Negative electrode for lithium secondary battery and method for producing same
By using a combination of carbon-based and silicon-based materials in lithium secondary batteries, combined with magnetic field and rolling technology, a stable negative electrode active layer is formed, which solves the poor charging and life characteristics of the negative electrode of lithium secondary battery during long-term charging and discharging. The problem of high energy density and capacity retention rate are achieved.
Patent Information
- Application Number
- CN202380029060.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-15
- Filing Date
- 2023-11-27
- Publication Date
- 2024-11-05
AI Technical Summary
The charging characteristics and life characteristics of the negative electrode of the existing lithium secondary battery are poor during long-term charging and discharging, especially due to the loss of the orientation of the carbon material due to the change in the volume of the silicon material, which reduces the durability of the electrode.
Using a negative electrode containing carbon-based and silicon-based negative electrode active materials, the negative electrode active layer is formed by controlling the arrangement value of the carbon-based negative electrode material to meet the specific equation range after activation, combining magnetic field and rolling technology to ensure that The migration path of lithium ions is robust, reducing material volume changes and orientation damage.
The high charging characteristics and life characteristics of lithium secondary batteries during long-term charging and discharging are realized, and the energy density and capacity retention rate of the battery are improved.
Smart Images

Figure CN118901150A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode for a lithium secondary battery, and to a lithium secondary battery having excellent charge and discharge characteristics and life characteristics by including the negative electrode.
[0002] This application claims priority to Korean Patent Application No. 10-2022-0169280 filed on December 7, 2022 and Korean Patent Application No. 10-2023-0076626 filed on June 15, 2023, the disclosures of which are incorporated herein by reference in their entirety. Background Art
[0003] In recent years, lithium secondary batteries are widely used not only in small devices such as portable electronic devices, but also in medium and large devices, such as battery packs or power storage in hybrid electric vehicles and electric vehicles. Therefore, research is being conducted on batteries that can meet various needs. In particular, lithium secondary batteries with high energy density and excellent life and cycle characteristics are being actively studied as power sources for medium and large devices.
[0004] A lithium secondary battery is a rechargeable power generation device consisting of a laminated structure of a positive electrode, a separator, and a negative electrode. When a lithium secondary battery is charged, a lithium deintercalation reaction is caused at the positive electrode inside the battery, in which the lithium contained in the positive electrode active material is oxidized and released, and a lithium intercalation reaction occurs at the negative electrode, in which the lithium is reduced and enters the negative electrode active material. Generally, the performance of a lithium secondary battery is mainly determined by the charging rate at the negative electrode, because the deintercalation reaction at the positive electrode active material is faster than the intercalation reaction at the negative electrode active material.
[0005] Carbon materials including graphite are widely used as negative electrode active materials for negative electrodes. For example, graphite has a layered structure in which carbon atom layers formed in a mesh structure are stacked. Therefore, graphite can allow lithium ions to enter the edge surface of the carbon layer (the surface where the layers overlap) during charging and diffuse between the layers, and release the diffused lithium ions from the edge surface of the carbon layer by deintercalation during discharge. In addition, graphite has a lower resistivity in the surface direction of the carbon layer than in the stacking direction of the carbon layer, so a conduction path for turning electrons is formed along the surface direction of the carbon layer.
[0006] In this regard, a technique has been proposed in the prior art for orienting the graphite contained in the negative electrode in a magnetic field to improve the charging performance of the negative electrode of a lithium secondary battery using a carbon material (such as graphite). Specifically, in its construction, the [0,0,2] crystal plane of the graphite is oriented in a magnetic field during the formation of the negative electrode so that it is almost vertical and fixed relative to the negative electrode current collector. In this case, the edge surface of the graphite carbon layer of the manufactured negative electrode faces the positive electrode active layer, which is conducive to the insertion and extraction of lithium ions, while shortening the conduction path of electrons, thereby improving the electronic conductivity of the negative electrode, which can improve the charging performance of the battery.
[0007] Meanwhile, when carbon materials (such as graphite) release lithium, the average potential is about 0.2 V (based on Li / Li + ), and the discharge potential is relatively flat. Therefore, the negative electrode containing graphite as the negative electrode active material has the advantage of high and constant secondary battery voltage. The capacity per unit mass of such a carbon material (such as graphite) is theoretically 372 mAh / g. However, since the capacity of the carbon material is increased to close to the theoretical capacity, it is difficult to further increase the capacity, and there is a limitation that it is difficult to increase the energy density of the manufactured negative electrode.
[0008] Therefore, various negative electrode active materials are being studied to improve the high capacity and energy density of lithium secondary batteries. For example, silicon materials such as silicon (Si) and silicon oxide (SiO2) have been studied recently because it has been found that silicon materials can reversibly adsorb and release a large amount of lithium by reacting with lithium compounds. Silicon materials have a theoretical maximum capacity of about 4020mAh / g (9800mAh / cc, specific gravity 2.23). This is a very large value compared to graphite-based materials, which means that silicon can be used as a high energy density and / or high capacity negative electrode material compared to graphite-based materials. However, silicon materials exhibit a large volume change (about 300%) during charge and discharge. Therefore, the electrode energy density of the negative electrode containing carbon materials and silicon materials as negative electrode active materials is high, but it has the limitation of low durability due to the significantly reduced adhesion between the negative electrode active layer and the negative electrode current collector. In particular, when the negative electrode is oriented so that the [0,0,2] crystal plane of graphite is almost horizontal relative to the negative electrode current collector, the carbon layer edge plane arrangement of the carbon material is significantly damaged and / or lost due to the large volume change of the silicon material. Therefore, the negative electrode is limited in that the charging characteristics and life characteristics of the negative electrode are significantly deteriorated when long-term charging and discharging are performed.
[0009] Therefore, there is a great need for negative electrode technology for lithium secondary batteries, which includes a combination of carbon and silicon materials as negative electrode active materials, which not only has excellent charge and discharge capacity and energy density but also exhibits high charge characteristics and life characteristics during long-term charge and discharge.
[0010] [Prior art literature]
[0011] [Patent Document]
[0012] Korean registered patent publication No.10-2020-0047287 Summary of the invention
[0013] [Technical issues]
[0014] An object of the present invention is to provide a negative electrode for a lithium secondary battery and a lithium secondary battery comprising the negative electrode, wherein the negative electrode comprises a carbon material and a silicon material together as negative electrode active materials, has excellent charge and discharge capacity and energy density, and exhibits high charge characteristics and life characteristics even during long-term charge and discharge.
[0015] [Technical solution]
[0016] In order to solve the above problems, in an exemplary embodiment, the present invention provides a negative electrode for a lithium secondary battery, comprising:
[0017] A negative electrode current collector; and
[0018] a negative electrode active layer, which is disposed on at least one side of the negative electrode current collector and comprises a carbon-based negative electrode active material and a silicon-based negative electrode active material,
[0019] The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1:
[0020] [Equation 1]
[0021] 0.5≤[OI a ] / [OI r ]<1.0
[0022] In equation 1,
[0023] OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation,
[0024] OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and
[0025] The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak at 2θ=77.5±0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0026] Here, the average particle size (Dc) of the carbon-based negative electrode active material is 5μm to 50μm, the average particle size (Ds) of the silicon-based negative electrode active material is 0.5μm to 10μm, and the average particle size ratio (Dc / Ds) of the carbon-based negative electrode active material to the silicon-based negative electrode active material can be 1 to 10.
[0027] In addition, the silicon-based negative electrode active material may be included in an amount of 1 wt % to 20 wt % based on the total weight of the negative electrode active material.
[0028] In addition, the carbon-based negative electrode active material may include one or more of natural graphite and artificial graphite.
[0029] In addition, the silicon-based negative electrode active material may include silicon (Si), silicon carbide (SiC) and silicon oxide (SiO q , wherein 0.8≤q≤2.5) is one or more of the following.
[0030] In addition, the negative electrode active layer may have a 150 mg / 25 cm 2 Up to 300mg / 25cm 2 The loading amount and the average thickness of 10μm to 100μm.
