Optical laminate with surface protective film and method for producing same

By using a dual surface protective film on the optical laminate, the precision defect inspection and surface protection of the optical laminate in VR goggles is solved, the defect detection and surface integrity in the early stage of assembly is ensured, and the quality of the product is improved. reliability.

CN118901035APending Publication Date: 2024-11-05NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027307.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-28
Filing Date
2023-03-07
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art is difficult to realize precise defect inspection of optical laminated bodies in VR goggles, while ensuring protection of the surface of the optical laminated body, especially in the need to prevent damage in the early stage of assembly.

Method used

An optical laminated body design is adopted with a double surface protective film, wherein the first surface protective film has low haze and excellent adhesive layer characteristics, which can protect the surface of the optical laminate before and after defect inspection, and pass a specific adhesive The layer and release liner structure prevent misdetecting.

Benefits of technology

It realizes precision defect inspection of the optical laminated body in the early stage of assembly to prevent damage, and ensures the integrity of the surface of the optical laminated body after the defect inspection, improving the quality and reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901035A_ABST
    Figure CN118901035A_ABST
Patent Text Reader

Abstract

The main purpose of the present invention is to provide an optical laminate which can be applied to VR goggles and which can achieve both surface protection and precision inspection of defects. According to the present invention, provided is an optical laminate with a surface protective film, comprising: an optical laminate including at least one optical member to be used in goggles with a display; and a first surface protective film and a second surface protective film which are sequentially bonded to one surface of the optical laminate toward the outside.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical laminate with a surface protection film and a method for producing the same. Background Art

[0002] Image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices) are rapidly becoming popular. In image display devices, optical components such as polarization components and phase difference components are generally used to realize image display and improve image display performance (e.g., refer to Patent Document 1).

[0003] In recent years, new uses of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing Virtual Reality (VR) have begun to be commercialized. In VR goggles, since the image displayed on the display panel is magnified for visual recognition by the viewer, stricter defect management is required for optical laminates used in VR goggles than for optical laminates used in existing image display devices.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-103286 Summary of the invention

[0007] Problems to be solved by the invention

[0008] As described above, strict defect management is required for the optical laminate used in VR goggles, and therefore, a precision defect inspection capable of detecting even minute defects is performed. On the other hand, it is preferred that the surface of the optical laminate is protected until the final assembly process. Therefore, the main purpose of the present invention is to provide an optical laminate that can be applied to VR goggles and that can take into account both surface protection and precision defect inspection.

[0009] Solutions to the problem

[0010] According to one aspect of the present invention, there are provided an optical laminate with a surface protection film according to [1] to [9], a method for producing an optical laminate with a surface protection film according to

[10] , and a method for producing a display system according to

[11] .

[0011] [1] An optical laminate with a surface protection film, comprising:

[0012] An optical laminate including at least one optical member used for goggles with a display; and

[0013] A first surface protective film and a second surface protective film are sequentially bonded to one surface of the optical layered body toward the outside.

[0014] [2] The optical laminate with a surface protection film according to [1], wherein

[0015] The haze of the first surface protection film is less than 5%.

[0016] [3] The optical layered body with a surface protection film according to [1] or [2], wherein the surface protection film described below is bonded to the optical layered body as the first surface protection film.

[0017] The above-mentioned first surface protection film has a first substrate and a first adhesive layer laminated on the first substrate. The absolute value of the maximum valley depth (Sv) of the surface of the first adhesive layer on the opposite side of the first substrate is less than 500nm. When the first substrate is observed under a microscope, in an observation area of ​​100μm×100μm, the number of defects with a maximum Feret diameter of more than 10μm is less than 3.

[0018] [4] The optical laminate with a surface protection film according to [3], wherein

[0019] The absolute value of the arithmetic mean height (Sa) of the surface of the first pressure-sensitive adhesive layer on the opposite side to the first substrate is 25 nm or less.

[0020] [5] The optical layered body with a surface protection film according to [1] or [2], wherein the surface protection film described below is bonded to the optical layered body as the first surface protection film.

[0021] The surface protection film comprises a first substrate and a first adhesive layer laminated on the first substrate, wherein the surface of the first adhesive layer opposite to the first substrate satisfies the following formula (1):

[0022] [Mathematical formula 1]

[0023]

[0024] (In formula (1), S represents the measurement field area of ​​the white light interferometer in the surface shape evaluation test described below; B-BA represents the area of ​​the black area in the two-dimensional image before binarization obtained in the surface shape evaluation test described below; A-WA represents the area of ​​the white area in the two-dimensional image after binarization obtained in the surface shape evaluation test described below.)

[0025] <Surface shape evaluation test>

[0026] Measuring the surface of the first adhesive layer opposite to the first substrate using a white light interferometer;

[0027] For the obtained interference data, the measurement surface is calculated in the analysis range of -1000nm to -2000nm through frequency domain analysis, and a two-dimensional image is obtained in which the corresponding part becomes a black area;

[0028] Then, the two-dimensional image was subjected to binarization analysis of the measurement surface using -100 nm as a threshold value, and a binarized image was obtained in which the portion below -100 nm was a white area.

[0029] [6] The optical laminate with a surface protection film according to [5], wherein

[0030] When the first substrate is observed under a microscope, the number of defects having a maximum Feret diameter of 10 μm or more is less than 3 in an observation area of ​​100 μm×100 μm.

[0031] [7] The optical laminate with a surface protection film according to any one of [1] to [6], wherein

[0032] The optical layered body includes a polarizing member, a first phase difference member, and a protective member facing the first surface protective film.

[0033] [8] The optical laminate with a surface protection film according to [7], wherein

[0034] The protection member includes a surface treatment layer, and the first surface protection film is bonded to the surface treatment layer.

[0035] [9] The optical laminate with a surface protection film according to any one of [1] to [8], wherein

[0036] The optical layered body has a pressure-sensitive adhesive layer on a surface opposite to the side on which the first surface protection film and the second surface protection film are bonded.

[0037]

[10] A method for producing an optical laminate with a surface protection film, the method comprising:

[0038] A first surface protection film and a second surface protection film are bonded to one surface of an optical layered body having at least one optical member.

[0039] The first surface protection film is selected from (i) and (ii):

[0040] (i) a surface protective film comprising a first substrate and a first adhesive layer laminated on the first substrate, wherein the absolute value of the maximum valley depth (Sv) of the surface of the first adhesive layer on the side opposite to the first substrate is 500 nm or less, and when the first substrate is observed under a microscope, the number of defects with a maximum Feret diameter of 10 μm or more in an observation area of ​​100 μm×100 μm is less than 3;

[0041] (ii) a surface protective film comprising a first substrate and a first adhesive layer laminated on the first substrate, wherein the surface of the first adhesive layer opposite to the first substrate satisfies the following formula (1),

[0042] [Mathematical formula 2]

[0043]

[0044] (In formula (1), S represents the measurement field area of ​​the white light interferometer in the surface shape evaluation test described below; B-BA represents the area of ​​the black area in the two-dimensional image before binarization obtained in the surface shape evaluation test described below; A-WA represents the area of ​​the white area in the two-dimensional image after binarization obtained in the surface shape evaluation test described below.)

[0045] <Surface shape evaluation test>

[0046] Measuring the surface of the first adhesive layer opposite to the first substrate using a white light interferometer;

[0047] For the obtained interference data, the measurement surface is calculated in the analysis range of -1000nm to -2000nm through frequency domain analysis, and a two-dimensional image is obtained in which the corresponding part becomes a black area;

[0048] Then, the two-dimensional image was subjected to binarization analysis of the measurement surface using -100 nm as a threshold value, and a binarized image was obtained in which the portion below -100 nm was a white area.

[0049]

[11] A method for manufacturing a display system, the method comprising:

[0050] A secondary laminate with a surface protection film is obtained by laminating another member to the side of the optical laminate with a surface protection film described in any one of [1] to [9] opposite to the side to which the first surface protection film and the second surface protection film are laminated;

[0051] peeling the second surface protection film from the secondary laminate with the surface protection film;

[0052] performing defect inspection on the secondary laminate with the surface protection film; and

[0053] The first surface protection film is peeled off from the secondary laminate with the surface protection film to obtain a secondary laminate,

[0054] Among them, the display system is goggles with a display.

[0055] Effects of the Invention

[0056] The optical laminate with surface protection film of the embodiment of the present invention has a structure in which two surface protection films are bonded to the surface of the optical laminate. Thus, even if the outer surface protection film is peeled off and removed before defect inspection, the optical laminate can be inspected for defects while the surface is protected by the inner surface protection film, and damage can be prevented until the assembly process is about to be performed. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a schematic cross-sectional view of an optical layered body with a surface protection film according to one embodiment of the present invention.

[0058] Figure 2 This is a schematic cross-sectional view for explaining a surface protection film that can be used for the optical layered body with a surface protection film according to the embodiment of the present invention.

[0059] Figure 3 This is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention.

[0060] Figure 4 It is shown that it can be used for Figure 3 A schematic cross-sectional view of an example of an optical stack of the display system shown.

[0061] Figure 5 It is shown that it can be used for Figure 3 A schematic cross-sectional view of an example of an optical stack of the display system shown.

[0062] Fig. 6A This is a schematic diagram for explaining a method for manufacturing a display system according to an embodiment of the present invention.

[0063] Figure 6B Then Fig. 6A .

[0064] Figure 6C Then Figure 6B .

[0065] Fig.6D Then Figure 6C .

[0066] Fig. 6E Then Fig.6D .

[0067] Explanation of symbols

[0068] 2 Display system

[0069] 4 Lens section

[0070] 10 Polarization component

[0071] 12 Display components

[0072] 14 Reflective polarizing element

[0073] 16. First lens unit

[0074] 18 Half Mirror

[0075] 20 first phase difference member

[0076] 22. Second phase difference member

[0077] 24 Second lens unit

[0078] 100 Optical laminate

[0079] 110 First surface protective film

[0080] 120 Second surface protective film

[0081] 200 Optical laminate with surface protection film DETAILED DESCRIPTION

[0082] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to these embodiments. In addition, in order to explain more clearly, the accompanying drawings sometimes schematically show the width, thickness, shape, etc. of each part compared with the embodiments, but this is only an example and does not limit the interpretation of the present invention.

[0083] (Definition of Terms and Symbols)

[0084] The definitions of terms and symbols in this specification are as follows.

[0085] (1) Refractive index (nx, ny, nz)

[0086] "nx" is the refractive index in the direction where the refractive index in the plane reaches the maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and "nz" is the refractive index in the thickness direction.

[0087] (2) In-plane phase difference (Re)

[0088] "Re(λ)" is the in-plane phase difference measured at 23°C with light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Re(λ) can be calculated by the formula: Re(λ) = (nx-ny)×d.

[0089] (3) Retardation in the thickness direction (Rth)

[0090] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C with light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Rth(λ) can be calculated by the formula: Rth(λ) = (nx-nz)×d.

[0091] (4) Nz coefficient

[0092] The Nz coefficient can be calculated by Nz=Rth / Re.

[0093] (5) Angle

[0094] In this specification, when an angle is mentioned, the angle includes both clockwise and counterclockwise relative to the reference direction. Therefore, for example, "45°" means 45° clockwise or counterclockwise. In addition, in this specification, "substantially parallel" includes the case within the range of 0°±10°, for example, 0°±5°, preferably 0°±3°, and more preferably 0°±1°, and "substantially orthogonal" includes the case within the range of 90°±10°, for example, 90°±5°, preferably 90°±3°, and more preferably 90°±1°.

[0095] A. Optical laminate with surface protection film

[0096] Figure 1 It is a schematic cross-sectional view of an optical laminate with a surface protective film according to an embodiment of the present invention. The optical laminate 200 with a surface protective film comprises: an optical laminate 100 including at least one optical component and used for goggles with a display; and a first surface protective film 110 and a second surface protective film 120 sequentially bonded to one side of the optical laminate 100 toward the outside. The optical laminate 100 may have an adhesive layer on the side opposite to the side bonded with the first surface protective film 110 and the second surface protective film 120. In this case, the adhesive layer may also be protected by a release liner. The first surface protective film 110, the second surface protective film 120, and the release liner are process components that are temporarily bonded (temporarily bonded) to the optical laminate 100, and are peeled off and removed when the optical laminate 100 is provided for use.

