.

[0203] The polycrystalline ceramic core 31, the first adhesive layer 32, the conductive layer 33, the second adhesive layer 34 and the barrier layer 35 can each be the same as the reference Figure 1 The layers of the composite substrate 6 included in the nitride semiconductor substrate 100 of the present invention described above are the same. The initial composite substrate 36 can be manufactured by the method described in the description of the composite substrate 6. In addition, the initial composite substrate 36 may be stacked with a plurality of layers, not limited to Figure 3 For example, the conductive layer 33 and the first adhesive layer 32 may be formed as required, but are not necessarily required to be present, and may be formed only on one side.

[0204] exist Figure 2 (a) and Figure 3 In the example shown, the planarization film 37 is bonded to only one side of the initial composite substrate 36. The planarization film 37 can be provided, for example, with the reference Figure 1 The planarizing film 7 described above is the same planarizing film, but is not limited thereto.

[0205] The silicon single crystal thin film 38 is bonded to the planarization film 37 and may be referred to as a substantial silicon layer. The silicon single crystal thin film 38 has a thickness of, for example, about 50 nm to 1000 nm and is used for epitaxial growth of a group III nitride semiconductor seed crystal layer containing GaN in step (2).

[0206] The silicon single crystal thin film 38 as the initial seed layer is preferably oriented to <111> of silicon single crystal film, but resistivity, etc. are not considered.

[0207] The silicon single crystal thin film 38 can be formed, for example, by laminating the thin film to the planarizing layer 37 in a laminating step and then peeling the thin film off by ion irradiation or the like so as to leave a desired thickness.

[0208] (Step (2): Step of Manufacturing a Group III Nitride Semiconductor Substrate for Bonding)

[0209] Next, as step (2), Figure 2 The process of manufacturing a III-nitride semiconductor substrate 200 for bonding is shown in (b). In this process (2), a III-nitride semiconductor seed layer 8 containing at least GaN is epitaxially grown on an initial support substrate 30 as a growth substrate, more specifically, on a silicon single crystal thin film 38 as an initial seed layer, to manufacture a III-nitride semiconductor substrate 200 for bonding containing a III-nitride semiconductor seed layer 8, wherein the crystallinity of the (0002) growth plane of GaN in the III-nitride semiconductor seed layer 8 is less than 550 arc seconds in terms of XRD half-peak width.

[0210] The step (2) can be performed in, for example, a MOCVD (Metal Organic Chemical Vapor Deposition) reactor.

[0211] In this step (2), epitaxial growth of a III-group nitride semiconductor seed layer (epitaxial layer) 8 such as AlN, AlGaN and GaN is performed on the silicon single crystal thin film 38 of the initial support substrate 30. The structure of the III-group nitride semiconductor seed layer 8 is not limited to this, and also includes a case where no AlGaN film is formed, and a case where AlN film is further formed after AlGaN film formation. In addition, it also includes a case where multiple layers of AlGaN are formed to change the Al composition. On the other hand, in step (2), GaN will inevitably grow. The film thickness can be changed according to the application, so it is not particularly limited.

[0212] During epitaxial growth, trimethylaluminum (TMAl) can be used as an Al source, trimethylgallium (TMGa) can be used as a Ga source, and NH 3 can be used as an N source. In addition, the carrier gas can be N 2 or H 2 , or any of the two gases, and the process temperature can be set to about 900 to 1200°C.

[0213] In step (2), the conditions can be controlled, for example, so that the III-nitride semiconductor seed crystal layer 8 is oriented in the axis direction. <111> A group III nitride semiconductor substrate 200 for bonding comprising a group III nitride semiconductor seed layer 8 is manufactured by epitaxially growing the GaN on a silicon single crystal thin film 38, wherein the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed layer 8 is less than 550 arc seconds in terms of XRD half-peak width, for example, more than 100 arc seconds and less than 550 arc seconds.

[0214] (Step (3): Step of forming a peeling layer on the silicon single crystal thin film by laser irradiation)

[0215] Next, the interface between the silicon single crystal thin film 38 and the group III nitride semiconductor seed crystal layer 8 of the group III nitride semiconductor substrate 200 for bonding manufactured in step (2) is treated as follows: Figure 2 As shown in (c), laser is irradiated to form Figure 4 The peeling layer 38a shown in (d).