[0031] In addition, in an exemplary embodiment, the present invention provides a method for manufacturing a negative electrode for a lithium secondary battery, comprising:
[0032] applying a negative electrode slurry containing a carbon-based negative electrode active material and a silicon-based negative electrode active material to at least one side of a negative electrode current collector,
[0033] applying a magnetic field to the applied negative electrode slurry, and
[0034] The negative electrode slurry to which the magnetic field is applied is dried and roll-pressed to form a negative electrode active layer.
[0035] The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1:
[0036] [Equation 1]
[0037] 0.5≤[OI a ] / [OI r ]<1.0
[0038] In equation 1,
[0039] OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation,
[0040] OI arepresents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and
[0041] The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak at 2θ=77.5±0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0042] Here, the step of applying the magnetic field may be performed at a magnetic field strength of 3,000 G to 9,000 G, and may be performed for 1 second to 30 seconds.
[0043] In addition, the roll pressing may be performed under the conditions of a temperature of 20° C. to 35° C. and a pressure of 50 MPa to 200 MPa.
[0044] Furthermore, in an exemplary embodiment, the present invention provides a lithium secondary battery provided with an electrode assembly including a positive electrode, a negative electrode of the present invention, and a separator provided between the positive electrode and the negative electrode.
[0045] Here, the positive electrode may include a positive electrode collector and a positive electrode active layer, the positive electrode active layer being disposed on at least one side of the positive electrode collector and including at least one positive electrode active material of lithium metal oxides represented by the following Chemical Formula 1 and Chemical Formula 2:
[0046] [Chemical formula 1]
[0047] Li x [Ni y Co z Mn w M 1 v ]O2
[0048] [Chemical formula 2]
[0049] LiM 2 p Mn 1-p O4
[0050] In Chemical Formula 1 and Chemical Formula 2,
[0051] M 1 is at least one element selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo,
[0052] x, y, z, w, and v are respectively 1.0 ≤ x ≤ 1.30, 0.5 ≤ y < 1, 0 < z ≤ 0.3, 0 < w ≤ 0.3, and 0 ≤ v ≤ 0.1, where y + z + w + v = 1,
[0053] M 2 is Ni, Co, or Fe, and
[0054] 0.05 ≤ p ≤ 1.0.
[0055] In addition, in an exemplary embodiment, a method for manufacturing a lithium secondary battery is provided, which includes:
[0056] Activating a lithium secondary battery including an electrode assembly, the electrode assembly including a positive electrode, the negative electrode of the present invention, and a separator disposed between the positive electrode and the negative electrode;
[0057] where the alignment value (O.I a ) of the carbon-based negative electrode active material after activation of the negative electrode active layer is 3 or less and satisfies the following Equation 1:
[0058] [Equation 1]
[0059] 0.5 ≤ [O.I a / [O.I r < 1.0
[0060] In Equation 1,
[0061] O.I r represents the alignment value (O.I) of the carbon-based negative electrode active material measured before activation,
[0062] O.I a represents the alignment value (O.I) of the carbon-based negative electrode active material measured after activation, and
[0063] the alignment value (O.I) represents the ratio of the area integral value of the peak at 2θ = 54.7 ± 0.2° representing the [0,0,4] plane to the peak at 2θ = 77.5 ± 0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0064] Herein, the activation process can be performed by charging and discharging at a rate of 0.01C to 0.9C at least twice.
[0065] [Advantageous Effects]
[0066] The negative electrode for a lithium secondary battery of the present invention includes a carbon-based negative electrode active material and a silicon-based negative electrode active material together as the negative electrode active material, and exhibits excellent charge and discharge capacity and energy density characteristics. In addition, by making the alignment value (O.I a) is lower than the arrangement value (OI) of the carbon-based negative electrode active material before activation. r ), the negative electrode has the advantage of exhibiting high charging characteristics and life characteristics during long-term charge and discharge. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 2 are images showing the arrangement of ab-axis crystal planes of graphite depending on whether a magnetic field is applied to the negative electrode slurry during the formation of the negative electrode active layer, wherein (a) is a case where the crystal planes of graphite are not arranged due to no application of a magnetic field, and (b) is a case where the crystal planes of graphite are arranged due to application of a magnetic field. DETAILED DESCRIPTION
[0068] The invention is susceptible to various modifications and may have numerous embodiments, some of which are described in detail below.
[0069] However, this is not intended to limit the present invention to any specific embodiment, and should be construed to include all modifications, equivalents, or replacements falling within the scope of the idea and technology of the present invention.
[0070] The terms "comprising" or "having" are used herein to indicate the presence of features, numbers, steps, actions, components or members, or a combination thereof, described in the specification, and it should be understood that the possibility of the presence or addition of one or more other features, numbers, steps, actions, components, members, or a combination thereof is not excluded in advance.
[0071] Furthermore, when a portion of a layer, film, region, or plate is disposed “on” another portion, this includes not only a case where the portion is disposed “directly” “on” another portion, but also a case where a third portion is interposed therebetween. Conversely, when a portion of a layer, film, region, or plate is disposed “under” another portion, this includes not only a case where the portion is disposed “directly” “under” another portion, but also a case where a third portion is interposed therebetween. Furthermore, in the present application, “on” may include not only a case where it is disposed on an upper portion, but also a case where it is disposed on a lower portion.
[0072] In addition, in the present invention, "comprising ... as a main component" may refer to containing 50% by weight or more (or 50% by volume or more), 60% by weight or more (or 60% by volume or more), 70% by weight or more (or 70% by volume or more), 80% by weight or more (or 80% by volume or more), 90% by weight or more (or 90% by volume or more), or 95% by weight or more (or 95% by volume or more) of a defined component relative to the total weight (or total volume). For example, "comprising graphite as a main component of the negative electrode active material" may refer to containing at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 90% by weight, or at least 95% by weight of graphite based on the total weight of the negative electrode active material, and in some cases may refer to the entire negative electrode active material being composed of graphite and containing 100% of graphite.
[0073] In addition, as used herein, "carbon-based negative electrode active materials are oriented" or "carbon-based negative electrode active materials are arranged" may refer to certain crystal planes (such as the ab-axis crystal planes of graphite) representing the two-dimensional planar structure of the carbon-based negative electrode active materials constituting the negative electrode active material particles being arranged at a predetermined slope relative to the surface of the negative electrode current collector, which may be different from the carbon-based negative electrode active material particles themselves being oriented in a certain direction within the negative electrode active layer.
[0074] In addition, "highly oriented carbon-based negative electrode active material" may refer to certain crystal planes (e.g., ab-axis crystal planes of graphite) representing a two-dimensional planar structure of the carbon-based negative electrode active material contained in the negative electrode active layer having a higher frequency and a predetermined slope relative to the negative electrode current collector surface. In some cases, it may also refer to the crystal planes of the carbon-based negative electrode active material contained in the negative electrode active layer being arranged at a high angle (e.g., an angle close to vertical, greater than 45°; specifically, greater than 60°) relative to the negative electrode current collector surface.
[0075] In addition, "a high alignment value of a carbon-based negative electrode active material" means that the "alignment value (OI)" mentioned herein has a larger value, which may refer to certain crystal planes (e.g., ab-axis crystal planes of graphite) representing a two-dimensional planar structure of the carbon-based negative electrode active material contained in the negative electrode active layer being arranged at a low angle (e.g., less than 45°) relative to the surface of the negative electrode current collector. Conversely, "a low alignment value of a carbon-based negative electrode active material" may refer to "alignment value (OI)" having a smaller value, so that the crystal planes of the carbon-based negative electrode active material contained in the negative electrode active layer are arranged at a high angle (e.g., an angle close to vertical, greater than 45°; specifically, greater than 60°) relative to the surface of the negative electrode current collector.
[0076] In addition, as used herein, "a crystal plane of a carbon-based negative electrode active material" refers to a plane where the atoms of the carbon-based negative electrode active material form a crystal shape. In the present invention, it may refer to a crystal plane containing a plane of a carbon-based negative electrode active material, or a crystal plane containing an a-axis / b-axis / ab-axis of a carbon-based negative electrode active material crystal.
[0077] In addition, as used herein, the average particle size (D 50 The term “median diameter” refers to the particle size at which the integral value of the particle size distribution is 50%, also known as the median diameter.
[0078] The present invention will be described in more detail below.