[0097] The optical laminate with surface protection film can be manufactured by laminating the first surface protection film and the second surface protection film on one side of the optical laminate. The first surface protection film and the second surface protection film can be laminated on one side of the optical laminate in sequence, or the laminate of the first surface protection film and the second surface protection film can be laminated on the optical laminate.

[0098] A-1. First surface protective film

[0099] like Figure 1 and Figure 2 As shown, the first surface protection film 110 includes a first substrate 112 and a first adhesive layer 114 laminated on the first substrate 112. A release liner 116 is bonded (temporarily bonded) to the first adhesive layer 114 to protect the first adhesive layer 114 until the first surface protection film 110 is used.

[0100] The haze of the first surface protective film is, for example, 5% or less, preferably 4% or less, more preferably 3% or less, further preferably 2% or less, further more preferably 1.5% or less, and typically 0.05% or more. When the haze of the first surface protective film is within the above range, even when the surface of the optical laminate is protected by the first surface protective film, precise defect inspection can be performed. The surface protective film having the haze in the above range can be obtained, for example, by using a substrate and / or adhesive layer with a low haze.

[0101] The 90° initial peeling force (P1) of the first surface protective film relative to the optical laminate is, for example, 0.05N to 0.25N, preferably 0.08N to 0.2N, and more preferably 0.10N to 0.15N. The 180° initial peeling force (P1') of the first surface protective film relative to the optical laminate is, for example, 0.05N to 0.25N, preferably 0.08N to 0.2N, and more preferably 0.10N to 0.15N. Generally speaking, when the film is peeled off from the end at a certain peeling speed, the peeling force of the film will increase in accordance with the peeling length just after the peeling starts, decrease after reaching the peak value, and stabilize at a constant value after a given time. In this specification, the initial peeling force refers to the peak value (maximum value) of the peeling force just after the peeling starts, and the conventional peeling force refers to the stabilized peeling force after a given time has passed since the peeling started.

[0102] The ratio (P2 / P1) of the 90° initial peeling force (P1) of the first surface protective film relative to the optical laminate to the 90° initial peeling force (P2) of the second surface protective film relative to the first surface protective film (the first substrate side surface of the first surface protective film) is, for example, 0.1 to 2.0, preferably 0.3 to 1.5, more preferably 0.5 to 1.0, and further preferably 0.5 to 0.9. In addition, the ratio (P2' / P1') of the 180° initial peeling force (P1') of the first surface protective film relative to the optical laminate to the 180° initial peeling force (P2') of the second surface protective film relative to the first surface protective film (the first substrate side surface of the first surface protective film) is, for example, 0.1 to 1.5, preferably 0.3 to 1.2, more preferably 0.5 to 1.0, and further preferably 0.5 to 0.9.

[0103] The normal peeling force (peeling angle 180°, tensile speed 300 mm / min) of the first surface protection film with respect to the optical laminate is, for example, 0.01 to 0.2 N / 25 mm, preferably 0.02 to 0.12 N / 25 mm, and more preferably 0.03 to 0.08 N / 25 mm.

[0104] The ratio (P2" / P1") of the normal peel force (P1") of the first surface protective film relative to the optical laminate to the normal peel force (P2") of the second surface protective film relative to the first surface protective film (first substrate side surface of the first surface protective film) is, for example, 0.1 to 3.0, preferably 0.5 to 2.5, and more preferably 1.0 to 2.0.

[0105] In one embodiment, when the first surface protection film (in a state where the release liner is peeled off and removed) is observed under a microscope, the number of defects having a maximum Feret diameter of 10 μm or more in an observation area of ​​100 μm×100 μm is preferably less than 3, more preferably 1 or less, and further preferably 0. When the number of defects of 10 μm or more observed under a microscope of the surface protection film is below the above upper limit, erroneous detection caused by the surface protection film can be more stably reduced in foreign matter inspection.

[0106] In one embodiment, when the first surface protection film (after the release liner is peeled off) is observed under a microscope, the number of defects having a maximum Feret diameter of less than 10 μm in an observation area of ​​100 μm×100 μm is, for example, 10 or less, preferably 5 or less, more preferably 3 or less, and more preferably 1 or less. Even if a defect is observed in the microscopic observation of the surface protection film, as long as the maximum Feret diameter is less than 10 μm and the number is below the above upper limit, it is possible to suppress erroneous detection of the defect in the foreign matter inspection.

[0107] <First base material>

[0108] When the first substrate 114 is observed under a microscope, the number of defects with a maximum Feret diameter of 10 μm or more in an observation area of ​​100 μm×100 μm is preferably less than 3, more preferably 1 or less, and further preferably 0. When the number of defects in the substrate is below the upper limit, false detection caused by the surface protective film can be reduced in foreign matter inspection. It should be noted that the details of the microscope observation will be described in the embodiments described later.

[0109] The tear strength of the first substrate is, for example, 0.5 N / mm or more, preferably 1 N / mm or more, and more preferably 2 N / mm or more. When the tear strength of the first substrate is above the above lower limit, it is possible to further reduce the false detection caused by the surface protective film in the foreign body inspection. The tear strength of the first substrate is typically 200 N / mm or less. It should be noted that the tear strength of the first substrate can be measured according to JIS K7128-1:1998.

[0110] The first substrate is formed by any appropriate resin film that can be used as a surface protection film. As a specific example of the material that becomes the main component of the resin film, cellulose resins such as cycloolefins (COP) such as polynorbornenes, polyesters such as polyethylene terephthalate (PET), triacetyl cellulose (TAC), polycarbonate (PC), (methyl) acrylic acid, polyvinyl alcohol, polyamide, polyimide, polyether sulfone, polysulfone, polystyrene, polyolefin, acetate and other transparent resins can be cited. In addition, thermosetting resins or ultraviolet curing resins such as (methyl) acrylic acid, carbamate, (methyl) acrylic acid carbamate, epoxy, silicone can also be cited. It should be noted that "(methyl) acrylic resin" refers to acrylic resin and / or methacrylic resin. In addition, glassy polymers such as siloxane polymers can also be cited. In addition, the polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imido group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl and nitrile group in the side chain can be used, for example, a resin composition having an alternating copolymer formed by isobutylene and N-methylmaleimide and acrylonitrile-styrene copolymer can be mentioned. The polymer film can be, for example, an extrusion molding of the above-mentioned resin composition. The material of the resin film can be used alone or in combination.

[0111] The first substrate preferably includes at least one transparent resin selected from COP, PET, TAC, PC and (meth) acrylic acid, more preferably includes at least one transparent resin selected from COP, PET, PC and (meth) acrylic acid, and further preferably includes at least one transparent resin selected from COP, PET and PC. If the first substrate includes the above-mentioned transparent resin, it is possible to more stably reduce the false detection caused by the surface protective film in foreign matter inspection and bubble inspection. In addition, if the first substrate includes any transparent resin of COP, PET, PC and (meth) acrylic acid, it is possible to reduce the false detection caused by the surface protective film in foreign matter inspection compared to the case where the first substrate includes TAC resin. In particular, if the first substrate includes any transparent resin of COP, PET and PC, it is possible to further stably reduce the false detection caused by the surface protective film in foreign matter inspection.

[0112] The first substrate may also contain antioxidants, ultraviolet absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, antistatic agents, etc. An easy-adhesion layer, an easy-slip layer, an anti-blocking layer, an antistatic layer, an anti-reflection layer, an anti-oligomer layer, etc. may also be provided on the surface of the first substrate (the surface opposite to the first adhesive layer).

[0113] The thickness of the first substrate is typically 5 μm or more, preferably 20 μm or more, and is typically 200 μm or less, preferably 100 μm or less.

[0114] <First adhesive layer>

[0115] The absolute value of the maximum valley depth (Sv) of the surface 114a on the opposite side of the first substrate 112 of the first adhesive layer 114 before being bonded to the optical laminate is, for example, less than 500nm, preferably less than 300nm, more preferably less than 250nm, particularly preferably less than 200nm, particularly preferably less than 100nm, and most preferably less than 50nm. The absolute value of the maximum valley depth (Sv) of the surface 114a is typically more than 5nm. It should be noted that the maximum valley depth (Sv) can be measured in accordance with JIS B0681-2:2018. When the absolute value of the maximum valley depth (Sv) of the surface 114a of the first adhesive layer 114 before being bonded to the optical laminate is less than the above-mentioned upper limit, even if the surface protective film is provided for defect inspection (for example, bubble inspection) in a state where the surface protective film is bonded to the optical laminate, the false detection caused by the surface protective film can be reduced.

[0116] The absolute value of the arithmetic mean height (Sa) of the surface 114a on the opposite side of the first substrate 112 of the first adhesive layer 114 before being bonded to the optical laminate is preferably 25nm or less, more preferably 10nm or less, further preferably 6nm or less, and particularly preferably 5nm or less. The absolute value of the arithmetic mean height (Sa) of the surface 114a is typically 0nm or more. It should be noted that the arithmetic mean height (Sa) can be measured in accordance with JIS B0681-2:2018. When the absolute value of the arithmetic mean height (Sa) of the surface 114a of the first adhesive layer 114 before being bonded to the optical laminate is below the above-mentioned upper limit, it is possible to stably reduce the false detection caused by the surface protective film in defect inspection (e.g., bubble inspection).

[0117] The surface 114a of the first pressure-sensitive adhesive layer 114 on the opposite side to the first substrate 112 before being bonded to the optical laminate preferably satisfies the following formula (1), more preferably satisfies the following formula (2), and further preferably satisfies the following formula (3).

[0118] [Mathematical formula 3]

[0119]

[0120] [Formula 4]

[0121]

[0122] [Formula 5]

[0123]

[0124] (In formula (1), S represents the measurement field area of ​​the white light interferometer in the surface shape evaluation test described below; B-BA represents the area of ​​the black area in the two-dimensional image before binarization obtained in the surface shape evaluation test described below; A-WA represents the area of ​​the white area in the two-dimensional image after binarization obtained in the surface shape evaluation test described below.)

[0125] <Surface shape evaluation test>

[0126] Measuring the surface of the first adhesive layer opposite to the first substrate using a white light interferometer;

[0127] For the obtained interference data, the measurement surface is calculated in the analysis range of -1000nm to -2000nm through frequency domain analysis, and a two-dimensional image is obtained in which the corresponding part becomes a black area;

[0128] Then, the two-dimensional image was subjected to binarization analysis of the measurement surface with a threshold of -100 nm, and a binarized image was obtained in which the portion below -100 nm was a white area. The details of the surface shape evaluation test will be described in the examples described later.

[0129] In the two-dimensional image before binarization, in the concave portion on the surface opposite to the first substrate in the first adhesive layer, the portion corresponding to the concave having a depth exceeding the detection limit of the white light interferometer becomes a black area, and the portion not corresponding to the black area becomes a white area. When the measurement field area S of the white light interferometer is 100%, the area B-BA of the black area in the two-dimensional image before binarization is, for example, 1.5% or less, preferably 0.3% or less, more preferably 0.2% or less, further preferably 0.1% or less, and typically 0% or more.

[0130] In the two-dimensional image after binarization (hereinafter, sometimes referred to as a binarized image), the portion corresponding to -100 nm or less relative to the measurement surface becomes a white area, and the other portion (the portion exceeding -100 nm relative to the measurement surface) becomes a black area. When the measurement field area S of the white light interferometer is set to 100%, the area A-WA of the white area in the binarized image is, for example, 1.3% or less, preferably 0.2% or less, more preferably 0.1% or less, further preferably 0.08% or less, and typically 0% or more.

[0131] If the surface of the first adhesive layer on the opposite side to the first substrate before being bonded to the optical laminate has a shape that satisfies the above-mentioned formula (1), preferably satisfies formula (2), and more preferably satisfies formula (3), then even if the surface protective film is bonded to the optical laminate and provided for defect inspection (for example, bubble inspection), erroneous detection caused by the surface protective film can be appropriately reduced.

[0132] The first adhesive layer typically contains at least one adhesive selected from the group consisting of a (meth)acrylic adhesive, a urethane adhesive, and a silicone adhesive. Preferably, the first adhesive layer contains a (meth)acrylic adhesive.