[0216] The wavelength of the laser at this time is preferably longer than the wavelength of light equal to the band gap energy of GaN, and shorter than the wavelength of light equal to the band gap energy of silicon single crystal. Specifically, it is preferably about 360nm or more and 1100nm or less. Thus, it is possible to aim at the silicon single crystal thin film 38 to form a peeling layer 38a, thereby suppressing damage to the III-nitride semiconductor seed crystal layer 8 containing GaN. In addition, the light energy (power) of the laser is not particularly limited as long as it can form the peeling layer 38a, but is preferably about 5W to 20W. The pitch of the irradiated laser is preferably set to about 30μm or less. By setting the irradiation pitch to less than 30μm, a peeling layer 38a that can fully perform the peeling in the step (6) described below can be formed.

[0217] By forming a peeling layer (destruction layer) 38a by laser irradiation and performing peeling, the difference in the ease of focusing the laser light between the III-nitride semiconductor seed crystal layer 8 containing GaN and the silicon single crystal can be utilized to form the peeling layer 38a on the silicon single crystal thin film 38 by using the laser light that penetrates the III-nitride semiconductor seed crystal layer 8 containing GaN, thereby suppressing the damage to the III-nitride semiconductor seed crystal layer 8 containing GaN. In addition, the laser light can be focused at a position deeper than the surface, so even when the III-nitride semiconductor seed crystal layer 8 containing GaN is formed into a film of several μm, the peeling layer 38a can be formed near the interface between the silicon single crystal thin film 38 and the III-nitride semiconductor seed crystal layer 8.

[0218] On the other hand, in the method of stripping by ion irradiation such as Smart Cut (registered trademark), the penetration depth is greatly limited. If a III-nitride semiconductor seed layer of more than several μm is formed, most ions will not be able to penetrate and stripping will not be possible. In addition, ion irradiation will cause damage to the crystal.

[0219] (Step (4): a step of preparing a composite substrate different from the initial composite substrate and laminating a planarizing layer on the composite substrate)

[0220] Next, prepare Figure 4 The composite substrate 6 shown below (e) is a supporting base substrate different from the initial composite substrate 36 prepared in step (1).

[0221] The composite substrate 6 prepared in step (4) is the same as the composite substrate included in the nitride semiconductor substrate of the present invention. Figure 1 The composite substrate 6 shown is the same as that shown in the figure, which is a composite substrate 6 stacked with multiple layers, and the multiple layers include: a polycrystalline ceramic core 1, a first bonding layer 2 bonded to the entire polycrystalline ceramic core 1, a second bonding layer 4 stacked on the entire first bonding layer 2, and a barrier layer 5 combined with the entire second bonding layer 4.

[0222] Next, the planarizing layer 7 is stacked on the prepared composite substrate 6 .

[0223] Regarding the method for manufacturing the composite substrate 6 and the planarization layer 7 , reference may be made to the description of the nitride semiconductor of the present invention.

[0224] (Step (5): Step of bonding the planarization layer and the group III nitride semiconductor seed crystal layer to obtain a bonded substrate)

[0225] Then, if Figure 4As shown in (e), the planarization layer 7 stacked on the composite substrate 6 prepared in step (4) is bonded to the III-nitride semiconductor seed layer 8 of the bonding III-nitride semiconductor substrate 200 (with a peeling layer 38a formed on the silicon single crystal thin film 38), thereby obtaining Figure 5 The bonding substrate 300 shown in (f).

[0226] (Step (6): Step of peeling a portion of the growth substrate (initial support substrate) from the bonding substrate)

[0227] Next, in the bonding substrate 300 produced in step (5), Figure 5 The peeling layer 38a shown in (f) is as follows Figure 5 As shown in (g), the silicon single crystal thin film 38 of the III-nitride semiconductor substrate 200 for bonding is divided into a portion 38 b and another portion 38 c , and then a portion of the initial support substrate 30 as a growth substrate is peeled off from the bonding substrate 300 .