[0079] Negative electrode for lithium secondary battery
[0080] In an exemplary embodiment, the present invention provides a negative electrode for a lithium secondary battery, comprising:
[0081] A negative electrode current collector; and
[0082] a negative electrode active layer, which is disposed on at least one side of the negative electrode current collector and comprises a carbon-based negative electrode active material and a silicon-based negative electrode active material,
[0083] The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1:
[0084] [Equation 1]
[0085] 0.5≤[OI a ] / [OI r ]<1.0
[0086] In equation 1,
[0087] OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation,
[0088] OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and
[0089] The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak at 2θ=77.5±0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0090] The negative electrode for lithium secondary battery of the present invention comprises a negative electrode current collector and a negative electrode active layer located on at least one side of the negative electrode current collector. The negative electrode active layer is a layer that realizes the electrical activity of the negative electrode and includes a negative electrode active material that realizes electrochemical redox reaction during charge and discharge of the battery.
[0091] Here, as the negative electrode active material contained in the negative electrode active layer, the present invention includes a carbon-based negative electrode active material having carbon atoms as a main component and a silicon-based negative electrode active material having silicon atoms as a main component.
[0092] The carbon-based negative electrode active material may have a layered structure in which carbon atom layers formed in a network structure are stacked. In a carbon-based negative electrode active material having such a structure, lithium ions can diffuse between layers by entering the edge face (the face of the layer stack) of the carbon layer during charging, and the diffused lithium ions during discharge can be released from the edge face of the carbon layer by deintercalation. Since the resistivity of the carbon-based negative electrode active material is lower in the surface direction of the carbon layer than in the stacking direction of the carbon layer, a conduction path for turning electrons is formed along the surface direction of the carbon layer.
[0093] Therefore, the present invention shortens the ion channel of lithium ions by controlling the crystal structure characteristics of the carbon-based negative electrode active material contained in the negative electrode active layer, and exhibits excellent charging performance by reducing the resistance in the surface direction of the carbon layer.
[0094] In one example, the carbon-based negative electrode active material included in the negative electrode active layer may have an arrangement value (OI) of 3.0 or less. a ), which represents the inclination degree of the ab axis crystal plane relative to the negative electrode current collector. Here, the arrangement value OI is the arrangement value calculated after the secondary battery is activated, which can be calculated by the following equation 3:
[0095] [Equation 3]
[0096] OI=I 004 / I 110
[0097] In equation 3,
[0098] I 004 It represents the peak area representing the [0,0,4] crystal plane in the X-ray diffraction spectrum (XRD) measurement of the negative electrode active layer.
[0099] I 110 It represents the peak area representing the [1,1,0] plane in the X-ray diffraction spectrum (XRD) measurement of the negative electrode active layer.
[0100] When measured by X-ray diffraction (XRD), the arrangement value (OI) of the carbon-based negative electrode active material can be an indicator of the degree to which the ab-axis crystal plane of the carbon-based negative electrode active material is oriented in a specific direction (specifically, relative to the surface of the negative electrode current collector). Specifically, in the X-ray diffraction measurement, for the carbon-based negative electrode active material graphite, the negative electrode active layer exhibits peaks at 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2° and 77.5±0.2°. These represent [0,0,2], [1,0,0], [1,0,1]R, [1,0,1]H, [0,0,4] and [1,1,0] faces of graphite. The peak at 2θ=43.4±0.2° can also be regarded as an overlap of the peak corresponding to the [1,0,1]R plane of the second carbon-based negative active material and the peak of the [1,1,1] plane of the current collector (eg, copper (Cu)).
[0101] Among them, the ratio of the areas obtained by integrating the corresponding intensities of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane and the peak at 2θ=77.5±0.2° representing the [1,1,0] plane can be used to measure the arrangement value (OI) of the second carbon-based negative electrode active material.
[0102] Since the peak at 2θ=54.7±0.2° is a peak representing a crystal plane having a slope with the negative current collector of the carbon-based negative electrode active material, the arrangement value (OI) may mean that when the value is close to 0, the slope relative to the surface of the negative electrode current collector is closer to 90°, and when the value is large, the slope relative to the surface of the negative electrode current collector is closer to 0° or 180°. In other words, the negative electrode active layer of the present invention may be arranged so that the carbon-based negative electrode active material has an angle of 60° or more, 70° or more, 70°-90°, 80°-90°, 65°-85° or 70°-85° relative to the negative electrode current collector. Therefore, compared with the case where the carbon-based negative electrode active material is arranged at a lower angle of less than 60°, the carbon-based negative electrode active material of the negative electrode active layer may have a lower arrangement value (OI).
[0103] As an example, the alignment value (OI) of the carbon-based negative electrode active material of the negative electrode active layer a ) may be 3.0 or less, more specifically, 0.1 to 3.0; 0.5 to 2.9; 1.0 to 2.9; 1.5 to 2.9; 1.8 to 2.9; 1.7 to 2.7; 1.8 to 2.3; 2.2 to 2.8; or 1.9 to 2.5. Here, the arrangement value (OI) indicates the degree of arrangement of the ab-axis crystal plane of the carbon-based negative electrode active material, and does not indicate the degree to which the carbon-based negative electrode active material particles are arranged by rotating themselves in the active layer.
[0104] In addition, the negative electrode active layer includes a silicon-based negative electrode active material. The silicon-based negative electrode active material has a theoretical maximum capacity of about 4020mAh / g, which can be used as a high energy density and / or high capacity negative electrode material. However, the silicon-based negative electrode active material exhibits a large volume change (about 300%) during charge and discharge, which may reduce the durability of the electrode. In particular, when the ab-axis crystal plane of the carbon-based negative electrode active material is oriented almost horizontally relative to the negative electrode current collector in order to improve the charging performance of the negative electrode active layer, the silicon-based negative electrode active material may be significantly damaged and / or lose its arrangement during charge and discharge. This orientation damage of the carbon-based negative electrode active material can significantly reduce the charging characteristics and life characteristics of the negative electrode during the long-term charge and discharge of the secondary battery.
[0105] However, the negative electrode of the present invention can be obtained by adjusting the arrangement value (OI) of the activated carbon-based negative electrode active material. a ) is realized to be lower than the arrangement value (OI) of the carbon-based negative electrode active material before activation. r ) to overcome the problems caused by silicon-based negative electrode active materials.
[0106] In one example, the arrangement value (OI) of the carbon-based negative electrode active material after activation is a ) is smaller than the arrangement value (OI) of the carbon-based negative electrode active material before activation. r ), so that the ratio of the arrangement values is greater than 0.5 and less than 1, so that the negative electrode satisfies equation 1:
[0107] [Equation 1]
[0108] 0.5≤[OI a ] / [OI r ]<1.0
[0109] In equation 1,
[0110] OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation,
[0111] OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and
[0112] The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak at 2θ=77.5±0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0113] Equation 1 indicates that after activation, the ab axis crystal plane of the carbon-based negative electrode active material is arranged with a higher slope relative to the negative electrode current collector. In other words, the orientation of the carbon-based negative electrode active material in the negative electrode active layer is improved by activation of the secondary battery.
[0114] Activation is the step of electrically activating a lithium secondary battery, which provides a pathway for lithium ions to migrate through the negative electrode active layer during charge and discharge. Lithium ions are intercalated between the layers of the carbon-based negative electrode active material and the crystals of the silicon-based negative electrode active material during charge, and deintercalated during discharge. Therefore, activation can be defined as a process that ensures such an intercalation and deintercalation pathway for lithium ions. Here, the carbon-based negative electrode active material may have the following characteristics: the ab-axis crystal plane is oriented with a high slope close to vertical relative to the negative electrode current collector, such as Figure 1 As shown, this shortens the travel path of lithium ions generated from the positive electrode active layer. However, if the secondary battery is subjected to long-term charge and discharge, volume changes due to the insertion and extraction of lithium ions in the carbon-based negative electrode active material may occur continuously. In addition, the silicon-based negative electrode active material located between the carbon-based negative electrode active materials undergoes volume expansion due to the insertion of lithium ions during charging. This contraction and expansion of the negative electrode active material can reduce the slope of the crystal plane of the carbon-based negative electrode active material relative to the negative electrode current collector.