[0133] The (meth)acrylic adhesive contains a polymer having a (meth)acrylic acid alkyl ester as a monomer component as a main component (hereinafter referred to as a (meth)acrylic acid polymer). In other words, the (meth)acrylic acid polymer contains a structural unit derived from the (meth)acrylic acid alkyl ester. The content ratio of the structural unit derived from the (meth)acrylic acid alkyl ester in the (meth)acrylic acid polymer is typically 50% by mass or more, preferably 80% by mass or more, more preferably 93% by mass or more, for example, 100% by mass or less, preferably 98% by mass or less.

[0134] The alkyl group of the (meth)acrylic acid alkyl ester may be linear or branched. The number of carbon atoms of the alkyl group is, for example, 1 to 18. Examples of the alkyl group include methyl, ethyl, butyl, 2-ethylhexyl, decyl, isodecyl, and octadecyl. The (meth)acrylic acid alkyl ester may be used alone or in combination. The average number of carbon atoms of the alkyl group is preferably 3 to 10.

[0135] In addition to the structural unit derived from the alkyl (meth)acrylate, the (meth)acrylic polymer may also contain a structural unit derived from a comonomer that can polymerize with the alkyl (meth)acrylate. Examples of the comonomer include carboxyl group-containing monomers and hydroxyl group-containing monomers. The comonomers may be used alone or in combination.

[0136] The carboxyl group-containing monomer is a compound containing a carboxyl group in its structure and containing polymerizable unsaturated double bonds such as (meth) acryloyl and vinyl. As the carboxyl group-containing monomer, for example, (meth) acrylic acid, (meth) carboxyethyl acrylate, maleic acid, fumaric acid, crotonic acid, preferably (meth) acrylic acid. If the (meth) acrylic polymer contains a structural unit derived from the carboxyl group-containing monomer, it is possible to achieve an improvement in the adhesive properties of the adhesive layer. In the case where the (meth) acrylic polymer contains a structural unit derived from the carboxyl group-containing monomer, the content ratio of the structural unit derived from the carboxyl group-containing monomer is preferably 0.01% by mass or more and 10% by mass or less.

[0137] Hydroxyl-containing monomers are compounds containing hydroxyl groups in their structures and containing polymerizable unsaturated double bonds such as (meth) acryloyl groups and vinyl groups. As hydroxyl-containing monomers, for example, 2-hydroxyethyl (meth) acrylate, 3-hydroxypropyl (meth) acrylate, 8-hydroxyoctyl (meth) acrylate, 12-hydroxylauryl (meth) acrylate, methyl acrylate (4-hydroxymethylcyclohexyl), 2-hydroxyethyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate, and 2-hydroxyethyl (meth) acrylate can be preferably cited. If the (meth) acrylic polymer includes a structural unit derived from a hydroxyl-containing monomer, the durability of the adhesive layer can be improved. In the case where the (meth) acrylic polymer includes a structural unit derived from a hydroxyl-containing monomer, the content ratio of the structural unit derived from the hydroxyl-containing monomer is preferably 0.01% by mass or more and 10% by mass or less in the (meth) acrylic polymer.

[0138] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, 100,000 to 2,000,000, or preferably 200,000 to 1,000,000.

[0139] In addition, the (meth) acrylic adhesive may contain a crosslinking agent. As the crosslinking agent, representative examples include organic crosslinking agents and multifunctional metal chelates, and preferably organic crosslinking agents may be mentioned. As the organic crosslinking agent, for example, isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents may be mentioned, and more preferably isocyanate crosslinking agents may be mentioned. When the adhesive contains a crosslinking agent, the content ratio of the crosslinking agent is usually 0.01 mass parts or more and 15 mass parts or less relative to 100 mass parts of the (meth) acrylic polymer.

[0140] The above-mentioned adhesives ((meth)acrylic adhesives, urethane adhesives and silicone adhesives) may also contain various additives in appropriate proportions as required. By adjusting the composition of the base polymer (e.g., the type and content ratio of the monomer, the type and content ratio of the crosslinking agent, etc.), the molecular weight of the base polymer, the type or content ratio of the additives, etc., an adhesive layer having desired adhesion to the adherend can be obtained.

[0141] Examples of the additives include polymerization initiators, solvents, polymerization catalysts, crosslinking catalysts, silane coupling agents, tackifiers, plasticizers, softeners, anti-degradation agents, fillers, colorants (pigments, dyes, etc.), ultraviolet absorbers, antioxidants, surfactants, antistatic agents, chain transfer agents, and the like.

[0142] The thickness of the first adhesive layer is typically 1 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and is typically 30 μm or less, preferably 20 μm or less.

[0143] The first adhesive layer can be formed on the surface of the first substrate by direct writing or by transfer. In the case of direct writing, the adhesive is directly applied to the surface of the first substrate to form the first adhesive layer. In the case of transfer, after the adhesive is applied to the surface of the release liner to form the first adhesive layer, the substrate is attached to the first adhesive layer. In particular, when the first substrate contains an amorphous resin with a relatively low glass transition temperature Tg (for example, below 150°C), the first adhesive layer is preferably formed by a transfer process. If it is a transfer process, it is possible to suppress the influence of the high temperature during drying necessary for the formation of the first adhesive layer on the first substrate.

[0144] <Release liner>

[0145] The release liner 116 is formed of any appropriate resin film that can be used as a release liner. Specific examples of the material that is the main component of the resin film include polyethylene terephthalate (PET), polyethylene, and polypropylene. The materials of the resin film can be used alone or in combination. The release liner 116 can be transparent or opaque.

[0146] A release layer may also be provided on the contact surface of the release liner 116 with the surface 114a of the first adhesive layer 114. As the release agent forming the release layer, for example, silicone release agents, fluorine release agents, and long-chain alkyl acrylate release agents can be cited, preferably silicone release agents, and more preferably vinyl-containing addition silicones. The release agents can be used alone or in combination. The thickness of the release layer is typically 50 nm or more and 400 nm or less.

[0147] The contact surface of the release liner 116 with the surface 114a of the first adhesive layer 114 is smooth. Specifically, the absolute value of the maximum peak height (Sp) of the contact surface of the release liner 116 with the first adhesive layer 114 is representatively less than 500nm, preferably less than 400nm, more preferably less than 300nm, and further preferably less than 100nm. When the absolute value of the maximum peak height (Sp) of the contact surface is below the above-mentioned upper limit, the maximum valley depth (Sv) of the surface on the opposite side of the first adhesive layer and the first substrate can be stably adjusted to below the above-mentioned upper limit. In addition, when the absolute value of the maximum peak height (Sp) of the contact surface is below the above-mentioned upper limit, the surface on the opposite side of the first adhesive layer and the first substrate can be stably adjusted to satisfy the above-mentioned formula (1). The absolute value of the maximum peak height (Sp) of the contact surface is representatively more than 10nm. It should be noted that the maximum peak height (Sp) can be measured according to JISB0681-2:2018.

[0148] The absolute value of the arithmetic mean height (Sa) of the contact surface of the release liner 116 with the surface 114a of the first adhesive layer 114 is typically 30 nm or less, preferably 20 nm or less, more preferably 10 nm or less, and further preferably 5 nm or less. The absolute value of the arithmetic mean height (Sa) of the contact surface is typically 0 nm or more.

[0149] The thickness of the release liner 116 is typically 5 μm or more, preferably 20 μm or more, and typically 60 μm or less, preferably 45 μm or less. When a release layer is applied, the thickness of the release liner includes the thickness of the release layer.

[0150] A-2. Second surface protective film

[0151] like Figure 1 As shown, the second surface protection film 120 has a second substrate 122 and a second adhesive layer 124 laminated on the second substrate. As with the first surface protection film, a release liner is attached (temporarily attached) to the second adhesive layer to protect the second adhesive layer until the second surface protection film is used.

[0152] The second surface protection film may be transparent (eg, haze ≤ 5%) or opaque.

[0153] The 90° initial peeling force of the second surface protective film relative to the first surface protective film (the first substrate side surface of the first surface protective film) is, for example, 0.01N to 0.20N, preferably 0.03N to 0.15N, and more preferably 0.05N to 0.12N. The 180° initial peeling force of the second surface protective film relative to the first surface protective film (the first substrate side surface of the first surface protective film) is, for example, 0.01N to 0.20N, preferably 0.03N to 0.15N, and more preferably 0.05N to 0.12N.

[0154] The normal peel force (peeling angle 180°, tensile speed 300 mm / min) of the second surface protection film relative to the first surface protection film (first substrate side surface of the first surface protection film) is, for example, 0.01 N / 25 mm to 0.2 N / 25 mm, preferably 0.03 N / 25 mm to 0.15 N / 25 mm, and more preferably 0.05 N / 25 mm to 0.1 N / 25 mm.

[0155] <Second base material>

[0156] The second substrate may be formed of any appropriate resin film that can be used as a surface protection film. Specific examples of the material that is the main component of the resin film are as described above for the first substrate.

[0157] The second substrate may also contain antioxidants, ultraviolet absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, antistatic agents, etc. An easy-adhesion layer, an easy-slip layer, an anti-blocking layer, an antistatic layer, an anti-reflection layer, an anti-oligomer layer, etc. may also be provided on the surface of the second substrate (the surface opposite to the second adhesive layer).

[0158] The thickness of the second substrate is typically 5 μm or more, preferably 20 μm or more, and is typically 200 μm or less, preferably 100 μm or less.

[0159] <Second adhesive layer>

[0160] Typically, the second adhesive layer contains at least one adhesive selected from a (meth)acrylic adhesive, a urethane adhesive, and a silicone adhesive. Preferably, the second adhesive layer contains a (meth)acrylic adhesive. Details of the (meth)acrylic adhesive are as described above for the first adhesive layer.

[0161] The above-mentioned adhesive ((meth)acrylic adhesive, urethane adhesive, and silicone adhesive) may contain a base polymer (or its constituent monomer components) and, if necessary, additives. Specific examples of the additives are as described above for the first adhesive layer.

[0162] The thickness of the second pressure-sensitive adhesive layer is typically 1 μm or more, preferably 5 μm or more, and is typically 30 μm or less, preferably 15 μm or less.

[0163] As a method for forming the second pressure-sensitive adhesive layer, the same method as the method for forming the first pressure-sensitive adhesive layer may be mentioned.

[0164] A-3. Optical laminate

[0165] The optical laminate includes at least one optical member and is used for goggles with a display. Examples of the optical member include a polarizing member (absorptive polarizing member, reflective polarizing member), a phase difference member, and the like.

[0166] A-3-1. Display system to which optical laminate can be applied

[0167] Figure 3 Schematic diagram showing the simplified structure of a display system (goggles with display) to which an optical laminate can be applied. Figure 3 , the configuration and shape of each component of the display system 2 are schematically shown. The display system 2 includes a display element 12, a reflective polarization component 14, a first lens unit 16, a half mirror 18, a first phase difference component 20, a second phase difference component 22, and a second lens unit 24. The reflective polarization component 14 is arranged on the display surface 12a side of the display element 12, that is, in front, and can reflect the light emitted from the display element 12. The first lens unit 16 is arranged on the optical path between the display element 12 and the reflective polarization component 14, and the half mirror 18 is arranged between the display element 12 and the first lens unit 16. The first phase difference component 20 is arranged on the optical path between the display element 12 and the half mirror 18, and the second phase difference component 22 is arranged on the optical path between the half mirror 18 and the reflective polarization component 14. Although not shown in the figure, the display system 2 may further include an absorptive polarization component between the reflective polarization component 14 and the second lens unit 24.

[0168] Components arranged in front of the half mirror (in the illustrated example, the half mirror 18 , the first lens unit 16 , the second phase difference element 22 , the reflective polarization element 14 , and the second lens unit 24 ) are sometimes collectively referred to as a lens unit (lens unit 4 ).

[0169] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying images. Light emitted from the display surface 12a passes through a polarizing member (representatively a polarizing film) 10 that may be included in the display element 12 and then emitted as first linearly polarized light.

[0170] The first phase difference member 20 includes a first λ / 4 member capable of converting the first linear polarization light incident on the first phase difference member 20 into a first circular polarization light. When the first phase difference member does not include a member other than the first λ / 4 member, the first phase difference member may be equivalent to the first λ / 4 member. The first phase difference member 20 may be integrally provided on the display element 12.

[0171] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarization member 14 toward the reflective polarization member 14. The half mirror 18 is integrally provided with the first lens portion 16.