[0228] The method for peeling is not particularly limited, but for example, the peeling can be performed by using an adhesive device. Figure 5 The front and back surfaces of the bonding substrate 300 shown in (f) are fixed to jigs, respectively, and a force is applied to the opposite sides to separate and peel the silicon single crystal thin film 38 by the peeling layer 38 a .

[0229] (Step (7): a step of removing the portion of the silicon single crystal thin film remaining on the bonding substrate to obtain a supporting substrate)

[0230] Then, through Figure 6 The peeling surface of the portion 38c of the silicon single crystal thin film remaining on the bonding substrate 300 shown in (h) is polished to remove a portion of the silicon single crystal thin film 38c. Figure 6 As shown in (i), a support substrate 10 is obtained, which includes a composite substrate 6 and a group III nitride semiconductor seed layer 8 as a group III nitride semiconductor seed layer bonded to the composite substrate 6 via a planarization layer 7. Figure 6 As shown in (i), the surface layer of the support substrate 10 is a group III nitride semiconductor seed crystal layer 8 containing GaN.

[0231] Through these steps, a support substrate 10 (GaN support substrate) can be manufactured, which includes a nitride semiconductor seed crystal layer 8 as a surface layer. The nitride semiconductor seed crystal layer 8 includes GaN and the crystallinity of the (0002) growth plane of GaN is 550 arc seconds or less in terms of XRD half-peak width.

[0232] (Step (8): a step of epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the supporting substrate to thereby produce a nitride semiconductor substrate)

[0233] Then, if Figure 6 As shown in (j), the group III nitride semiconductor layer 20 containing GaN is epitaxially grown on the group III nitride semiconductor seed crystal layer 8 of the supporting substrate 10. The conditions for epitaxial film formation can be the same as those in step (2).

[0234] Through the above-described steps (1) to (8), it is possible to produce Figure 6 The nitride semiconductor substrate 100 shown in (j).

[0235] (Second embodiment)

[0236] Next, refer to Figure 7 to Figure 9 A second embodiment of the method for producing a nitride semiconductor substrate according to the present invention will be described.

[0237] The second embodiment uses Figure 7 The present invention is greatly different from the first embodiment in that the silicon single crystal substrate 40 shown in (a) is used as the growth substrate instead of the initial support substrate 30. The differences from the first embodiment will be mainly described below.

[0238] In step (1), as described above, prepare Figure 7 The silicon single crystal substrate 40 shown in (a) is used as a growth substrate.

[0239] The silicon single crystal substrate 40 is preferably oriented in the axis direction <111> Silicon single crystal substrate, but resistivity, etc. are not considered.

[0240] In step (2), in the same manner as in the first embodiment, a group III nitride semiconductor seed crystal layer 8 containing at least GaN is epitaxially grown on a silicon single crystal substrate 40 as a growth substrate to produce a semiconductor device such as the semiconductor device of FIG. Figure 7 The III-nitride semiconductor substrate 200 for bonding shown in (b) includes a III-nitride semiconductor seed layer 8, wherein the crystallinity of the (0002) growth plane of GaN in the III-nitride semiconductor seed layer 8 is less than 550 arc seconds in terms of XRD half-peak width, for example, greater than 100 arc seconds and less than 550 arc seconds.

[0241] In step (3), Figure 7 In the manner shown in (c) of FIG. 1 , a laser is irradiated near the interface between the silicon single crystal substrate 40 as the growth substrate and the group III nitride semiconductor seed crystal layer 8 to form a separation layer. The separation layer can be formed in the same manner as in the first embodiment.

[0242] Step (4) is the same as that of the first embodiment.

[0243] In step (5), the planarization layer 7 stacked on the composite substrate 6 prepared in step (4) is bonded to the group III nitride semiconductor seed crystal layer 8 of the group III nitride semiconductor substrate 200 for bonding (the peeling layer 40a is formed on the silicon single crystal substrate 40), thereby obtaining Figure 8 The bonding substrate 300 shown in (d).

[0244] In step (6), in the bonding substrate 300 produced in step (5), Figure 8 The peeling layer 40a shown in (d) is as follows Figure 8 As shown in (e), the silicon single crystal substrate 40 of the bonding III-nitride semiconductor substrate 200 is divided into a part 40b and another part 40c, and then the part 40b of the silicon single crystal substrate as the growth substrate is peeled off from the bonding substrate 300. The peeling can be performed in the same manner as in the first embodiment.