[0115] Therefore, the negative electrode of the present invention can ensure the migration path of lithium ions while minimizing the damage and / or loss of the slope of the ab-axis crystal plane of the carbon-based negative electrode active material contained in the negative electrode active layer relative to the negative electrode current collector during activation. The migration path of lithium ions thus determined is robust, so that even if the secondary battery is charged and discharged for a long time, the deformation is very small, and the possibility of damage and / or loss of the arrangement of the carbon-based negative electrode active material in the negative electrode active layer is significantly reduced.
[0116] The negative electrode of the present invention can be implemented so that the arrangement value (OI) of the activated carbon-based negative electrode active material a ) is lower than the arrangement value (OI) of the carbon-based negative electrode active material before activation. r ), thus satisfying Equation 1, i.e., greater than or equal to 0.5 and less than 1.0 (i.e., 0.5≤[OI a ] / [OI r ]<1.0). Specifically, the negative electrode may satisfy Equation 1, wherein 0.5 is greater than or equal to 0.5 and less than or equal to 0.95 (ie, 0.5≤[OI a ] / [OI r ]≤0.95), more specifically, the negative electrode may satisfy Equation 1, wherein is greater than or equal to 0.6 and less than or equal to 0.95 (ie, 0.6≤[OI a ] / [OI r ]≤0.95); 0.65 to 0.75 (i.e., 0.65≤[OIa ] / [OI r ]≤0.75); 0.85 to 0.95 (i.e., 0.85≤[OI a ] / [OI r ]≤0.95); 0.70 to 0.93 (i.e., 0.70≤[OI a ] / [OI r ]≤0.93); or 0.72 to 0.90 (i.e., 0.72≤[OI a ] / [OI r ]≤0.90). Therefore, the negative electrode of the present invention exhibits excellent charging characteristics and life characteristics during long-term charge and discharge of the secondary battery.
[0117] In addition, the present invention can control the type, shape, particle size, content, etc. of the carbon-based negative electrode active material and the silicon-based negative electrode active material contained in the negative electrode active layer to meet predetermined conditions, thereby ensuring the migration path of lithium ions in the negative electrode active layer during the activation process of the secondary battery.
[0118] First, the carbon-based negative electrode active material may include graphite. Graphite may include natural graphite or artificial graphite. For example, the first carbon-based negative electrode active material and the second carbon-based negative electrode active material may include natural graphite or artificial graphite alone, or in some cases include a mixture of natural graphite and artificial graphite. In this case, the weight ratio of natural graphite to artificial graphite may be 5-50:50-95 or 10-40:60-90. By including natural graphite and artificial graphite in a mixing ratio as described above, the carbon-based negative electrode active material can achieve a higher orientation of the carbon-based negative electrode active material relative to the surface of the negative electrode collector while enhancing the adhesion of the negative electrode collector and the negative electrode active layer.
[0119] In one example, the carbon-based negative active material may include natural graphite and artificial graphite in a weight ratio of 10-30:70-90.
[0120] In another example, the carbon-based negative active material may include natural graphite and artificial graphite in a weight ratio of 25-45:55-75.
[0121] In yet another example, the carbon-based negative active material may include only artificial graphite.
[0122] In addition, the carbon-based negative electrode active material is preferably a spherical graphite assembly formed by agglomeration of multiple flake graphites. Flake graphite includes natural graphite, artificial graphite, calcined carbon (bulk mesophase) based on tar and pitch, graphitized coke (raw coke, green coke, pitch coke, needle coke, petroleum coke, etc.), and preferably a variety of highly crystalline natural graphite assemblies are used. In addition, a graphite assembly can be formed by assembling 2 to 100 pieces, preferably 3 to 20 pieces of flake graphite.
[0123] Such carbon-based negative electrode active materials may have a spherical particle shape. In this case, the sphericity of the graphite particles may be greater than or equal to 0.75, for example, 0.75 to 1.0; 0.75 to 0.95; 0.8 to 0.95; or 0.90 to 0.99. As used herein, "sphericity" may refer to the ratio of the shortest diameter (short diameter) to the longest diameter (long diameter) of any diameter passing through the center of the particle. A sphericity of 1 means that the shape of the particle is spherical. Sphericity can be determined by measuring the sphericity using a particle shape analyzer; or measuring the shape of the particles using a scanning electron microscope (SEM), an energy dispersive spectrometer, etc., and then analyzing the measurement results.
[0124] The present invention can achieve high conductivity of the negative electrode active layer by making the shape of the carbon-based negative electrode active material close to spherical. Therefore, the negative electrode containing the spherical carbon-based negative electrode active material can increase the capacity of the secondary battery and has the advantage of increasing the specific surface area per unit weight of the negative electrode active material, which can improve the adhesion between the negative electrode active layer and the current collector.
[0125] In addition, examples of silicon-based negative electrode active materials may include silicon (Si), silicon carbide (SiC), silicon monoxide (SiO) or silicon dioxide (SiO2), which may be included in the negative electrode active layer alone or in combination. When silicon monoxide (SiO) and silicon dioxide (SiO2) are uniformly mixed or compounded and included in the negative electrode active layer as silicon-based negative electrode active materials, they may be labeled as silicon oxide (SiO q , where 0.8≤q≤2.5).
[0126] In addition, the silicon-based negative electrode active material can be doped with or alloyed with Li, Mg, Al, Ca, Ti, etc. In addition, in order to suppress the volume expansion during charging in the presence of oxygen (O) and improve the conductivity of the negative electrode active material, the silicon-based negative electrode active material can be surface treated with a carbon coating or the like.
[0127] In addition, the carbon-based negative electrode active material and the silicon-based negative electrode active material (ie, all negative electrode active materials) in the negative electrode active layer may account for at least 85 parts by weight of the negative electrode active layer, more specifically, at least 90 parts by weight, at least 93 parts by weight, or at least 95 parts by weight.
[0128] In addition, relative to the total weight of all negative electrode active materials, the content of the silicon-based negative electrode active material can be 1 to 20 weight%, more specifically 5 weight % to 20 weight %, 1 weight % to 9 weight %, 5 weight % to 15 weight %, 3 weight % to 7 weight %, 11 weight % to 19 weight %, 13 weight % to 17 weight %, 15 weight % to 20 weight %, 8 weight % to 14 weight %, or 5 weight % to 9 weight %. By adjusting the total content ratio of all negative electrode active materials contained in the negative electrode active layer and the content ratio of the silicon-based negative electrode active material contained in all negative electrode active materials to the above range, the present invention can increase the charging capacity per unit mass while reducing lithium consumption and irreversible capacity loss during the activation process of the secondary battery. In addition, by minimizing the volume change of the negative electrode active layer during the charge and discharge of the secondary battery, the structural stability of the negative electrode active layer can be improved, thereby improving the life characteristics of the secondary battery.
[0129] In addition, the carbon-based negative electrode active material and the silicon-based negative electrode active material contained in the negative electrode active layer may have a predetermined average particle size (D 50 Specifically, the average particle size (D 50 , Dc) can be 5 μm to 50 μm, and the average particle size of the silicon-based negative electrode active material (D 50 , Ds) can be 0.5 μm to 10 μm, and the average particle size ratio (Dc / Ds) of the carbon-based negative electrode active material to the silicon-based negative electrode active material can be 1 to 10.
[0130] Specifically, the carbon-based negative electrode active material may exhibit an average particle size (D 50 , Dc), and can be selectively applied within this range to match the average thickness of the negative electrode active layer. For example, the average particle size (D 50 ) can be from 5μm to 40μm; from 5μm to 30μm; from 10μm to 40μm; from 15μm to 30μm; from 25μm to 50μm; from 11μm to 19μm; from 15μm to 25μm; from 20μm to 30μm; from 5μm to 20μm; from 5μm to 10μm; from 5μm to 15μm; from 10μm to 20μm; from 15μm to 30μm; from 15μm to 20μm; from 21μm to 26μm; from 25μm to 30μm; from 11μm to 17μm; from 16μm to 23μm; from 5μm to 9μm; from 14μm to 17μm; or from 16μm to 19μm.
[0131] Spherical carbon-based negative electrode active materials can benefit from a smaller particle diameter to maximize the disorder of each particle in the expansion direction, thereby preventing the particles from expanding when charged with lithium ions. However, if the particle size of the carbon-based negative electrode active material is less than 5.0 μm, a large amount of binder is required due to the increase in the number of particles per unit volume, and the sphericity and spheroidization yield may be low. On the other hand, if the average particle size exceeds 50 μm, the expansion rate of the negative electrode active material increases significantly during the charge and discharge of the secondary battery, and thus the cohesion between the negative electrode active material particles decreases; and the cohesion between the negative electrode active material particles and the current collector may decrease with repeated charge and discharge, resulting in a significant decrease in the cycle characteristics.