[0172] The second phase difference member 22 includes a second λ / 4 member that allows the light reflected by the reflective polarization member 14 and the half mirror 18 to pass through the reflective polarization member 14. When the second phase difference member does not include a member other than the second λ / 4 member, the second phase difference member may be equivalent to the second λ / 4 member. The second phase difference member 22 may be integrally provided on the first lens portion 16.

[0173] The first circularly polarized light emitted from the first λ / 4 member included in the first phase difference member 20 passes through the half mirror 18 and the first lens unit 16, and is converted into the second linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The second linearly polarized light emitted from the second λ / 4 member does not pass through the reflective polarization member 14, but is reflected toward the half mirror 18. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarization member 14 is the same direction as the reflection axis of the reflective polarization member 14. Therefore, the second linearly polarized light incident on the reflective polarization member 14 is reflected by the reflective polarization member 14.

[0174] The second linear polarized light reflected by the reflective polarization member 14 is converted into the second circular polarized light by the second λ / 4 member included in the second phase difference member 22, and the second circular polarized light emitted from the second λ / 4 member passes through the first lens unit 16 and is reflected by the half mirror 18. The second circular polarized light reflected by the half mirror 18 passes through the first lens unit 16 and is converted into the third linear polarized light by the second λ / 4 member included in the second phase difference member 22. The third linear polarized light is transmitted through the reflective polarization member 14. At this time, the polarization direction of the third linear polarized light incident on the reflective polarization member 14 is the same direction as the transmission axis of the reflective polarization member 14. Therefore, the third linear polarized light incident on the reflective polarization member 14 is transmitted through the reflective polarization member 14.

[0175] The light transmitted through the reflective polarization element 14 passes through the second lens portion 24 and enters the eye 26 of the user.

[0176] For example, the absorption axis of the polarization component 10 included in the display element 12 and the reflection axis of the reflective polarization component 14 can be arranged approximately parallel to each other, or can be arranged approximately orthogonal to each other. The angle formed by the absorption axis of the polarization component 10 included in the display element 12 and the slow axis of the 1st λ / 4 component included in the first phase difference component 20 is, for example, 40° to 50°, 42° to 48°, or approximately 45°. The angle formed by the absorption axis of the polarization component included in the display element 12 and the slow axis of the 2nd λ / 4 component included in the second phase difference component 22 is, for example, 40° to 50°, 42° to 48°, or approximately 45°.

[0177] In the lens portion 4, a space can be formed between the first lens portion 16 and the second lens portion 24. In this case, the component arranged between the first lens portion 16 and the second lens portion 24 is preferably provided integrally in any one of the first lens portion 16 and the second lens portion 24. For example, the component arranged between the first lens portion 16 and the second lens portion 24 is preferably integrated with any one of the first lens portion 16 and the second lens portion 24 via an adhesive layer. According to such a method, for example, the operability of each component can be excellent. The adhesive layer can be formed by an adhesive or an adhesive. Specifically, the adhesive layer can be an adhesive layer or an adhesive layer. The thickness of the adhesive layer is, for example, 0.05μm to 30μm.

[0178] A-3-2. Configuration of optical laminate

[0179] Figure 4 is able to Figure 3A simplified cross-sectional view of an optical laminate used in an exemplary display system. The optical laminate 100a includes an adhesive layer 31, a polarizing element 10, a first phase difference element 20, and a first protective element 41 in sequence. The polarizing element 10, the first phase difference element 20, and the first protective element 41 are stacked together via adhesive layers 51 and 52. The adhesive layers 51 and 52 are typically adhesive layers or adhesive layers, preferably adhesive layers. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm. During the period until it is provided for use, the surface of the adhesive layer 31 is protected by a release liner 61. It should be noted that the first surface protective film and the second surface protective film are adhered to the side surface of the first protective element 41 of the optical laminate 100a.

[0180] exist Figure 4 In the example shown, the first phase difference component 20 includes, in addition to the first λ / 4 component 20a, a component (so-called positive C plate) 20b whose refractive index characteristics can show the relationship of nz>nx=ny. The first phase difference component 20 has a stacked structure of the first λ / 4 component 20a and the first positive C plate 20b. Preferably, as shown in the example in the figure, the first λ / 4 component 20a is located closer to the polarization component 10 side than the first positive C plate 20b, but their configuration may also be the opposite. In addition, the first positive C plate 20b may also be omitted. The first λ / 4 component 20a and the first positive C plate 20b may be stacked, for example, via an adhesive layer not shown in the figure. In addition, in the first phase difference component 20, it is configured so that the angle between the absorption axis of the polarization component 10 and the slow axis of the first λ / 4 component 20a is preferably 40° to 50°, more preferably 42° to 48°, for example, about 45°.

[0181] The optical laminate 100a can be applied to, for example, Figure 3The manufacture of a display system of an embodiment in which the first phase difference member 20 is integrally arranged on the display element 12 in the exemplary display system. For example, by peeling off the release liner 61 from the optical laminate 100a, and attaching the polarization member 10 to the liquid crystal unit in a manner that makes the polarization member 10 become the front side (visible side) polarization member of the liquid crystal unit together with the back side polarization member, a display system in which the first phase difference member 20 and the liquid crystal panel (display element) are set as one can be manufactured. In addition, for example, by peeling off the release liner 61 from the optical laminate 100a, and attaching it to the front of the organic EL panel via the adhesive layer 31, a display system in which the first phase difference member 20 and the organic EL panel (display element) are set as one can be manufactured. In this case, from the viewpoint of anti-reflection, a third phase difference member including a 3rd λ / 4 member can be configured between the optical laminate 100a and the organic EL panel. The third phase difference member can be included in the optical laminate. For example, the optical laminate can have an adhesive layer, a third phase difference member, a polarization member, a first phase difference member, and a protective member in sequence. The third λ / 4 member can be arranged so that the slow axis of the third λ / 4 member and the absorption axis of the polarization member 10 form an angle of, for example, 40° to 50°, 42° to 48°, or about 45°.

[0182] <Polarization member>

[0183] The polarizing element 10 is typically an absorbing polarizing element including a resin film containing a dichroic substance (sometimes referred to as an absorbing polarizing film), and may further include a protective layer on one or both sides thereof as required. The protective layer is typically bonded to the absorbing polarizing film via any appropriate adhesive layer. As an adhesive forming the adhesive layer, a UV curable adhesive can be typically cited.

[0184] The orthogonal transmittance (Tc) of the absorption type polarization component (absorption type polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and further preferably 0.05% or less. The single transmittance (Ts) of the absorption type polarization component (absorption type polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarization degree (P) of the absorption type polarization component (absorption type polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.

[0185] The above-mentioned orthogonal transmittance, single transmittance and polarization degree can be measured, for example, using an ultraviolet visible spectrophotometer. The polarization degree P can be measured using an ultraviolet visible spectrophotometer for single transmittance Ts, parallel transmittance Tp and orthogonal transmittance Tc, and the obtained Tp and Tc can be obtained by the following formula. It should be noted that Ts, Tp and Tc are Y values ​​obtained by measuring the 2-degree field of view (C light source) of JIS Z8701 and correcting for visibility.

[0186] Polarization degree P (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0187] The thickness of the absorption-type polarizing film is, for example, 1 μm to 20 μm, 2 μm to 15 μm, 12 μm or less, 10 μm or less, 8 μm or less, or 5 μm or less.

[0188] The absorption-type polarizing film may be produced by a single-layer resin film or by using a laminate of two or more layers.

[0189] In the case of a single-layer resin film, for example, a hydrophilic polymer film such as a polyvinyl alcohol (PVA) film, a partially formalized PVA film, or a partially saponified ethylene-vinyl acetate copolymer film can be subjected to dyeing treatment using a dichroic substance such as iodine or a dichroic dye, stretching treatment, etc., thereby obtaining an absorption-type polarizing film. Among them, an absorption-type polarizing film obtained by dyeing a PVA film with iodine and uniaxially stretching the film is preferred.

[0190] The dyeing using iodine can be performed by, for example, immersing the PVA film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching can be performed after the dyeing treatment or while dyeing. In addition, the dyeing can also be performed after the stretching. The PVA film can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. as needed.

[0191] As a laminate made using the above-mentioned two or more layers, there can be cited a laminate of a resin substrate and a PVA-type resin layer (PVA-type resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-type resin layer formed by coating on the resin substrate. The absorption-type polarizing film obtained by using a laminate of a resin substrate and a PVA-type resin layer formed by coating on the resin substrate can be made by the following method: for example, a PVA-type resin solution is applied to a resin substrate, dried to form a PVA-type resin layer on the resin substrate, and a laminate of a resin substrate and a PVA-type resin layer is obtained; the laminate is stretched and dyed to make the PVA-type resin layer into an absorption-type polarizing film. In this embodiment, it is preferred to form a polyvinyl alcohol-type resin layer containing a halide and a polyvinyl alcohol-type resin on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution for stretching. In addition, stretching can further include stretching the laminate in a gas atmosphere at a high temperature (for example, above 95°C) before stretching in a boric acid aqueous solution as needed. In addition, in the present embodiment, it is preferred that the laminate is subjected to a drying shrinkage treatment in which the laminate shrinks by more than 2% in the width direction by heating while being conveyed in the length direction. Representatively, the manufacturing method of the present embodiment includes sequentially performing an auxiliary stretching treatment in a gas atmosphere, a dyeing treatment, a stretching treatment in an aqueous solution, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, the crystallinity of the PVA can be improved even when the PVA is coated on the thermoplastic resin, and high optical properties can be achieved. In addition, by simultaneously improving the orientation of the PVA in advance, it is possible to prevent problems such as the reduction of the orientation and dissolution of the PVA when immersed in water in the subsequent dyeing process and the stretching process, and high optical properties can be achieved. In addition, when the PVA-type resin layer is immersed in a liquid, the orientation disorder of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-type resin layer does not contain a halide. Thus, the optical properties of the absorption-type polarizing film obtained by the treatment process of immersing the laminate in a liquid such as a dyeing treatment and a stretching treatment in an aqueous solution can be improved. Further, the laminate is shrunk in the width direction by drying and shrinking treatment, thereby improving the optical properties. The obtained laminate of resin substrate / absorption type polarizing film can be used directly (that is, the resin substrate can be used as a protective layer of absorption type polarizing film), or the resin substrate can be peeled off from the laminate of resin substrate / absorption type polarizing film, and any appropriate protective layer corresponding to the purpose can be stacked on the peeling surface or on the side opposite to the peeling surface. The details of the manufacturing method of such an absorption type polarizing film are recorded in, for example, Japanese Patent Publication No. 2012-73580 and Japanese Patent No. 6470455. The records of these publications as a whole are cited in this specification as a reference.

[0192] The protective layer can be formed by any appropriate film that can be used as a protective layer of the absorption type polarizing film. As a specific example of the material that becomes the main component of the film, there can be cited: cycloolefins (COP) such as polynorbornenes, polyesters such as polyethylene terephthalate (PET), cellulose resins such as triacetyl cellulose (TAC), polycarbonate (PC), (meth) acrylic acid, polyvinyl alcohol, polyamide, polyimide, polyether sulfone, polysulfone, polystyrene, polyolefin, acetate and other transparent resins. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid, carbamate, (meth) acrylic acid carbamate, epoxy, silicone, etc. can also be cited. It should be noted that "(meth) acrylic resin" refers to acrylic resin and / or methacrylic resin. In addition, glassy polymers such as siloxane polymers can also be cited. In addition, the polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imido group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl and nitrile group in the side chain can be used, for example, a resin composition having an alternating copolymer formed by isobutylene and N-methylmaleimide and acrylonitrile-styrene copolymer can be mentioned. The polymer film can be, for example, an extrusion molding of the above-mentioned resin composition. The material of the resin film can be used alone or in combination.

[0193] The thickness of the protective layer is typically 100 μm or less, for example, 5 μm to 80 μm, preferably 10 μm to 50 μm, and more preferably 15 μm to 35 μm.

[0194] <1st λ / 4 member>

[0195] The in-plane phase difference Re(550) of the first λ / 4 component 20a is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases in accordance with the wavelength of the measurement light. The Re(450) / Re(550) of the first λ / 4 component is, for example, not less than 0.75 and less than 1, or not less than 0.8 and not more than 0.95.