[0245] In step (7), by Fig. 9 The peeling surface of the portion 40c of the silicon single crystal thin film remaining on the bonding substrate 300 shown in (f) is polished to remove the portion 40c of the silicon single crystal thin film. Fig. 9 The supporting substrate 10 shown in (g) includes a composite substrate 6 and a group III nitride semiconductor seed layer 8 as a group III nitride semiconductor seed layer bonded to the composite substrate 6 via a planarization layer 7. Fig. 9 As shown in (g), the surface layer of the support substrate 10 is a group III nitride semiconductor seed crystal layer 8 containing GaN.

[0246] Step (8) is the same as in the first embodiment.

[0247] Through the above-described steps (1) to (8), it is possible to produce Fig. 9 The nitride semiconductor substrate 100 shown in (h).

[0248] In the method for manufacturing a nitride semiconductor substrate of the present invention described above by taking an example, since the lattice constant difference between the III-nitride semiconductor layer (e.g., GaN epitaxial layer) 20 containing GaN and the supporting substrate 10 can be made extremely small, it is possible to form a III-nitride semiconductor layer 20 containing GaN with less dislocation and good crystallinity. In addition, by repeating this method, a III-nitride semiconductor layer 20 with even less dislocation can be formed.

[0249] In addition, the III-nitride semiconductor layer 20 formed by this method can be stacked thicker due to less dislocation. In addition, since the support substrate 10 including the composite substrate 6 stacked with a plurality of layers is used as the support substrate, the warping of the III-nitride semiconductor layer 20 during growth due to the difference in thermal expansion coefficient can be reduced, so that the III-nitride semiconductor layer 20 without cracks and with a large thickness can be formed. Therefore, the III-nitride semiconductor layer 20 can be finally peeled off from the support substrate 10 and used as an independent substrate.

[0250] On the other hand, in the past, even if a III-nitride semiconductor seed crystal containing GaN was formed on a composite substrate stacked with multiple layers, it was still impossible to make the lattice constant appropriate, and thus it was impossible to form a III-nitride semiconductor seed crystal layer in which the crystallinity of the GaN (0002) growth plane was less than 550 arc seconds in terms of XRD half-peak width.

[0251] Furthermore, in the first embodiment, if Figure 5 As shown in (g), since the initial support substrate 30 is peeled off from the bonding substrate 300 by dividing the silicon single crystal thin film 38, the substrate obtained by bonding the silicon single crystal to the surface of the peeled initial support substrate 30 can be reused as the initial support substrate, thereby achieving the advantage of cost reduction. It is also possible to remove a portion 38b of the silicon single crystal thin film 8 remaining on the surface as needed, and bond the silicon single crystal after SiO2 film formation. In the case of removal through a back ground, etc., the substrate cannot be reused.

[0252] Alternatively, as the composite substrate 6 prepared in step (4), the following may be prepared: Fig.10 or Fig.11 The composite substrate 6 shown is used instead of Figure 1 The composite substrate 6 shown in the figure has a planarization layer 7 laminated only on the surface (front surface) of the composite substrate 6 .

[0253] In the method for manufacturing a nitride semiconductor substrate of this modified example, a leakage path caused by the conductive layer on the surface side of the support substrate is not generated, and a nitride semiconductor substrate excellent in high-frequency characteristics can be manufactured.

[0254] In addition, as the initial composite substrate 36, the Figure 3 The example of the structure shown is described, but the structure of the initial composite substrate is not limited to Figure 3 , for example, it can also be Fig.10 or Fig.11 The composite substrate 6 shown has the same structure.

[0255] Example

[0256] Hereinafter, the present invention will be specifically described using Examples and Comparative Examples, but the present invention is not limited to these Examples and Comparative Examples.

[0257] (Example 1)

[0258] In Example 1, using Figure 2 and Figures 4 to 6 The nitride semiconductor substrate is manufactured by the manufacturing flow of the first embodiment shown.

[0259] (Process (1))

[0260] First, create a previous reference Figure 2 (a) and Figure 3 The initial support substrate (GaN support substrate) 30 described above serves as a growth substrate.