[0132] In addition, the average particle size (D 50 , Ds) can be 0.5μm to 10μm, more specifically 0.5μm to 5μm; 0.5μm to 3μm; 0.5μm to 2μm; 0.5μm to 1μm; 1μm to 5μm; 3μm to 7μm; 5μm to 10μm; 1μm to 3μm; 4μm to 9μm; 0.8μm to 1.2μm; or 6μm to 9.5μm.
[0133] When the average particle size of the silicon-based negative electrode active material is less than 0.5 μm, it is difficult to make the second negative electrode active layer uniformly dispersed, and as the secondary battery is charged and discharged, the redox reaction of the agglomerated area and the non-agglomerated area of the silicon-based negative electrode active material occurs unevenly, which may lead to the degradation of the second negative electrode active layer. In addition, when the average particle size of the silicon-based negative electrode active material exceeds 10 μm, the volume expansion of the silicon-based negative electrode active material increases significantly during the charging process, thereby reducing the slope of the ab axis crystal plane of the carbon-based negative electrode active material (i.e., increasing the arrangement value (OI)), resulting in a significant decrease in the cycle characteristics as the secondary battery is repeatedly charged and discharged.
[0134] In addition, the average particle size ratio (Dc / Ds) of the carbon-based negative electrode active material and the silicon-based negative electrode active material may be 1 to 10, more specifically 2 to 7; 2 to 5; 3 to 7; 4 to 8; 5 to 10; 6 to 9; or 1.5 to 4.7.
[0135] By satisfying the average particle size ratio (Dc / Ds) of the carbon-based negative electrode active material and the silicon-based negative electrode active material within the above range, the present invention can induce a structure in which the silicon-based negative electrode active material is filled in the gaps formed by multiple carbon-based negative electrode active materials. In this case, the gap acts as a buffer to buffer the volume expansion of the silicon-based negative electrode active material during the charge and discharge process of the secondary battery, so that the volume expansion of the negative electrode active layer can be minimized. In addition, if the average particle size ratio (Dc / Ds) exceeds the upper limit of the above range, the degradation of the negative electrode active layer will be accelerated during the charge and discharge of the secondary battery, resulting in a shortened life.
[0136] Meanwhile, the average thickness of the negative electrode active layer may be 10 μm to 100 μm, more specifically 20 μm to 90 μm; 50 μm to 90 μm; 80 μm to 90 μm; 40 μm to 70 μm; 55 μm to 68 μm.
[0137] In addition, the average loading of the negative electrode active layer can be 150 mg / 25 cm 2 Up to 300mg / 25cm 2 , more specifically 180mg / 25cm 2 Up to 280mg / 25cm 2 ; 180mg / 25cm 2 Up to 250mg / 25cm 2 ; 200mg / 25cm 2 Up to 250mg / 25cm 2 ; or 200mg / 25cm 2 Up to 220mg / 25cm 2 .
[0138] By adjusting the average thickness and / or the average loading amount of the negative electrode active layer to the above range, the crystallinity of the negative electrode active material contained in the negative electrode active layer can be easily controlled, and the energy density of the negative electrode can be further increased.
[0139] Furthermore, the negative electrode active layer of the present invention may optionally include a conductive material, a binder, other additives, etc., in addition to the negative electrode active material as a main component, as required.
[0140] The conductive material may include one or more of carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, etc., but is not limited thereto.
[0141] In one example, the negative electrode active layer may include carbon black, carbon nanotubes, carbon fibers, etc., alone or in combination, as the conductive material.
[0142] In this case, the content of the conductive material may be 0.1 to 10 parts by weight, more specifically 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, 2 to 6 parts by weight, or 0.5 to 2 parts by weight, based on a total of 100 parts by weight of the negative electrode active layer. By controlling the content of the conductive material within the range as described above, the present invention can prevent the resistance of the negative electrode from increasing due to the low content of the conductive material and reducing the charge capacity, and can prevent the content of the negative electrode active material from decreasing due to excessive conductive material to cause a decrease in charge capacity, or prevent the rapid charge characteristics from decreasing due to an increase in the load amount of the negative electrode active layer.
[0143] In addition, the binder can be suitably applied as a component that helps the bonding of the negative electrode active material to the conductive material and to the current collector, and its degree does not reduce the electrical properties of the electrode. Specifically, the binder may include one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber (SBR) and fluorinated rubber.
[0144] Based on a total of 100 parts by weight of the negative electrode active layer, the content of the binder may be 0.1 to 10 parts by weight, more specifically 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, or 2 to 6 parts by weight. By controlling the content of the binder contained in the negative electrode active layer within the above range, the present invention can prevent the adhesion degradation of the active layer caused by the low content of the binder, or prevent the degradation of the electrical properties of the electrode caused by the excessive amount of the binder.
[0145] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used, and in the case of copper or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can also be used. In addition, considering the conductivity and total thickness of the manufactured negative electrode, the average thickness of the negative electrode current collector can be appropriately adopted to be 1 to 500 μm.
[0146] Method for manufacturing negative electrode for lithium secondary battery
[0147] In addition, in an exemplary embodiment, the present invention provides a method for manufacturing a negative electrode for a lithium secondary battery, comprising:
[0148] applying a negative electrode slurry containing a carbon-based negative electrode active material and a silicon-based negative electrode active material to at least one side of a negative electrode current collector,
[0149] applying a magnetic field to the applied negative electrode slurry, and
[0150] The negative electrode slurry to which the magnetic field is applied is dried and roll-pressed to form a negative electrode active layer.
[0151] The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1:
[0152] [Equation 1]
[0153] 0.5≤[OIa ] / [OI r ]<1.0
[0154] In equation 1,
[0155] OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation,
[0156] OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and
[0157] The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak at 2θ=77.5±0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0158] The method for manufacturing the negative electrode of the present invention refers to a method for manufacturing the negative electrode of the present invention described above. The method for manufacturing the negative electrode can be performed by applying a negative electrode slurry on a negative electrode current collector, applying a magnetic field to the surface of the applied negative electrode slurry, and drying and rolling each negative electrode slurry to form a negative electrode active layer.
[0159] Here, the step of applying the negative electrode slurry includes coating the surface of the moving negative electrode current collector by releasing the negative electrode slurry containing the carbon-based negative electrode active material. The above steps can be implemented in any manner conventionally applied in the art without limitation, but preferably a die coating method can be used. The die coating method can be performed by a slit die having a gasket for controlling the release conditions of the negative electrode slurry. In this case, by controlling the shape of the gasket, the load amount, coating thickness, etc. of the negative electrode slurry applied to the negative electrode current collector can be easily controlled.
[0160] In addition, the negative electrode slurry may include a carbon-based negative electrode active material and a silicon-based negative electrode active material as main components, and may optionally further include a conductive material, a binder, other additives, etc. as needed. In this case, the carbon-based negative electrode active material and the silicon-based negative electrode active material and the conductive material, the binder, other additives, etc. have the same composition as the composition of the negative electrode for the above-mentioned lithium secondary battery, so a detailed description is omitted.
[0161] In addition, the step of applying a magnetic field to the negative electrode slurry may be a process of controlling the crystal properties of the negative electrode active material contained in the negative electrode slurry to reduce the disorder of the carbon-based negative electrode active material contained in the negative electrode slurry. Specifically, the step may include applying a magnetic field to the surface of the negative electrode slurry applied to the negative electrode current collector so that the ab-axis crystal planes of the carbon-based negative electrode active material contained in each negative electrode slurry are arranged at a high angle relative to the negative electrode current collector.
[0162] In this case, the application of the magnetic field can be performed by the magnetic components provided on the upper and lower parts of the negative electrode collector, and the negative electrode collector moves along with the negative electrode slurry applied to its surface. In addition, the polarities of the magnetic components provided on the upper and lower parts can be different from each other.
[0163] In addition, the arrangement value (OI) of the carbon-based negative electrode active material contained in the negative electrode slurry can be adjusted by the applied magnetic field strength, application time, etc., so that the step of applying the magnetic field can be performed under predetermined magnetic field strength and application time conditions.