[0196] The refractive index characteristics of the first λ / 4 component preferably show a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within the range that does not impair the effect of the present invention, ny<nz may sometimes be satisfied. The Nz coefficient of the first λ / 4 component is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0197] The first λ / 4 member may be formed of any appropriate material that can satisfy the above-mentioned characteristics. The first λ / 4 member may be, for example, a stretched film of a resin film or an alignment fixing layer of a liquid crystal compound.

[0198] As the resin contained in the above-mentioned resin film, there can be mentioned: polycarbonate resin, polyester carbonate resin, polyester resin, polyvinyl acetal resin, polyarylate resin, cyclic olefin resin, cellulose resin, polyvinyl alcohol resin, polyamide resin, polyimide resin, polyether resin, polystyrene resin, acrylic resin, etc. These resins can be used alone or in combination. As a method of combination, for example, blending and copolymerization can be mentioned. In the case where the first λ / 4 component shows a reverse dispersion wavelength characteristic, a resin film containing a polycarbonate resin or a polyester carbonate resin (hereinafter, sometimes referred to as a polycarbonate resin) can be suitably used.

[0199] As the above-mentioned polycarbonate resin, any appropriate polycarbonate resin can be used. For example, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from alicyclic diols, alicyclic dimethanols, di, tri or polyethylene glycols and alkylene glycols or spirodiols. Preferably, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, structural units derived from alicyclic dimethanols and / or structural units derived from di, tri or polyethylene glycols; more preferably, it contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from di, tri or polyethylene glycols. The polycarbonate resin may also contain structural units derived from other dihydroxy compounds as needed. It should be noted that details of the polycarbonate resin that can be suitably used for the first λ / 4 component and the method for forming the first λ / 4 component are described in, for example, Japanese Patent Gazette No. 2014-10291, Japanese Patent Gazette No. 2014-26266, Japanese Patent Gazette No. 2015-212816, Japanese Patent Gazette No. 2015-212817, and Japanese Patent Gazette No. 2015-212818, and the records in these gazettes are cited as references in this specification.

[0200] The thickness of the first λ / 4 member formed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.

[0201] The orientation fixing layer of the above-mentioned liquid crystal compound is a layer in which the liquid crystal compound is oriented along a given direction within the layer and its orientation state is fixed. It should be noted that the "orientation fixing layer" is a concept that includes an orientation solidification layer obtained by solidifying a liquid crystal monomer as described later. In the 1st λ / 4 component, representatively, the rod-shaped liquid crystal compound is oriented in a state arranged along the slow axis direction of the 1st λ / 4 component (parallel orientation (homogeneous alignment)). As rod-shaped liquid crystal compounds, for example, liquid crystal polymers and liquid crystal monomers can be cited. The liquid crystal compound is preferably capable of polymerization. If the liquid crystal compound is capable of polymerization, the orientation state of the liquid crystal compound can be fixed by polymerizing after orienting the liquid crystal compound.

[0202] The orientation fixing layer (liquid crystal orientation fixing layer) of the above-mentioned liquid crystal compound can be formed by the following method: an orientation treatment is applied to the surface of a given substrate, a coating liquid containing a liquid crystal compound is applied to the surface, and the liquid crystal compound is oriented along the direction corresponding to the above-mentioned orientation treatment to fix the orientation state. As an orientation treatment, any appropriate orientation treatment can be adopted. Specifically, mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment can be cited. As specific examples of mechanical orientation treatment, friction treatment and stretching treatment can be cited. As specific examples of physical orientation treatment, magnetic field orientation treatment and electric field orientation treatment can be cited. As specific examples of chemical orientation treatment, inclined evaporation method and optical orientation treatment can be cited. The processing conditions of various orientation treatments can adopt any appropriate conditions according to the purpose.

[0203] The liquid crystal compound can be aligned by treating it at a temperature corresponding to the type of the liquid crystal compound at which it exhibits a liquid crystal phase. By such a temperature treatment, the liquid crystal compound is in a liquid crystal state and is aligned in the alignment treatment direction of the substrate surface.

[0204] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state can be fixed by subjecting the aligned liquid crystal compound to polymerization or crosslinking treatment as described above.

[0205] As the above-mentioned liquid crystal compound, any appropriate liquid crystal polymer and / or liquid crystal monomer can be used. Liquid crystal polymer and liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for making liquid crystal orientation fixing layers are described in, for example, Japanese Patent Publication No. 2006-163343, Japanese Patent Publication No. 2006-178389, and International Publication No. 2018 / 123551. The records of these publications are cited as references in this specification.

[0206] The thickness of the first λ / 4 member composed of the liquid crystal alignment fixing layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.

[0207] <1st positive C plate>

[0208] The thickness direction phase difference Rth(550) of the first positive C plate 20b is preferably -50nm to -300nm, more preferably -70nm to -250nm, further preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane phase difference Re(550) of the first positive C plate is, for example, less than 10nm.

[0209] The first positive C plate can be formed of any appropriate material. The first positive C plate is preferably composed of a film containing a liquid crystal material fixed in a homeotropic orientation. The liquid crystal material (liquid crystal compound) capable of homeotropic orientation can be a liquid crystal monomer or a liquid crystal polymer. As a specific example of such a liquid crystal compound and a method for forming a positive C plate, there can be cited the liquid crystal compound and the method for forming the phase difference layer described in

[0020] to

[0028] of Japanese Patent Gazette No. 2002-333642. In this case, the thickness of the first positive C plate is preferably 0.5μm to 5μm.

[0210] <First protection member>

[0211] Typically, the first protective member 41 includes a substrate. The substrate may be composed of any appropriate film. As the material of the main component of the film constituting the substrate, for example, cellulose resins such as triacetyl cellulose (TAC), polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyether sulfones, polysulfones, polystyrenes, cycloolefins such as polynorbornene, polyolefins, (meth) acrylic acid, acetate resins, etc. can be cited. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 15 μm to 35 μm.

[0212] The first protective member preferably has a substrate and a surface treatment layer formed on the substrate. The first protective member having a surface treatment layer can be configured in such a way that the surface treatment layer is located on the front side. Specifically, the surface treatment layer can be located on the outermost surface of the optical laminate 100a. The surface treatment layer can have any appropriate function. As the surface treatment layer, for example, there can be mentioned: a hard coating layer, an anti-reflection layer, an anti-adhesion layer, and an anti-glare layer. The first protective member may also have more than two layers of surface treatment layers. The water contact angle on the surface of the surface treatment layer can be, for example, greater than 90° and less than 125°, and, for example, greater than 100° and less than 115°.

[0213] The anti-reflection layer is provided to prevent reflection of external light, etc. As the anti-reflection layer, for example, a fluororesin layer, a resin layer containing nanoparticles (representatively hollow nanoparticles, such as hollow nano silica particles), or an anti-reflection layer having a nanostructure (such as a moth eye structure) can be cited. The thickness of the anti-reflection layer is preferably 0.05 μm to 1 μm. As a method for forming the above-mentioned resin layer, for example, a sol-gel method, a thermal curing method using isocyanate, an ionizing radiation curing method (representatively a photocuring method) using a cross-linking monomer (such as a multifunctional acrylate) and a photopolymerization initiator can be cited. In one embodiment, the anti-reflection layer is provided on the outermost surface of the first protective member, and a first surface protective film is attached to the surface of the anti-reflection layer. According to the embodiment in which the anti-reflection layer is provided on the outermost surface of the first protective member, an excellent anti-reflection effect can be obtained in a display system in which a space is formed between the semi-reflecting mirror 18 and the first phase difference member 20.

[0214] The hard coat layer preferably has sufficient surface hardness, excellent mechanical strength, and excellent light transmittance. The hard coat layer can be formed of any appropriate resin. Typically, the hard coat layer can be formed of an ultraviolet curable resin. Examples of ultraviolet curable resins include polyesters, acrylics, urethanes, amides, silicones, and epoxies. The thickness of the hard coat layer is, for example, 0.5 μm or more, preferably 1 μm or more, for example, 20 μm or less, preferably 15 μm or less.

[0215] <Adhesive layer>

[0216] The adhesive layer 31 can be composed of any appropriate adhesive. As specific examples, acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives can be cited. By adjusting the type, quantity, combination and ratio of the monomers of the base resin forming the adhesive, as well as the amount of the cross-linking agent, the reaction temperature, the reaction time, etc., it is possible to prepare an adhesive with desired characteristics corresponding to the purpose. The base resin of the adhesive can be used alone or in combination of two or more. As the base resin, an acrylic resin can be preferably used. Specifically, the adhesive layer is preferably formed by an acrylic adhesive.

[0217] The thickness of the adhesive layer is typically 1 μm or more, preferably 5 μm or more, more preferably 12 μm or more, and is typically 60 μm or less, preferably 30 μm or less, more preferably 23 μm or less.

[0218] <Release liner>

[0219] The release liner 61 is formed of any appropriate resin film. Specific examples of the material that is the main component of the resin film include polyethylene terephthalate (PET), polyethylene, and polypropylene. The materials of the resin film can be used alone or in combination. The release liner can be transparent (for example, the haze is less than 5%, and for example, less than 3%), or opaque.

[0220] A release treatment layer may be provided on the contact surface of the release liner 61 with the adhesive layer 31. Examples of release treatment agents for forming the release treatment layer include silicone-based release treatment agents, fluorine-based release treatment agents, and long-chain alkyl acrylate-based release treatment agents. The release treatment agents may be used alone or in combination. The thickness of the release treatment layer is typically 50 nm or more and 400 nm or less.

[0221] The thickness of the release liner is typically 5 μm or more, preferably 20 μm or more, and typically 60 μm or less, preferably 45 μm or less. When a release treatment layer is applied, the thickness of the release liner includes the thickness of the release treatment layer.

[0222] Figure 5 Yes, you can Figure 3A simplified cross-sectional view of another optical laminate used in the exemplified display system. The optical laminate 100b includes an adhesive layer 32, a second phase difference member 22, and a second protective member 42 in sequence. The second phase difference member 22 and the second protective member 42 are stacked together via an adhesive layer 53. The adhesive layer 53 is typically an adhesive layer or an adhesive layer, preferably an adhesive layer. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm. During the period until it is provided for use, the surface of the adhesive layer 32 is protected by a release liner 62. The first surface protective film and the second surface protective film are attached to the second protective member 42 side of the optical laminate 100b.

[0223] exist Figure 5 In the example shown, the second phase difference member 22 includes, in addition to the second λ / 4 member 22a, a member (so-called positive C plate) 22b whose refractive index characteristics can show the relationship of nz>nx=ny. The second phase difference member 22 has a stacked structure of the second λ / 4 member 22a and the second positive C plate 22b. Preferably, as shown in the example in the figure, the second λ / 4 member 22a is located closer to the second protective member 42 side than the second positive C plate 22b, but their configuration may also be the opposite. In addition, the second positive C plate 22b may also be omitted. The second λ / 4 member 22a and the second positive C plate 22b may be stacked, for example, via an adhesive layer not shown.

[0224] The optical laminate 100b can be applied to, for example, Figure 3 The manufacturing of the display system of the embodiment in which the second phase difference member 22 is integrally provided in the first lens unit 16 in the exemplary display system. Specifically, by peeling the release liner 62 from the optical laminate 100b and attaching it to the first lens unit 16 via the adhesive layer 32, the display system in which the second phase difference member 22 is integrally provided in the first lens unit 16 can be manufactured.

[0225] <Second λ / 4 member>

[0226] The in-plane phase difference Re(550) of the second λ / 4 component 22a is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The second λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases in accordance with the wavelength of the measurement light. The Re(450) / Re(550) of the second λ / 4 component is, for example, greater than 0.75 and less than 1, or greater than 0.8 and less than 0.95.

[0227] The refractive index characteristics of the second λ / 4 component preferably show a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within the range that does not impair the effect of the present invention, ny<nz may sometimes be satisfied. The Nz coefficient of the second λ / 4 component is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0228] The second λ / 4 member may be formed of any appropriate material that can satisfy the above-mentioned characteristics. The second λ / 4 member may be, for example, a stretched film of a resin film or an alignment fixing layer of a liquid crystal compound. The same description as that of the first λ / 4 member may be applied to the second λ / 4 member formed of a stretched film of a resin film or an alignment fixing layer of a liquid crystal compound. The first λ / 4 member and the second λ / 4 member may have the same or different configurations (for example, forming materials, thickness, optical properties, etc.).