[0261] In step (1), the axis is oriented to <111> The silicon single crystal is attached to the planarization layer 37 and then peeled off by ion irradiation in such a way that the thickness remains, thereby forming a silicon single crystal thin film 38.

[0262] (Process (2))

[0263] The initial support substrate 30 is placed in an MOCVD reactor, and epitaxial growth of a III-group nitride semiconductor seed layer including AlN, AlGaN, and GaN is performed on the initial support substrate 30. The initial support substrate 30 is placed in a wafer pocket called a satellite tray. During epitaxial growth, TMAl is used as an Al source, TMGa is used as a Ga source, and NH3 is used as an N source.

[0264] In addition, either N2 or H2 was used as the carrier gas, and the process temperature was set to 1200°C.

[0265] In step (2), when the GaN support substrate is placed on a satellite tray for epitaxial growth, the epitaxial layer is formed in order of AlN and AlGaN from the substrate side toward the growth direction, and then GaN is epitaxially grown.

[0266] Therefore, if Figure 2 As shown in (b), a III-nitride semiconductor seed layer (epitaxial layer) 8 is formed on the silicon single crystal thin film 38 of the initial support substrate 30, thereby manufacturing a III-nitride semiconductor substrate for bonding (GaN on GaN support substrate) 200. The total film thickness of the III-nitride semiconductor seed layer (epitaxial layer) 8 is 1 μm.

[0267] (Process (3))

[0268] Then, if Figure 2As shown in (c), the vicinity of the interface between the silicon single crystal thin film 38 of the group III nitride semiconductor substrate 200 for bonding produced in step (2) and the group III nitride semiconductor seed crystal layer (epitaxial layer) 8 is irradiated with laser light.

[0269] The wavelength of the laser at this time is 1064nm, and the irradiation interval is 5μm. In addition, the light energy of the laser is 12W. Through this step (3), Figure 4 The peeling layer 38a shown in (d).

[0270] (Process (4))

[0271] Prepare Figure 4 The composite substrate 6 as a supporting base substrate shown below (e) is different from the initial composite substrate 36 prepared in step (1). In addition, a planarization layer 7 is stacked on the composite substrate 6. The composite substrate 6 and the planarization layer 7 are produced by a method in which the process of bonding the surface layer silicon single crystal thin film 38 is not performed in the method of producing the initial supporting substrate 30 in step (1).

[0272] (Process (5))

[0273] Then, if Figure 4 As shown in (e), the III-nitride semiconductor substrate 200 for bonding produced in steps (1) to (3) is attached to the planarization layer 7 formed on the composite substrate 6 to obtain Figure 5 The bonding substrate 300 shown in (f) is shown in FIG. The bonding step is performed at room temperature.

[0274] (Process (6))

[0275] In the bonding substrate 300 produced in step (5), Figure 5 The peeling layer 38a shown in (f) is used to bond the silicon single crystal thin film 38 of the III-nitride semiconductor substrate 200. Figure 5 As shown in (g), the silicon single crystal thin film 38 is divided into a part 38b and another part 38c, and a part of the initial support substrate 30 as the growth substrate is peeled off from the bonding substrate 300. The upper and lower parts of the bonding substrate 300 are fixed to a clamp, and an external force in the opposite direction is applied, thereby dividing the silicon single crystal thin film 38 at the peeling layer.

[0276] (Process (7))

[0277] After the peeling in step (6), Figure 6 As shown in (h), a portion 38c of the silicon single crystal thin film remaining on the surface of the bonding substrate 300 is polished. The silicon single crystal thin film is completely removed by polishing by about 100nm. Figure 6As shown in (i), a supporting substrate 10 is obtained, which includes a composite substrate 6 and a group III nitride semiconductor seed crystal layer 8 bonded to the composite substrate 6 via a planarization layer 7 .

[0278] The crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer 8 on the surface of the support substrate 10 was 540 arc seconds in terms of the XRD half-peak width.