[0164] Specifically, the step of applying a magnetic field can apply a magnetic field of less than 10,000G (Gauss), more specifically 3,000G to 9,000G; 3,000G to 8,500G; 3,500G to 8,500G; 4,000G to 8,200G; 3,600G to 4,500G; 4,500G to 6,500G; 5,000G to 7,000G; 6,000G to 8,500G; 7,000G to 8,500G; 6,000G to 6,500G; 4,000G to 5,000G.
[0165] In addition, the step of applying a magnetic field can be performed for a time of 1 second to 30 seconds, more specifically 1 second to 20 seconds; 1 second to 15 seconds; 1 second to 10 seconds; 5 seconds to 20 seconds; 10 seconds to 20 seconds; 11 seconds to 19 seconds; 14 seconds to 18 seconds; 4 seconds to 9 seconds; or 6 seconds to 11 seconds.
[0166] In one example, the step of applying a magnetic field may include applying a magnetic field of 4,700±50 G to the negative electrode slurry for 3 to 8 seconds.
[0167] In another example, the step of applying the magnetic field may include applying a magnetic field of 4,700±50 G to the negative electrode slurry for 12 seconds to 17 seconds.
[0168] In addition, the step of applying a magnetic field can be performed by introducing magnetic components at the upper and lower parts of the applied negative electrode slurry, wherein the size of the magnetic components is controlled to be larger than the size of the negative electrode slurry. For example, the length ratio of the magnetic component can be 105% to 200% based on the length in the width direction of the negative electrode slurry, and more specifically, the length ratio can be 110% to 180%; 110% to 160%; 110% to 140%; 110% to 130%; 130% to 150%; or 105% to 120% based on the length in the width direction of the negative electrode slurry. In this case, the magnetic field applied to the negative electrode slurry is uniformly applied to the entire surface of the negative electrode slurry, which can produce a uniform arrangement value (OI) of the carbon-based negative electrode active material.
[0169] In addition, the step of forming the negative electrode active layer may refer to a process of drying and rolling the negative electrode slurry to which the magnetic field is applied to firmly fix the oriented carbon-based negative electrode active material. Therefore, the step of forming the negative electrode active layer may be implemented without limitation as long as it is any method capable of maintaining the arrangement value (OI) of the carbon-based negative electrode active material contained in the negative electrode active layer.
[0170] For example, the drying may be performed by applying heat energy to the negative electrode slurry using a hot air dryer, a vacuum oven, or the like to dry the negative electrode slurry.
[0171] In addition, roll pressing is a step of increasing the density of the negative electrode active layer by applying pressure to the dried negative electrode slurry using a roll press, etc. In this case, the roll pressing may be performed without increasing the arrangement value (OI) of the carbon-based negative electrode active material of the dried negative electrode slurry.
[0172] Specifically, the roll pressing may be performed at a temperature close to room temperature, and more specifically, the roll pressing may be performed at a temperature of 20°C to 35°C, 20°C to 30°C, or 20°C to 25°C.
[0173] In addition, rolling can be carried out at a rolling speed of 2m / s to 7m / s, and more specifically at a rolling speed of 2m / s to 6.5m / s, 2m / s to 6m / s, 2m / s to 5.5m / s, 2m / s to 5m / s, 2m / s to 4.5m / s, 2m / s to 4m / s, 2.5m / s to 4m / s, 2.5m / s to 3.5m / s, 3.5m / s to 5m / s, 5m / s to 7m / s, 5.5m / s to 6.5m / s or 6m / s to 7m / s.
[0174] In addition, the rolling may be performed under a pressure condition of 50 MPa to 200 MPa, more specifically, 50 MPa to 150 MPa, 50 MPa to 100 MPa, 100 MPa to 200 MPa, 150 MPa to 200 MPa, or 80 MPa to 140 MPa.
[0175] By rolling the dried negative electrode slurry under the above temperature, speed and / or pressure conditions, the present invention can increase the energy density of the negative electrode while minimizing the variation in the arrangement value of the carbon-based negative electrode active material contained in the formed negative electrode active layer.
[0176] As an example, the carbon-based negative electrode active material of the negative electrode active layer formed by the above conditions can have a minimum arrangement value change, so that the arrangement value (OI) of the carbon-based negative electrode active material after rolling is r ) may be less than 5, and may satisfy the following equation 2:
[0177] [Equation 2]
[0178] 0.1≤[OI c ] / [OI r ]≤0.7
[0179] In equation 2
[0180] OI c represents the arrangement value (OI) of the carbon-based negative electrode active material measured before rolling of the negative electrode active layer,
[0181] OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured after rolling of the negative electrode active layer, and
[0182] The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the [0,0,4] plane to the peak at 2θ=77.5±0.2° representing the [1,1,0] plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
[0183] Specifically, the arrangement value (OI) of the carbon-based negative electrode active material after rolling of the negative electrode active layer r ) can be 4.5 or less, 4.0 or less, 1.0 to 4.0, 2.0 to 4.0, 2.0 to 3.5, 2.0 to 3.0, 2.0 to 3.0, 3.0 to 4.0, 3.0 to 3.5, 1.8 to 2.5, or 1.8 to 3.4.
[0184] In addition, the negative electrode active layer can satisfy Equation 2, which represents the ratio of the arrangement values of the carbon-based negative electrode active material before and after rolling (OI c / OI r ) is 0.1 to 0.7 (i.e. 0.1≤[OI c ] / [OI r ]≤0.7), more specifically 0.1 to 0.65 (i.e. 0.1≤[OI c ] / [OI r ]≤0.65); 0.3 to 0.65 (i.e. 0.3≤[OI c ] / [OI r ]≤0.65); 0.4 to 0.65 (i.e. 0.4≤[OI c ] / [OI r ]≤0.65); 0.50 to 0.63 (i.e. 0.50≤[OI c ] / [OI r ]≤0.63); 0.45 to 0.55 (i.e. 0.45≤[OI c ] / [OI r]≤0.55); or 0.55 to 0.65 (i.e. 0.55≤[OI c ] / [OI r ]≤0.65).
[0185] The method of manufacturing a negative electrode for a lithium secondary battery of the present invention has the above configuration, which can manufacture a negative electrode having excellent charge and discharge capacity and energy density and having high charge characteristics and life characteristics during long-term charge and discharge of a secondary battery.
[0186] Lithium secondary battery
[0187] Furthermore, in an exemplary embodiment, the present invention provides a lithium secondary battery including an electrode assembly including a positive electrode, the negative electrode of the present invention as described above, and a separator disposed between the positive electrode and the negative electrode.
[0188] The lithium secondary battery of the present invention includes an electrode assembly, in which a plurality of positive electrodes and a plurality of negative electrodes are alternately arranged and a separator is located therebetween. The lithium secondary battery having the negative electrode of the present invention has excellent charge and discharge capacity and energy density, and has excellent charge and discharge characteristics and life characteristics even under long-term charge and discharge, and can therefore be used as a power source for medium and large-sized equipment such as electric vehicles.
[0189] In this case, the negative electrode has the same configuration as described above, and thus a detailed description is omitted.
[0190] In addition, the positive electrode may include a positive electrode active layer including a positive electrode active material on a positive electrode current collector, and the positive electrode active layer may optionally further include a conductive material, a binder, other additives, etc. as needed.
[0191] The positive electrode active material may include one or more of lithium metal oxides represented by the following Chemical Formula 1 and Chemical Formula 2, which can undergo an electrochemical reaction on the positive electrode current collector to reversibly intercalate and deintercalate lithium ions:
[0192] [Chemical formula 1]
[0193] Li x [Ni y Co z Mn w M 1 v ]O2
[0194] [Chemical formula 2]
[0195] LiM 2 p Mn q P r O4
[0196] In Chemical Formulas 1 and 2,
[0197] M 1 is at least one element selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo,
[0198] x, y, z, w, and v are respectively 1.0 ≤ x ≤ 1.30, 0.5 ≤ y < 1, 0 < z ≤ 0.3, 0 < w ≤ 0.3, and 0 ≤ v ≤ 0.1, where y + z + w + v = 1,
[0199] M 2 is Ni, Co, or Fe, and
[0200] p is 0.05 ≤ p ≤ 1.0, q is 2 - p, and r is from 0 to 1.