[0229] <Second positive C plate>

[0230] The thickness direction phase difference Rth(550) of the second positive C plate 22b is preferably -50nm to -300nm, more preferably -70nm to -250nm, further preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane phase difference Re(550) of the second positive C plate is, for example, less than 10nm.

[0231] The second positive C plate can be formed of any appropriate material that can satisfy the above characteristics. The same description as the first positive C plate can be applied to the constituent material of the second positive C plate. The first positive C plate and the second positive C plate can have the same composition (for example, forming material, thickness, optical properties, etc.) or different compositions.

[0232] <Second protection member>

[0233] The second protective member 42 typically includes a substrate, preferably a substrate and a surface treatment layer formed on the substrate. In this case, the surface treatment layer can be located on the outermost surface of the optical laminate 100b. Regarding the details of the substrate and the surface treatment layer, the same description as the first protective member can be applied. According to an embodiment in which an anti-reflection layer is provided on the outermost surface of the second protective member 42 as a surface treatment layer, in a display system in which the second phase difference member 22 is integrated with the first lens unit 16, the reflective polarization member 14 is integrated with the second lens unit 24, and a space is formed between them, an excellent anti-reflection effect can be obtained.

[0234] The same description as that of the pressure-sensitive adhesive layer 31 and the release liner 61 used in the optical layered body 100 a can be applied to the pressure-sensitive adhesive layer 32 and the release liner 62 used in the optical layered body 100 b , respectively.

[0235] B. Method of manufacturing a display system

[0236] According to another aspect of the present invention, a method for manufacturing a display system (goggles with a display) is provided, which uses an optical laminate with a surface protection film as described in item A. The method for manufacturing a display system according to an embodiment of the present invention includes: peeling off the second surface protection film from the optical laminate with a surface protection film as described in item A to obtain an optical laminate with only the first surface protection film bonded thereto; and inspecting for defects on an object to be inspected in which the optical laminate with only the first surface protection film bonded thereto is bonded to another component. The peeling off of the second surface protection film may be performed before or after the production of the object to be inspected (i.e., the bonding of the optical laminate with the surface protection film to another component).

[0237] A method for manufacturing a display system according to an embodiment of the present invention includes:

[0238] The optical laminate with a surface protection film described in item A is laminated with another member on the side opposite to the side where the first surface protection film and the second surface protection film are laminated to obtain a secondary laminate with a surface protection film;

[0239] peeling the second surface protection film from the secondary laminate with the surface protection film;

[0240] performing defect inspection on the secondary laminate with the surface protection film; and

[0241] The first surface protection film is peeled off from the secondary laminate with the surface protection film to obtain a secondary laminate.

[0242] The obtained secondary laminate is subjected to an assembly step and assembled together with other components to form a display system. Hereinafter, an example of a method for manufacturing the display system of the present invention will be described with reference to FIG.

[0243] Fig. 6A The optical laminate 200 with a surface protection film shown has Figure 4 In the optical laminate 100a illustrated in the example, a first surface protective film 110 and a second surface protective film 120 are sequentially bonded to the surface of the first protective material 41 of the optical laminate 100a toward the outside. In one embodiment, the optical laminate 100a is processed into a shape corresponding to the shape of the bonded body (another member 300 shown in FIG. 6(b)). For example, the optical laminate 200 with a surface protective film is processed into a desired shape by cutting, punching, cutting, etc.

[0244] like Figure 6B As shown, the release liner 61 is peeled off from the optical laminate 200 with a surface protection film and attached to the visible side (front) surface of the optical component (e.g., liquid crystal cell, organic EL panel) 300 via the exposed adhesive layer 31 to obtain a secondary laminate 400a with a surface protection film.

[0245] Next, if Figure 6C As shown, the second surface protection film 120 is peeled off from the secondary laminate 400a with a surface protection film, thereby obtaining the secondary laminate 400b with a surface protection film.

[0246] Next, if Fig.6D As shown, defect inspection is performed on the secondary laminate 400 b with a surface protection film in a state where the surface is protected by the first surface protection film 110 .

[0247] Next, if Fig. 6E As shown, the first surface protection film 110 is peeled off from the secondary laminate 400b with a surface protection film judged as a good product in the defect inspection, thereby obtaining a secondary laminate 400c. The secondary laminate 400c is used for assembly of a display system.

[0248] According to the above-mentioned manufacturing method, it is possible to appropriately prevent the attachment of scratches, foreign matter, dirt, etc. on the surface of the optical laminate until it is immediately introduced into the display system, and it is possible to perform precise defect inspection on the optical component immediately before it is introduced into the display system. Such an effect is particularly advantageous for the case where the manufacturing of the optical laminate, the manufacturing of the display element, the assembly (assembly) of the display system and other processes are carried out in different places. In one embodiment, the optical laminate is shipped to the display element manufacturer (for example, the first semi-finished product) in the state of an optical laminate with a surface protective film to which two surface protective films are attached. Fig. 6A ); by bonding the optical laminate with a surface protective film to an optical component such as a liquid crystal unit and an organic EL element, a display element (a liquid crystal panel, an organic EL panel, etc.) to which an optical laminate with a surface protective film is bonded is obtained (for example, Figure 6B ); then, the second surface protective film is peeled off, and the defect inspection of the display element is performed in a state where the surface is protected by the first surface protective film (for example, Figure 6C and D); the display element judged as a qualified product in the defect inspection is shipped to the manufacturer of the display system as a second semi-finished product in a state where the first surface protective film is attached; the display element can be provided for assembly with other components (for example, Fig. 6E). According to the manufacturing method of this embodiment, it is possible to appropriately prevent defects (scars, foreign matter, dirt, etc.) when shipping the first semi-finished product, inspect defects when manufacturing the second semi-finished product, and prevent defects (scars, foreign matter, dirt, etc.) when shipping the second semi-finished product, and as a result, it is possible to contribute to the efficient manufacturing of the final product.

[0249] The manufacturing method of the display system is not limited to the example shown in the figure. For example, the second surface protective film may be peeled off before the release liner is peeled off and bonded to the optical component, and the defect inspection may be performed before bonding to the optical component. For example, after the second surface protective film and the release liner are peeled off and the optical laminated body in a state where only the first surface protective film is bonded is inspected for defects, the optical laminated body may be bonded to the optical component. In addition, for example, after the second surface protective film is peeled off and the optical laminated body in a state where the first surface protective film and the release liner are bonded is inspected for defects, the release liner may be peeled off and the optical laminated body may be bonded to the optical component.

[0250] Defect inspection can be performed by automatic optical inspection (AOI), visual inspection, etc. Preferably, defect inspection includes automatic optical inspection (AOI). Depending on the purpose, defect inspection can be performed by a transmission optical system, a reflection optical system, or a combination thereof.

[0251] Example

[0252] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. It should be noted that the thickness is a value measured by the following measurement method.

[0253] <Thickness>

[0254] The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL Ltd., product name “JSM-7100F”). The thickness exceeding 10 μm was measured using a digital micrometer (manufactured by Anritsu Co., Ltd., product name “KC-351C”).

[0255] <Haze of surface protection film>

[0256] For each surface protection film, the release liner was peeled off from the pressure-sensitive adhesive layer, and the haze was measured in accordance with JIS K7136 by irradiating light from the substrate side of the surface protection film using a haze meter ("NDH-5000" manufactured by Nippon Denshoku Industries Co., Ltd.).

[0257] [Manufacturing Example 1A: Preparation of Surface Protection Film A]

[0258] <Acrylic polymer A>

[0259] In a reaction container equipped with a thermometer, a stirrer, a condenser and a nitrogen inlet pipe, 96.2 parts by mass of 2-ethylhexyl acrylate (2EHA) as a monomer component and 3.8 parts by mass of hydroxyethyl acrylate (HEA) and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were added together with 150 parts by mass of ethyl acetate, and nitrogen was introduced while slowly stirring at 23°C to replace the nitrogen. Then, the liquid temperature was maintained at about 65°C for 6 hours of polymerization reaction to prepare a solution of acrylic polymer A (concentration 40% by mass). The weight average molecular weight of acrylic polymer A was 540,000.

[0260] <Adhesive composition A>

[0261] Ethyl acetate was added to the solution of acrylic polymer A to dilute it to a concentration of 20 mass %. To 500 mass parts (100 mass parts of solid content) of this solution, 4 mass parts of isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 mass parts (0.03 mass parts of solid content) of dibutyltin dilaurate (1 mass % ethyl acetate solution) as a crosslinking catalyst were added and stirred to prepare an adhesive composition A.

[0262] <Surface protection film A>

[0263] Adhesive composition A was applied to one side of a substrate (PET film, "CE905-38" manufactured by KOLON, thickness 38 μm), and then dried to form an adhesive layer (thickness 15 μm). Next, a release liner (manufactured by Toyobo Co., Ltd., product number TG704) was attached to the surface of the adhesive layer opposite to the substrate. Thus, a surface protective film A was obtained. The haze of the surface protective film A was 1.8%.

[0264] [Manufacturing Example 1B: Preparation of Surface Protection Film B]

[0265] A PET film ("CE901-38" manufactured by KOLON, thickness 38 μm) was used as the substrate, and an adhesive layer (thickness 15 μm) was formed in the same manner as in Manufacturing Example 1A. Next, a release liner (manufactured by Toyobo Co., Ltd., product number TG704) was attached to the surface of the adhesive layer opposite to the substrate. Thus, a surface protective film B was obtained. The haze of the surface protective film B was 3.9%.

[0266] [Manufacturing Example 1C: Preparation of Surface Protection Film C]

[0267] A surface protection film C was obtained in the same manner as in Production Example 1A except that a PET film (Mitsubishi Chemical Corporation "Product No. T100C38", thickness 38 μm) was used as a substrate and the adhesive composition A was applied to the corona-treated surface thereof to form an adhesive layer having a thickness of 5 μm. The haze of the surface protection film C was 2.6%.

[0268] The surface protection film B and the release liner used for the production thereof were evaluated in the following (1) to (5).

[0269] (1) Surface shape evaluation test of adhesive layer

[0270] In the surface protection film, the release liner is peeled off from the pressure-sensitive adhesive layer to expose the surface of the pressure-sensitive adhesive layer on the opposite side to the substrate.

[0271] Next, the surface protection film after removal of the release liner was placed in a white light interferometer (Zygo NewView7300, manufactured by Zygo Corporation) so that the exposed surface of the pressure-sensitive adhesive layer faced the objective lens, and interference data of the pressure-sensitive adhesive layer surface was measured under the following conditions.

[0272] White light interferometer measurement conditions:

[0273] Objective lens: ×10

[0274] Internal lens: ×1.0

[0275] Resolution: 1.09μm

[0276] Measurement field of view (S): 0.3641mm 2

[0277] Removed: Cylinder

[0278] The obtained interference data were calculated using frequency domain analysis (calculation software; MetroPro) on the measurement surface (reference surface) in the analysis range (depth direction) of -1000nm to -2000nm, and a two-dimensional image was obtained in which the corresponding part became a black area.

[0279] In addition, the measurement plane (reference plane) was set based on the plane which becomes the average height in the measurement field area. Table 2 shows the area (B-BA) of the black region in the two-dimensional image.

[0280] Next, the two-dimensional image was binarized and analyzed with a threshold of -100 nm on the measurement surface, and a binary image was obtained in which the portion below -100 nm was a white area. Table 2 shows the area (A-WA) of the white area in the binary image.

[0281] Next, the ratio of the sum of the area of ​​the black region in the two-dimensional image (B-BA) and the area of ​​the white region in the binary image (A-WA) to the measurement field area S of the white light interferometer was calculated (see the above (Equations (1) to (3)). The results are shown in Table 2.

[0282] (2) Measurement of the maximum valley depth and arithmetic mean height on the surface of the adhesive layer

[0283] The minimum value relative to the average surface in the measured field of view in the two-dimensional image obtained by the above-mentioned white light interferometer measurement is taken as the maximum valley depth (Sv). In addition, the value of Ra is taken as the arithmetic mean height (Sa). It should be noted that the maximum valley depth and the arithmetic mean height use the average value of the data of three randomly selected points. The results are shown in Table 2.