[0279] (Process (8))

[0280] On the supporting substrate 10 manufactured up to step (7), as Figure 6 As shown in (j), a GaN layer is epitaxially grown as a group III nitride semiconductor layer 20. The epitaxial growth conditions at this time are the same as those in step (2) except for the film thickness. The GaN layer 20 is formed in such a manner that the film thickness is 5 μm in total with the GaN layer already present in the group III nitride semiconductor seed crystal layer 8. Thus, a film such as Figure 6 (j) shows the nitride semiconductor substrate 100 of Example 1.

[0281] Then, the crystallinity of GaN contained in the GaN layer 20 was measured. As a result, the crystallinity of the (0002) growth plane of GaN was 250 arc seconds in terms of the XRD half-peak width.

[0282] Furthermore, the GaN layer 20 does not contain cracks.

[0283] (Example 2)

[0284] In Example 2, by Figure 7 to Figure 9 The nitride semiconductor substrate is manufactured according to the manufacturing flow of the second embodiment shown.

[0285] (Process (1))

[0286] First, prepare the growth substrate Figure 7 The silicon single crystal substrate 40 shown in (a) is oriented in the axis direction of <111> .

[0287] (Process (2))

[0288] The silicon single crystal substrate 40 is placed in an MOCVD reactor, and epitaxial growth of a III-group nitride semiconductor seed layer including AlN, AlGaN, and GaN is performed on the silicon single crystal substrate 40. The silicon single crystal substrate 40 is placed in a wafer carrier called a satellite tray. During epitaxial growth, TMAl is used as an Al source, TMGa is used as a Ga source, and NH3 is used as an N source.

[0289] In addition, either N2 or H2 is used as the carrier gas, and the process temperature is 1200°C.

[0290] In step (2), when the GaN support substrate is placed on a satellite tray for epitaxial growth, the epitaxial layer is formed in order of AlN and AlGaN from the substrate side toward the growth direction, and then GaN is epitaxially grown.

[0291] Therefore, if Figure 7 As shown in (b), a III-nitride semiconductor seed layer (epitaxial layer) 8 is formed on a silicon single crystal substrate 40 to produce a bonding III-nitride semiconductor substrate (GaN on Si substrate) 200. The total film thickness of the III-nitride semiconductor seed layer (epitaxial layer) 8 is 1 μm.

[0292] (Process (3))

[0293] Then, if Figure 7 As shown in (c), the vicinity of the interface between the silicon single crystal substrate 40 of the group III nitride semiconductor substrate 200 for bonding produced in step (2) and the group III nitride semiconductor seed crystal layer (epitaxial layer) 8 is irradiated with laser light.

[0294] The wavelength of the laser light at this time was 1064 nm, and the irradiation pitch was 5 μm. The optical energy of the laser light was 12 W. Through this step (3), a separation layer was formed on the silicon single crystal substrate 40 .

[0295] (Process (4))

[0296] In the same manner as step (4) of Example 1, a composite substrate 6 and a planarizing layer 7 are produced.

[0297] (Process (5))

[0298] Next, the III-nitride semiconductor substrate 200 for bonding produced in steps (1) to (3) is bonded onto the planarized layer 7 formed on the composite substrate 6 produced in step (4), thereby obtaining Figure 8 The bonding substrate 300 shown in (d) is shown in FIG. The bonding step is performed at room temperature.

[0299] The subsequent steps (6) to (8) are the same as those in Example 1.

[0300] The crystallinity of the GaN (0002) growth plane of the Group III nitride semiconductor seed crystal layer 8 on the surface layer of the support substrate 10 obtained in step (7) was 540 arc seconds in terms of the XRD half-peak width.

[0301] In addition, the following is measured: Fig. 9 The crystallinity of GaN in the GaN layer 20 as the surface layer of the nitride semiconductor substrate 100 shown in (h) showed that the crystallinity of the (0002) growth plane of GaN was 450 arc seconds in terms of the XRD half-peak width.

[0302] Furthermore, the GaN layer 20 does not contain cracks.

[0303] (Comparative Example)

[0304] In the comparative example, in step (2) of Example 1, a GaN layer was formed to a total film thickness of 5 μm to produce a GaN-on-GaN supporting substrate. This supporting substrate was used as a nitride semiconductor substrate in the comparative example.