[0201] The lithium metal oxides represented by Chemical Formulas 1 and 2 are materials respectively containing high contents of nickel (Ni) and manganese (Mn), and when used as a positive electrode active material, compared with conventionally used positive electrode active materials such as lithium iron phosphate (LiFeO4), have the advantage of being able to stably supply high-capacity and / or high-voltage electric power.
[0202] In this case, the lithium metal oxide represented by Chemical Formula 1 may include LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2, LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2, etc., and the lithium metal oxide represented by Chemical Formula 2 may include LiNi 0.7 Mn 1.3 O4, LiNi 0.5 Mn 1.5 O4, LiNi 0.3 Mn 1.7O4, etc., which can be used alone or in combination.
[0203] In addition, the positive electrode active material may be contained in an amount of at least 85 parts by weight, and more specifically at least 90 parts by weight, at least 93 parts by weight, or at least 95 parts by weight, based on the weight of the positive electrode active layer.
[0204] Furthermore, the positive electrode active layer may further include a conductive material, a binder, other additives, and the like in addition to the positive electrode active material.
[0205] In this case, the conductive material used to improve the electrical properties of the positive electrode can be any material conventionally used in the art, but more specifically can include at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, denka black, ketjen black, Super-P, channel black, furnace black, lamp black, summer black, graphene and carbon nanotubes.
[0206] In addition, based on a total of 100 parts by weight of each positive electrode active layer, the content of the conductive material is 0.1-5 parts by weight, more specifically, based on a total of 100 parts by weight of each positive electrode active layer, the content of the conductive material is 0.1 to 4 parts by weight; 2 to 4 parts by weight; 1.5 to 5 parts by weight; 1 to 3 parts by weight; 0.1 to 2 parts by weight; or 0.1 to 1 part by weight.
[0207] In addition, the binder is used to bind the positive active material, the positive electrode additive and the conductive material to each other, and can be used without restriction as long as it has this function. Specifically, the binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate and copolymers thereof. In one example, the binder may include polyvinylidene fluoride.
[0208] In addition, the content of the binder may be 1 to 10 parts by weight based on a total of 100 parts by weight of each positive electrode active layer, more specifically, 2 to 8 parts by weight or 1 to 5 parts by weight based on a total of 100 parts by weight of each positive electrode active layer.
[0209] The total thickness of the positive electrode active layer is not particularly limited, but may be 50 to 300 μm, more specifically 100 to 200 μm; 80 to 150 μm; 120 to 170 μm; 150 to 300 μm; 200 to 300 μm; or 150 to 190 μm.
[0210] In addition, as the positive electrode current collector, the positive electrode can use a positive electrode current collector having high conductivity and not causing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can also be used. In addition, considering the conductivity and total thickness of the positive electrode to be manufactured, the average thickness of the current collector can be appropriately 3 μm to 500 μm.
[0211] In addition, the separator placed between the positive electrode and the negative electrode of each unit cell is an insulating film with high ion permeability and mechanical strength, and it is not particularly limited as long as it is those conventionally used in the art, but may include one or more polymers, such as chemically resistant and hydrophobic polypropylene; polyethylene; polyethylene-propylene copolymer. The separator may be in the form of a porous polymer substrate, such as a sheet or non-woven fabric including the above polymers, and in some cases may be in the form of a composite separator in which organic or inorganic particles are coated on a porous polymer substrate by an organic binder. In addition, the separator may have an average pore size of 0.01 to 10 μm and an average thickness of 5 to 300 μm.
[0212] Meanwhile, the lithium secondary battery of the present invention may be shaped into but not specifically limited to include a stacked, zigzag or zigzag-stacked electrode assembly. As an example, the lithium secondary battery of the present invention may be a pouch-type secondary battery or a prismatic secondary battery.
[0213] Pouch-type and / or prismatic secondary batteries have an advantage of being highly exploitable in terms of energy density because they can pack high-density secondary batteries within a limited space.
[0214] Method for manufacturing lithium secondary battery
[0215] In addition, in one embodiment, the present invention provides a method for manufacturing the above-mentioned lithium secondary battery.
[0216] The method for manufacturing a lithium secondary battery of the present invention comprises: inserting an electrode assembly including a positive electrode, a negative electrode of the present invention and a separator disposed between the positive electrode and the negative electrode into a battery case; injecting a nonaqueous electrolyte; and activating the assembled lithium secondary battery.
[0217] The activation step may refer to electrically activating the lithium secondary battery and providing a pathway for lithium ions to migrate into the negative electrode active layer during charge and discharge.
[0218] Here, the present invention may be performed under certain conditions to ensure that the slope of the ab-axis crystal plane of the carbon-based negative electrode active material contained in the negative electrode active layer relative to the negative electrode current collector during secondary battery activation minimizes damage and / or loss to the migration path of lithium ions.
[0219] Specifically, the activation step may be performed under a constant current condition of less than 1 C rate for two or more charge and discharge cycles. More specifically, the activation step may be performed under a constant current condition of a C rate of 0.01C to 0.9C, 0.01C to 0.75C, 0.01C to 0.5C, 0.05C to 0.5C, or 0.05C to 0.3C. In addition, the activation step may be performed at least 2 times, at least 3 times, at least 4 times, at least 2 to 5 times, or at least 2 to 4 times of charge and discharge.
[0220] By performing multiple charge and discharge cycles at a low current density of less than 1C during the activation of the secondary battery, the present invention can ensure the migration path of lithium ions while minimizing the change in the arrangement value of the ab-axis crystal plane of the carbon-based negative electrode active material contained in the negative electrode active layer. The lithium ion migration path thus determined can reduce the shrinkage and expansion of the carbon-based negative electrode active material and the silicon-based negative electrode active material during the charge and discharge after activation. Therefore, the lithium secondary battery of the present invention can exhibit excellent charge and discharge characteristics and life characteristics, because the change can enable the carbon-based negative electrode active material to maintain a higher ab-axis crystal plane orientation even when charged and discharged for a long time.
[0221] Hereinafter, the present invention will be described in more detail through examples and experimental examples.
[0222] However, the following embodiments and experimental examples are examples of the present invention, and the present invention is not limited to the following embodiments and experimental examples.
[0223] Examples 1 to 3 and Comparative Examples 1 to 6: Preparation of lithium secondary batteries
[0224] Preparation of negative electrode
[0225] As a carbon-based negative electrode active material, natural graphite (average particle size (D 50 ): 18±1μm) and artificial graphite (average particle size (D 50 ): 16±1 μm); as a silicon-based negative electrode active material, silicon oxide (SiO2) was prepared; and a negative electrode slurry was prepared using the prepared carbon-based negative electrode active material and the silicon-based negative electrode active material.
[0226] Specifically, a mixed graphite (average particle size (D 50 ): about 17 μm) and silicon oxide (SiO2) were mixed in a weight ratio as shown in Table 1 to prepare a negative electrode active material. 95 parts by weight of the prepared negative electrode active material, 1 part by weight of carbon black as a conductive material, 1.5 parts by weight of carboxymethyl cellulose (CMC) as a binder, and 2.5 parts by weight of styrene butadiene rubber (SBR) were mixed with water to achieve a solid content of 50% to prepare a negative electrode slurry.
[0227] Once the negative electrode slurry was prepared, it was cast on a copper sheet (thickness: 10 μm) in roll-to-roll transport (transport speed: 5 m / min) using a dual die coater. At this time, the loading amount of the applied negative electrode slurry was 208-210 mg / 25 cm 2 .
[0228] A permanent magnet having a length ratio of 110%-120% relative to the length in the width direction of the negative electrode slurry is placed on the upper part of the applied negative electrode slurry and the lower part of the negative electrode current collector, and a magnetic field is applied at a field strength of 4,700G for a time as shown in Table 1. The negative electrode slurry to which the magnetic field is applied is hot-air dried to form a negative electrode active layer, in which the carbon-based negative electrode active material has an orientation on the negative electrode current collector. The formed negative electrode active layer is subjected to X-ray diffraction (XRD) spectral analysis to measure the spectrum. The measurement conditions of X-ray diffraction are as follows:
[0229] -Target: Cu (Kα-ray) graphite monochromator
[0230] - Slits: Divergence slit = 1 degree, Receiving slit = 0.1 mm, Scattering slit = 1 degree
[0231] - Measurement area: [1,1,0] plane: 76.5°<2θ<78.5° / [0,0,4] plane: 53.5°<2θ<56.0°.