[0284] (3) Determination of the maximum peak height and arithmetic mean height of the release liner

[0285] In the above (1), the release liner after peeling off the adhesive layer is set in the above white light interferometer, and the interference data of the release liner is measured under the above conditions to obtain a two-dimensional image. The maximum value relative to the average surface in the visual field area in the obtained two-dimensional image is taken as the maximum peak height (Sp). In addition, the value of Ra is taken as the arithmetic mean height (Sa). It should be noted that the maximum peak height and the arithmetic mean height adopt the average value of the data of three randomly selected points. The results are shown in Table 1.

[0286] (4) Determination of the number of defects in the substrate by microscopic observation

[0287] The surface of the substrate was observed using a microscope (manufactured by OLYMPUS, trade name BX51, eyepiece magnification 10×, objective magnification 10×). Next, a 0.1 mm×0.1 mm area was randomly selected from the observation field and the number of defects having a maximum Feret diameter of 10 μm or more was measured by visual observation.

[0288] The results are shown in Table 1.

[0289] (5) Determination of tear strength of substrate

[0290] Basically, the measurement was performed in accordance with JIS K7128-1:1998.

[0291] Specifically, the substrate was cut into a size of 150 mm × 50 mm. Next, a 75 mm slit was cut from the center of the end of the short side in a direction parallel to the long side to prepare a sample sheet. It should be noted that for the tear strength in the MD direction, the sample was prepared in a manner such that the long side direction was parallel to the MD direction, and for the tear strength in the TD direction, the sample was prepared in a manner such that the long side direction was parallel to the TD direction.

[0292] The obtained test piece was placed in a tensile testing machine and evaluated at a tensile speed of 200 mm / min (temperature 23°C / relative humidity 50%) to measure the tearing force. The tear strength f was calculated based on the obtained tearing force. (f = Ft / d (Ft: tearing force of the test piece [N], d: thickness of the test piece [mm])). The results are shown in Table 1.

[0293] [Table 1]

[0294]

[0295] [Table 2]

[0296]

[0297] ※Threshold is -100nm

[0298] [Peel force evaluation: initial peel force]

[0299] For surface protection films A and B, the 90° and 180° initial peeling forces of the protective member produced in the manufacturing example 5 described later relative to the surface treatment layer side surface were measured. In addition, for surface protection film C, the 90° and 180° initial peeling forces of surface protection film A or B relative to the substrate side surface were measured. The measurement was performed with N=10, and the average value was taken as the initial peeling force. The results are shown in Table 3. It should be noted that the method for measuring the initial peeling force is as follows.

[0300] <Method for measuring initial peel force>

[0301] (1) Surface protection films A and B

[0302] Cut a rectangular film (50mm×50mm) from the protective member and bond it to the SUS plate via a double-sided adhesive tape (manufactured by Nitto Denko Corporation, “No.535A”). At this time, bonding was performed in such a way that the acrylic film side became the SUS plate side. Next, the surface protective film A or B cut into the same shape was bonded to the surface treatment layer of the protective member in a superimposed manner by a manual roller reciprocating once, thereby obtaining a laminate having a structure of [SUS plate / protective member / surface protective film]. An adhesive tape (manufactured by Nitto Denko Corporation, “No.315”, width 25mm) cut into a length of about 10cm was placed 2cm away from the corner of the surface protective film of the laminate, and bonded by a 2kg roller reciprocating once, thereby obtaining a measurement sample.

[0303] The peeling force when the surface protection film was peeled off from the corner of the measurement sample was measured under the following conditions, and the peak value immediately after the start of the measurement was defined as the initial peeling force of the surface protection film A or B.

[0304] · Measurement device: Tensile testing machine (manufactured by Kyowa Interface Science Co., Ltd., adhesive film peeling analysis device "VPA-2", turn on the power, and age for more than 30 minutes.)

[0305] ·Measurement environment: 23±5℃, 60±20RH%

[0306] Peeling speed: 300 mm / min

[0307] Peeling angle: 90° or 180°

[0308] (2) Surface protection film C

[0309] The surface protective film A or B was cut into a rectangular film piece (50 mm×50 mm), the release liner was peeled off, and the film was attached to a SUS plate via the exposed adhesive layer. The surface protective film C was attached to the substrate layer surface of the surface protective film. The initial peeling force of the protective film C was measured in the same manner as in the above (1), except that the surface protective film A or B was cut into a rectangular film piece (50 mm×50 mm), the release liner was peeled off, and the film was attached to a SUS plate via the exposed adhesive layer.

[0310] [Table 3]

[0311]

[0312] [Peel force evaluation: conventional peel force]

[0313] For surface protection films A and B, the normal peeling force was measured relative to the surface treatment layer side surface of the protective member of the optical laminate prepared in Example 1 described later. In addition, for surface protection film C, the normal peeling force was measured relative to the substrate side surface of surface protection film A or B. The measurement was performed with N=30, and the average value was taken as the normal peeling force. The results are shown in Table 4. It should be noted that the method for measuring the normal peeling force is as follows.

[0314] <Conventional peel force measurement method>

[0315] The surface protective film was cut into a size of 25 mm in width and 100 mm in length, and after the release liner was peeled off from the adhesive layer, it was pressed against the adherend with a roller at a pressure of 0.25 MPa and a feed speed of 0.3 m / min. The sample was left to stand for 30 minutes in an environment at a temperature of 23°C and a relative humidity of 50%, and then a peeling test was performed in the same environment at a peeling angle of 180° and a tensile speed of 300 mm / min, and the 180° peeling force was measured.

[0316] [Table 4]

[0317]

[0318] [Manufacturing Example 2: Preparation of Polarizing Film]

[0319] A 30 μm thick polyvinyl alcohol (PVA) resin film (manufactured by Kuraray Co., Ltd., product name "PE3000") was uniaxially stretched in the length direction to 5.9 times the length using a roller stretching machine, and then swollen, dyed, cross-linked, and cleaned, and finally dried to produce an absorption-type polarizing film with a thickness of 12 μm.

[0320] Specifically, the swelling treatment was carried out while being treated in pure water at 20°C and stretched to 2.2 times. Next, the dyeing treatment was carried out while being treated in a 30°C aqueous solution in which the weight ratio of iodine to potassium iodide was 1:7 after the iodine concentration was adjusted so that the monomer transmittance of the obtained absorption-type polarizing film reached 45.0%, and the film was stretched to 1.4 times. Furthermore, the cross-linking treatment adopted a two-stage cross-linking treatment, and the first stage of the cross-linking treatment was treated while being stretched to 1.2 times in an aqueous solution of boric acid and potassium iodide dissolved at 40°C. The boric acid content of the aqueous solution of the first stage of the cross-linking treatment was 5.0% by weight, and the potassium iodide content was 3.0% by weight. The second stage of the cross-linking treatment was treated while being stretched to 1.6 times in an aqueous solution of boric acid and potassium iodide dissolved at 65°C. The boric acid content of the aqueous solution of the second stage of the cross-linking treatment was 4.3% by weight, and the potassium iodide content was 5.0% by weight. In addition, the cleaning treatment was carried out in a potassium iodide aqueous solution at 20°C. The potassium iodide content of the aqueous solution in the washing treatment was adjusted to 2.6 wt %. Finally, the aqueous solution was dried at 70° C. for 5 minutes to obtain an absorption-type polarizing film.

[0321] As protective layers, a triacetylcellulose (TAC) resin film with HC (TAC thickness: 25 μm, HC thickness: 7 μm) was laminated on one side of the obtained absorption-type polarizing film, and a cycloolefin resin film (thickness: 13 μm) was laminated on the other side. Specifically, the curable adhesive was applied so that the total thickness was about 1 μm, and the film was laminated using a roller press. Then, UV light was irradiated from the TAC film side to cure the adhesive.

[0322] Thus, a polarizing film having a structure of [TAC film (protective layer) / absorptive polarizing film / COP film (protective layer)] was obtained.

[0323] [Manufacturing Example 3: Preparation of λ / 4 Member]

[0324] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10-6 parts by mass of calcium acetate monohydrate as a catalyst were added. -2 Mass parts (6.78×10 -5 mol). After the reactor was replaced with nitrogen under reduced pressure, it was heated by a heat medium and stirring was started when the internal temperature reached 100°C. The internal temperature reached 220°C 40 minutes after the start of the temperature rise, and the pressure was reduced while controlling to maintain the temperature, so that it reached 13.3kPa after 90 minutes after reaching 220°C. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a 100°C reflux condenser, so that a certain amount of monomer components contained in the phenol vapor was returned to the reactor, and the uncondensed phenol vapor was introduced into a 45°C condenser for recovery. After nitrogen was introduced into the first reactor to temporarily restore it to atmospheric pressure, the reaction liquid after oligomerization in the first reactor was transferred to the second reactor. Next, the temperature rise and pressure reduction in the second reactor were started, so that it reached an internal temperature of 240°C and a pressure of 0.2kPa after 50 minutes. Then, the polymerization was carried out until the given stirring power was reached. When the predetermined power was reached, nitrogen gas was introduced into the reactor to restore the pressure, and the produced polyester carbonate resin was extruded into water, and the strands were cut to obtain pellets.

[0325] The obtained polyester carbonate resin (pellets) was vacuum dried at 80°C for 5 hours, and then a film-making device equipped with a single screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder was used to produce a long strip of resin film with a thickness of 135 μm. The obtained long strip of resin film was stretched in the width direction at a stretching temperature of 143°C and a stretching ratio of 2.8 times to obtain a stretched film (λ / 4 member) with a thickness of 47 μm. The Re(550) of the obtained stretched film was 143 nm, the Re(450) / Re(550) was 0.86, and the Nz coefficient was 1.12.

[0326] [Manufacturing Example 4: Preparation of Positive C Plate]

[0327] A liquid crystal coating liquid was prepared by dissolving 20 parts by weight of a side chain liquid crystal polymer represented by the following chemical formula (1) (the numbers 65 and 35 in the formula represent the molar % of the monomer unit, and for convenience, it is represented as a block polymer: the weight average molecular weight is 5000), 80 parts by weight of a polymerizable liquid crystal showing a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Chiba Specialty Chemicals: trade name IRGACURE 907) in 200 parts by weight of cyclopentanone. Then, the coating liquid was applied to a PET substrate subjected to a vertical alignment treatment using a wire bar coater, and then heated and dried at 80°C for 4 minutes to orient the liquid crystal. The liquid crystal layer was irradiated with ultraviolet rays to cure the liquid crystal layer, thereby forming a positive C plate with a thickness of 4 μm and an Rth (550) of -100 nm on the substrate.

[0328] [Chemical formula 1]

[0329]

[0330] [Manufacturing Example 5: Preparation of Protective Member]

[0331] The hard coating layer forming material shown below was applied to an acrylic film (thickness 40 μm) having a lactone ring structure, and the coating layer was dried to form a hard coating layer with a thickness of 0.5 μm. Next, the antireflection layer forming material shown below was applied to the surface of the hard coating layer, heated at 80°C for 1 minute, and the heated coating layer was irradiated with a high pressure mercury lamp with a cumulative light intensity of 300 mJ / cm 2 The coating layer was cured by ultraviolet light to form an antireflection layer with a thickness of 0.1 μm. Thus, a protective member having a structure of [acrylic film / hard coat layer / antireflection layer] was obtained.

[0332] (Hard coat layer forming material)

[0333] A material for forming a hard coat layer was prepared by adding 0.5 wt % of a leveling agent to an acrylic resin raw material (manufactured by Dainippon Ink Co., Ltd., trade name: GRANDIC PC1071), and further diluting with ethyl acetate so that the solid content concentration reaches 50 wt %. It should be noted that the leveling agent is a copolymer obtained by copolymerizing dimethylsiloxane:hydroxypropylsiloxane:6-isocyanatehexylisocyanuric acid:aliphatic polyester at a molar ratio of 6.3:1.0:2.2:1.0.

[0334] (Anti-reflection layer forming material)

[0335] 100 parts by weight of a multifunctional acrylate containing pentaerythritol triacrylate as the main component (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300", solid content 100% by weight), 150 parts by weight of hollow nano-silica particles (manufactured by JGC Catalysts & Chemicals Co., Ltd., trade name "THRULYA 5320", solid content 20% by weight, weight average particle size 75 nm), 50 parts by weight of solid nano-silica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle size 10 nm), 12 parts by weight of an additive containing a fluorine element (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD 907", solid content 100% by weight) were mixed. A mixed solvent of TBA (tert-butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 was added to the mixture as a diluent so that the overall solid content reached 4 weight %, and the mixture was stirred to prepare an anti-reflection layer forming material.