[0305] The crystallinity of GaN in the surface layer of the nitride semiconductor substrate of the comparative example was measured. As a result, the crystallinity of the (0002) growth plane of GaN was 600 arc seconds in terms of the XRD half-peak width.

[0306] From the above results, it can be seen that the III-nitride semiconductor layer 20 serving as the surface layer of the nitride semiconductor substrate 100 of Examples 1 and 2 of the present invention can suppress the generation of dislocations, and the crystallinity of the (0002) growth plane of GaN is less than 550 arc seconds in terms of the XRD half-peak width, which is better than the crystallinity of the GaN in the surface layer of the nitride semiconductor substrate of the comparison example.

[0307] Furthermore, it was confirmed that no warping occurred in the Group III nitride semiconductor layer 20 as the surface layer of the nitride semiconductor substrate 100 of Examples 1 and 2.

[0308] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any embodiments having substantially the same configuration and exhibiting the same functions and effects as the technical concept described in the claims of the present invention are all within the technical scope of the present invention.

Claims

1. A nitride semiconductor substrate, wherein a group III nitride semiconductor layer including GaN is formed on a support substrate, wherein: The supporting substrate comprises: A composite substrate, which is formed by stacking a plurality of layers, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer stacked on the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer; and, A group III nitride semiconductor seed layer, which is bonded to the composite substrate via a planarization layer and contains at least GaN; The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

2. A nitride semiconductor substrate, wherein a group III nitride semiconductor layer including GaN is formed on a support substrate, characterized in that: The supporting substrate comprises: A composite substrate, which is stacked with a plurality of layers, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a barrier layer bonded to the entire first adhesive layer, a second adhesive layer bonded to the back side of the barrier layer, and a conductive layer bonded to the back side of the second adhesive layer; and, A group III nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer bonded only to a surface of the composite substrate and comprising at least GaN; The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

3. A nitride semiconductor substrate, wherein a group III nitride semiconductor layer including GaN is formed on a support substrate, characterized in that: The supporting substrate comprises: A composite substrate, which is formed by stacking a plurality of layers, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a conductive layer bonded to the back side of the first adhesive layer, a second adhesive layer bonded to the back side of the conductive layer, and a barrier layer bonded to the surface and side of the first adhesive layer, the side of the conductive layer, and the side and back of the second adhesive layer; and, A group III nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer bonded only to a surface of the composite substrate and comprising at least GaN; The group III nitride semiconductor layer is formed on the group III nitride semiconductor seed crystal layer, and the crystallinity of the GaN (0002) growth plane of the group III nitride semiconductor seed crystal layer is less than 550 arc seconds in terms of XRD half-peak width.

4. The nitride semiconductor substrate according to any one of claims 1 to 3, characterized in that The group III nitride semiconductor layer includes at least one of AlN and AlGaN in addition to GaN.

5. The nitride semiconductor substrate according to any one of claims 1 to 4, characterized in that The polycrystalline ceramic core includes aluminum nitride.

6. The nitride semiconductor substrate according to any one of claims 1 to 5, characterized in that The first adhesive layer and the second adhesive layer respectively include tetraethyl silicate and / or silicon oxide, and the barrier layer includes silicon nitride.

7. The nitride semiconductor substrate according to any one of claims 1 to 6, wherein The first adhesive layer and the second adhesive layer have a thickness of 50 to 200 nm respectively, and the barrier layer has a thickness of 100 to 1500 nm.

8. The nitride semiconductor substrate according to any one of claims 1 to 7, wherein The planarization layer includes at least one selected from the group consisting of tetraethyl silicate, silicon oxide, aluminum oxide, silicon nitride, and silicon oxynitride, and has a thickness of 500 nm to 3000 nm.

9. The nitride semiconductor substrate according to any one of claims 1 to 8, wherein The group III nitride semiconductor seed crystal layer has a thickness of 100 nm or more.

10. The nitride semiconductor substrate according to claim 1, wherein: The composite substrate further includes a conductive layer laminated on the entire first adhesive layer or laminated on one side of the first adhesive layer between the first adhesive layer and the second adhesive layer.

11. The nitride semiconductor substrate according to claim 10, wherein: The conductive layer has a thickness of 50 nm to 500 nm.

12. The nitride semiconductor substrate according to any one of claims 1, 10 and 11, wherein: The composite substrate further includes a back surface conductive layer stacked on the back surface side surface to which the Group III nitride semiconductor seed crystal layer is not bonded.

13. A method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that: The process includes the following steps: Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer; Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width; Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer; Step (4), wherein a composite substrate formed by stacking a plurality of layers is prepared as a composite substrate different from the initial composite substrate, and a planarization layer is stacked on the composite substrate, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a second adhesive layer stacked on the entire first adhesive layer, and a barrier layer bonded to the entire second adhesive layer; Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate; Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate; Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

14. The method for manufacturing a nitride semiconductor substrate according to claim 13, wherein: In step (4), a substrate further including a conductive layer laminated on the entire first adhesive layer or laminated on one side of the first adhesive layer between the first adhesive layer and the second adhesive layer is prepared as the composite substrate.

15. A method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that: The process includes the following steps: Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer; Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width; Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer; Step (4), wherein, as a composite substrate different from the initial composite substrate, a composite substrate formed by stacking a plurality of layers is prepared, and a planarization layer is stacked only on a surface of the composite substrate, the plurality of layers comprising a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a barrier layer bonded to the entire first adhesive layer, a second adhesive layer bonded to the back surface of the barrier layer, and a conductive layer bonded to the back surface of the second adhesive layer; Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate; Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate; Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

16. A method for manufacturing a nitride semiconductor substrate, comprising epitaxially growing a group III nitride semiconductor layer on a group III nitride semiconductor seed layer containing at least GaN, characterized in that: The process includes the following steps: Step (1), wherein, in order to manufacture a Group III nitride semiconductor substrate for bonding, a silicon single crystal substrate or an initial support substrate is prepared as a growth substrate, wherein the initial support substrate is formed by bonding a silicon single crystal thin film as an initial seed layer to an initial composite substrate having a plurality of layers stacked thereon via an initial planarizing layer; Step (2), wherein a group III nitride semiconductor substrate for bonding comprising the group III nitride semiconductor seed crystal layer is manufactured by epitaxially growing a group III nitride semiconductor seed crystal layer comprising at least GaN on the growth substrate, wherein the crystallinity of the (0002) growth plane of GaN in the group III nitride semiconductor seed crystal layer is 550 arc seconds or less in terms of XRD half-peak width; Step (3), irradiating the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate with the vicinity of the interface between the group III nitride semiconductor seed crystal layer and a laser beam to form a peeling layer; Step (4), wherein, as a composite substrate different from the initial composite substrate, a composite substrate formed by stacking a plurality of layers is prepared, and a planarization layer is stacked only on a surface of the composite substrate, wherein the plurality of layers include a polycrystalline ceramic core, a first adhesive layer bonded to the entire polycrystalline ceramic core, a conductive layer bonded to the back surface of the first adhesive layer, a second adhesive layer bonded to the back surface of the conductive layer, and a barrier layer bonded to the surface and side surface of the first adhesive layer, the side surface of the conductive layer, and the side surface and back surface of the second adhesive layer; Step (5), wherein the planarization layer stacked on the composite substrate prepared in step (4) is bonded to the Group III nitride semiconductor seed crystal layer of the Group III nitride semiconductor substrate for bonding to obtain a bonding substrate; Step (6), wherein the silicon single crystal substrate or the silicon single crystal thin film of the bonding group III nitride semiconductor substrate is separated at the peeling layer, and a portion of the growth substrate is peeled off from the bonding substrate; Step (7), wherein the portion of the silicon single crystal substrate or the silicon single crystal thin film remaining on the bonding substrate is removed by polishing the peeling surface, thereby obtaining a supporting substrate comprising the composite substrate and the III-nitride semiconductor seed crystal layer bonded to the composite substrate via a planarization layer; and Step (8) includes epitaxially growing a Group III nitride semiconductor layer containing GaN on the Group III nitride semiconductor seed crystal layer of the support substrate to produce a nitride semiconductor substrate.

17. The method for manufacturing a nitride semiconductor substrate according to any one of claims 13 to 16, wherein: The wavelength of the laser light used in step (3) is 360 nm to 1100 nm.