[0336] [Manufacturing Example 6: Preparation of Adhesive Layer]

[0337] A monomer mixture containing 80.3 parts of butyl acrylate, 16 parts of phenoxyethyl acrylate, 3 parts of N-vinyl-2-pyrrolidone (NVP), 0.3 parts of acrylic acid, and 0.4 parts of 4-hydroxybutyl acrylate was added to a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was added together with 100 parts of ethyl acetate to 100 parts of the above-mentioned monomer mixture (solid content), and nitrogen was introduced while slowly stirring to perform nitrogen replacement. Next, the liquid temperature in the flask was maintained at around 55°C and a polymerization reaction was performed for 8 hours to prepare an acrylic polymer solution. The weight average molecular weight of the acrylic polymer is 1.5 million. With respect to 100 parts of the solid content of the obtained acrylic polymer solution, 0.3 parts of benzoyl peroxide (BPO: Nyper BMT manufactured by NOF Corporation) as a crosslinking agent was added to prepare an acrylic adhesive solution.

[0338] The obtained PSA composition was applied to the release-treated layer of a release liner (Cerapeel, manufactured by Toray Industries, Inc.), and dried at 155° C. for 3 minutes to form a 20 μm-thick PSA layer.

[0339] [Example 1]

[0340] (1) A surface protection film laminate was obtained using surface protection film A as a first surface protection film and surface protection film C as a second surface protection film. Specifically, a release liner was peeled off from surface protection film C and attached to the substrate surface of surface protection film A to obtain a surface protection film laminate having a structure of [release liner / surface protection film A / surface protection film C].

[0341] (2) The pressure-sensitive adhesive layer obtained in Production Example 6 was bonded together with a release liner to the COP protective layer-side surface of the polarizing film obtained in Production Example 2 to obtain a pressure-sensitive adhesive layer-attached polarizing film.

[0342] (3) The positive C plate is transferred to a λ / 4 member (stretched film) via an ultraviolet curing adhesive (thickness 1 μm after curing) to obtain a phase difference member. The protective member obtained in Manufacturing Example 5 is bonded to the positive C plate side of the obtained phase difference member via another acrylic adhesive layer. At this time, bonding is performed in a manner such that the acrylic film of the protective member is located on the side of the phase difference member (in other words, in a manner such that the anti-reflection layer becomes the outermost surface). Next, another acrylic adhesive layer formed on the release liner is bonded to the side surface of the λ / 4 member. Thus, a laminate having a structure of [protective member / positive C plate / λ / 4 member / acrylic adhesive layer / release liner] is obtained.

[0343] (4) For the surface protection film laminate obtained in (1), the release liner on the side of the surface protection film A is peeled off and then bonded to the protective component side surface of the laminate obtained in (3) via the exposed adhesive layer. Just after bonding, a knife is cut from the top to punch out a rectangular film A. It should be noted that the rectangular film A is punched out using a knife die that can make the slow axis of the λ / 4 component parallel to the short side direction. Similarly, the polarizing film with an adhesive layer obtained in (2) is cut from the top to punch out a rectangular film B. It should be noted that the rectangular film B is punched out using a knife die that can make the absorption axis of the absorption-type polarizing film tilted 45° relative to the longitudinal direction. After the release liner of film A is peeled off, it is bonded to film B without applying tension and aligned in the longitudinal direction. As described above, film A is punched out in such a manner that the slow axis of the λ / 4 component is parallel to the short side direction, and film B is punched out in such a manner that the absorption axis of the absorption type polarizing film is tilted 45°, so that the angle formed by the absorption axis of the absorption type polarizing film and the slow axis of the λ / 4 component becomes 45°.

[0344] As described above, an optical laminate with a surface protective film having a structure of [optical laminate (release liner / adhesive layer / polarizing member / λ / 4 member / positive C plate / protective member) / surface protective film A / surface protective film C] was obtained.

[0345] [Example 2]

[0346] An optical layered body with a surface protection film having a structure of [optical layered body / surface protection film B / surface protection film C] was obtained in the same manner as in Example 1 except that the surface protection film B was used as the first surface protection film.

[0347] [Comparative Example 1]

[0348] An optical laminate with a surface protective film having a structure of [optical laminate / surface protective film C] was obtained in the same manner as in Example 1, except that the surface protective film C was bonded only to the protective member side surface (antireflection layer surface) of the laminate obtained in (3) of the above Example 1.

[0349] [Comparative Example 2]

[0350] An optical laminate with a surface protective film having a structure of [optical laminate / surface protective film A] was obtained in the same manner as in Example 1, except that the surface protective film A was bonded only to the protective member side surface (antireflection layer surface) of the laminate obtained in (3) of the above Example 1.

[0351] [Comparative Example 3]

[0352] An optical laminate with a surface protective film having a structure of [optical laminate / surface protective film B] was obtained in the same manner as in Example 1, except that the surface protective film B was bonded only to the protective member side surface (antireflection layer surface) of the laminate obtained in (3) of the above Example 1.

[0353] [Defect inspection]

[0354] The optical laminate with a surface protective film obtained in the above-mentioned embodiments and comparative examples was cut into a size of 371.87 mm × 236.58 mm and used as a sample to be inspected. For the samples to be inspected of Examples 1 and 2, the release liner and the second surface protective film were peeled off for defect inspection, and for the samples to be inspected of Comparative Examples 1 to 3, the release liner was peeled off for defect inspection. Specifically, the above-mentioned sample to be inspected was set in the clamping part of the optical automatic appearance inspection device, and defects (scars, foreign matter, bubbles, etc.) with a size of 100 μm or more in the sample were detected. Next, the part where the defect with a size of 100 μm or more was detected was observed under a microscope, thereby confirming whether it was a false detection of the defect caused by the surface protective film or a defect of the optical laminate. The inspection defect incidence rate was calculated based on the "formula: inspection defect incidence rate (%) = number of false detections / total number of detections × 100", and the failure evaluation of the inspection was performed based on the following criteria. The presence or absence of scratches with a size of 100 μm or more on the surface of the surface protection film was confirmed, and the scratches were evaluated based on the following criteria.

[0355] <Evaluation of the feasibility of inspection>

[0356] ○(Good): Inspection defect rate: 0%

[0357] △(Qualified): Inspection defect rate: more than 0% and less than 10%

[0358] ×(Defective): The defective rate is more than 10%

[0359] <Scar Evaluation>

[0360] ○ (Good): No scratches larger than 100 μm

[0361] × (bad): There are scratches of 100 μm or more

[0362] [Table 5]

[0363]

[0364] As shown in Table 5, the optical laminate with a surface protective film in the embodiment having a configuration in which a double surface protective film is bonded to the surface of the optical laminate can be protected from damage by the outer surface protective film before defect inspection. In addition, even if the outer surface protective film is peeled off and removed during defect inspection, the optical laminate can be inspected for defects while being bonded to the inner surface protective film, and the surface can be appropriately protected until it is provided for assembly. Furthermore, by using a film with a small haze as the inner surface protective film, automatic inspection of the optical laminate can be appropriately performed while being bonded to the surface protective film.

[0365] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, the above-described embodiments may be replaced with substantially the same configuration, a configuration that exhibits the same effects, or a configuration that achieves the same purpose.

[0366] Industrial Applicability

[0367] The optical laminate with a protective film according to the embodiment of the present invention can be used, for example, for the production of goggles with a display such as VR goggles.

Claims

1. An optical laminate with a surface protection film, comprising: An optical laminate including at least one optical member used for goggles with a display; and A first surface protection film and a second surface protection film are sequentially bonded to one surface of the optical layered body toward the outside.

2. The optical laminate with a surface protection film according to claim 1, wherein The haze of the first surface protection film is less than 5%.

3. The optical layered body with a surface protective film according to claim 1, wherein the following surface protective film is bonded to the optical layered body as the first surface protective film, The surface protection film comprises a first substrate and a first adhesive layer laminated on the first substrate, wherein the absolute value of the maximum valley depth (Sv) of the surface of the first adhesive layer on the opposite side of the first substrate is less than 500 nm, and when the first substrate is observed under a microscope, in an observation area of ​​100 μm×100 μm, the number of defects with a maximum Feret diameter of more than 10 μm is less than 3.

4. The optical laminate with a surface protection film according to claim 3, wherein An absolute value of an arithmetic mean height (Sa) of a surface of the first pressure-sensitive adhesive layer on the opposite side to the first substrate is 25 nm or less.

5. The optical layered body with a surface protective film according to claim 1, wherein the following surface protective film is bonded to the optical layered body as the first surface protective film, The surface protection film comprises a first substrate and a first adhesive layer laminated on the first substrate, wherein a surface of the first adhesive layer opposite to the first substrate satisfies the following formula (1): In formula (1), S represents the measurement field area of ​​the white light interferometer in the following surface shape evaluation test; B-BA represents the area of ​​the black area in the two-dimensional image before binarization obtained in the following surface shape evaluation test; A-WA represents the area of ​​the white area in the two-dimensional image after binarization obtained in the following surface shape evaluation test, Surface shape evaluation test: Measuring the surface of the first adhesive layer opposite to the first substrate using a white light interferometer; For the obtained interference data, the measurement surface is calculated in the analysis range of -1000nm to -2000nm through frequency domain analysis, and a two-dimensional image is obtained in which the corresponding part becomes a black area; Then, the two-dimensional image was subjected to binarization analysis of the measurement surface using -100 nm as a threshold value, and a binarized image was obtained in which the portion below -100 nm was a white area.

6. The optical laminate with a surface protection film according to claim 5, wherein When the first substrate is observed under a microscope, the number of defects having a maximum Feret diameter of 10 μm or more is less than 3 in an observation area of ​​100 μm×100 μm.

7. The optical laminate with a surface protection film according to claim 1, wherein The optical laminate includes a polarizing member, a first phase difference member, and a protective member in this order toward the first surface protective film.

8. The optical laminate with a surface protection film according to claim 7, wherein The protective member comprises a surface treatment layer, The first surface protection film is attached to the surface treatment layer.

9. The optical laminate with a surface protection film according to claim 1, wherein The optical laminate has a pressure-sensitive adhesive layer on a surface opposite to the side on which the first surface protection film and the second surface protection film are bonded.

10. A method for producing an optical laminate with a surface protection film, the method comprising: A first surface protection film and a second surface protection film are bonded to one surface of an optical layered body having at least one optical member. The first surface protection film is selected from (i) and (ii): (i) a surface protective film comprising a first substrate and a first adhesive layer laminated on the first substrate, wherein the absolute value of the maximum valley depth (Sv) of the surface of the first adhesive layer on the side opposite to the first substrate is 500 nm or less, and when the first substrate is observed under a microscope, the number of defects with a maximum Feret diameter of 10 μm or more in an observation area of ​​100 μm×100 μm is less than 3; (ii) a surface protective film comprising a first substrate and a first adhesive layer laminated on the first substrate, wherein the surface of the first adhesive layer opposite to the first substrate satisfies the following formula (1), In formula (1), S represents the measurement field area of ​​the white light interferometer in the following surface shape evaluation test; B-BA represents the area of ​​the black area in the two-dimensional image before binarization obtained in the following surface shape evaluation test; A-WA represents the area of ​​the white area in the two-dimensional image after binarization obtained in the following surface shape evaluation test, Surface shape evaluation test: Measuring the surface of the first adhesive layer opposite to the first substrate using a white light interferometer; For the obtained interference data, the measurement surface is calculated in the analysis range of -1000nm to -2000nm through frequency domain analysis, and a two-dimensional image is obtained in which the corresponding part becomes a black area; Then, the two-dimensional image was subjected to binarization analysis of the measurement surface using -100 nm as a threshold value, and a binarized image was obtained in which the portion below -100 nm was a white area.

11. A method for manufacturing a display system, the method comprising: A secondary laminate with a surface protection film is obtained by laminating another member on the side of the optical laminate with a surface protection film according to any one of claims 1 to 9 opposite to the side on which the first surface protection film and the second surface protection film are laminated; peeling the second surface protection film from the secondary laminate with the surface protection film; Conducting defect inspection on the secondary laminate with the surface protection film; as well as The first surface protection film is peeled off from the secondary laminate with the surface protection film to obtain a secondary laminate, Among them, the display system is goggles with a display.