[0232] The formed negative electrode active layer was then rolled at a pressure of 100-150 MPa and a transmission rate of 3 m / s at 22±1° C. to prepare a negative electrode for a lithium secondary battery (average thickness of the negative electrode active layer before rolling: 87-88 μm / average thickness after rolling: 58-66 μm). The rolled negative electrode active layer was further subjected to X-ray diffraction (XRD) spectroscopy analysis to measure the spectrum.
[0233] Using the following Equation 3, the alignment value (OI) of the mixed graphite was calculated from the spectra measured before and after rolling, respectively, and the results are shown in Table 1 below.
[0234] [Equation 3]
[0235] OI=I 004 / I 110
[0236] In equation 3,
[0237] I 004 It represents the peak area representing the [0,0,4] crystal plane in the X-ray diffraction spectrum (XRD) measurement of the negative electrode active layer.
[0238] I 110It represents the peak area representing the [1,1,0] plane in the X-ray diffraction spectrum (XRD) measurement of the negative electrode active layer.
[0239] Table 1
[0240]
[0241] Preparation of positive electrode
[0242] The LiNi with a particle size of 5 μm 0.7 Co 0.1 Mn 0.1 Al 0.1 O2 was prepared as a positive electrode active material, which was mixed with a carbon-based conductive material and polyvinylidene fluoride as a binder in a weight ratio of 94:3:3 in N-methylpyrrolidone (NMP) to form a positive electrode slurry, and applied to an aluminum sheet. The positive electrode slurry was then dried in a vacuum oven at 120°C and rolled to prepare a positive electrode (average thickness of the positive electrode active layer: 100±10μm).
[0243] Preparation of lithium secondary batteries
[0244] Separators containing 18 μm polypropylene were placed between the positive electrodes obtained above and the negative electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 6, respectively, to manufacture electrode assemblies. The manufactured electrode assemblies were inserted into a case, and the nonaqueous electrolyte composition was injected into the case to assemble a lithium secondary battery.
[0245] The assembled lithium secondary battery was activated at 22±1° C. to prepare a lithium secondary battery. The activation was performed under constant current conditions, and the current density was shown in Table 2 below.
[0246] The negative electrode was disassembled from each activated lithium secondary battery to perform X-ray diffraction (XRD) spectrum analysis of the negative electrode active layer. The X-ray diffraction (XRD) conditions were the same as those previously performed. The arrangement value (OI) of the mixed graphite was calculated based on the measured X-ray diffraction spectrum. a ). In addition, the arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode was calculated. a ) and the arrangement value (OI) of the carbon-based negative electrode active material before activation r The results are shown in Table 2 below.
[0247] Table 2
[0248]
[0249] Experimental example
[0250] In order to confirm the performance of the negative electrode of the present invention, the lithium secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were evaluated for initial charge and discharge capacity and life characteristics.
[0251] Specifically, for each lithium secondary battery activated in Examples 1 to 3 and Comparative Examples 1 to 6, a charge and discharge cycle was performed. Charging was performed by charging to 5mV at a temperature of 25°C with a constant current (CC) of 1.0C and then charging at a constant voltage (CV) until the charging current was 0.005C (cut-off current). After charging, it was allowed to stand for 20 minutes and then discharged to 1.5V at a constant current (CC) of 1.0C at a temperature of 25°C. The capacity of each lithium secondary battery was measured during charging and discharging, and the measured charge and discharge capacity was determined as the initial charge and discharge capacity of each lithium secondary battery. The results are shown in Table 3 below.
[0252] For each lithium secondary battery for which the initial charge and discharge capacity was measured, 299 charge and discharge cycles were performed under the same conditions. At the end of the 299th charge and discharge, the charge and discharge capacity of each lithium secondary battery was measured. The measured charge and discharge capacity was determined as the 300th charge and discharge capacity of each lithium secondary battery, and the capacity retention rate was calculated based on the initial charge and discharge capacity. The results are shown in Table 3 below.
[0253] Table 3
[0254]
[0255] As shown in Table 3, it can be seen that the negative electrode of the present invention has excellent charge and discharge capacity and excellent life characteristics.
[0256] Specifically, in the configuration of the lithium secondary battery of the embodiment, (1) the arrangement value (OI a ) is controlled to be less than 3, (2) the ratio of the arrangement value of the carbon-based negative electrode active material before and after activation (OI a / OI r ) is controlled to be greater than 0.5 and less than 1. Therefore, the lithium secondary battery has a charge capacity greater than 461 mAh / g and a discharge capacity greater than 398 mAh / g during initial charge and discharge, respectively, and a capacity retention rate greater than 87% after 300 charge and discharge cycles.
[0257] On the other hand, the lithium secondary battery of the comparative example does not include all of the above configurations and therefore has a lower initial charge and discharge capacity than that of the example, or even if equivalent, is confirmed to have a significantly lower capacity retention rate after 300 charge and discharge cycles.
[0258] This shows that by including the carbon-based negative electrode active material and the silicon-based negative electrode active material together, the negative electrode of the embodiment has a high charge and discharge capacity and energy density. In addition, the negative electrode ensures the migration path of lithium ions in the negative electrode active layer during activation, which means that even if the secondary battery is charged and discharged for a long time, the shrinkage and expansion of the negative electrode active material caused by the insertion and extraction of lithium ions are suppressed, and the damage and / or loss of the arrangement value (OI) of the carbon-based negative electrode active material is minimized.
[0259] From these results, it can be seen that the negative electrode for lithium secondary batteries of the present invention has excellent charging characteristics and life characteristics during long-term charge and discharge.
[0260] Although the above content has been described with reference to the preferred exemplary embodiments of the present invention, those skilled in the art or those having ordinary knowledge in the art will appreciate that various modifications and changes may be made to the present invention without departing from the concept and technical scope of the present invention described in the following claims.
[0261] Therefore, the technical scope of the present invention is not limited to the contents described in the detailed description of the specification, but should be defined by the patent claims.
Claims
1. A negative electrode for a lithium secondary battery, comprising: Anode current collector; as well as a negative electrode active layer, which is disposed on at least one side of the negative electrode current collector and comprises a carbon-based negative electrode active material and a silicon-based negative electrode active material, The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1: [Equation 1] 0.5≤[OI a ] / [OI r ]<1.0 In equation 1, OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation, OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the (0,0,4) plane to the peak at 2θ=77.5±0.2° representing the (1,1,0) plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
2. The negative electrode for a lithium secondary battery according to claim 1, wherein the average particle size (Dc) of the carbon-based negative electrode active material is 5 μm to 50 μm, and the average particle size (Ds) of the silicon-based negative electrode active material is 0.5 μm to 10 μm, The average particle size ratio (Dc / Ds) of the carbon-based negative electrode active material to the silicon-based negative electrode active material is 1 to 10.
3. The negative electrode for a lithium secondary battery according to claim 1, wherein The silicon-based negative electrode active material may be contained in an amount of 1 wt % to 20 wt % based on the total weight of the negative electrode active material. 4 . The negative electrode for a lithium secondary battery as claimed in claim 1 , wherein the carbon-based negative electrode active material comprises one or more of natural graphite and artificial graphite.
5. The negative electrode for lithium secondary battery according to claim 1, wherein the silicon-based negative electrode active material comprises silicon (Si), silicon carbide (SiC) and silicon oxide SiO q One or more of, wherein 0.8≤q≤2.
5.
6. The negative electrode for lithium secondary battery according to claim 1, wherein the loading amount of the negative electrode active layer is 150 mg / 25 cm 2 Up to 300mg / 25cm 2 .
7. The negative electrode for a lithium secondary battery according to claim 1, wherein The average thickness of the negative electrode active layer is 10 μm to 100 μm.
8. A method for manufacturing a negative electrode for a lithium secondary battery, comprising: applying a negative electrode slurry containing a carbon-based negative electrode active material and a silicon-based negative electrode active material to at least one side of a negative electrode current collector, applying a magnetic field to the applied negative electrode slurry, and The negative electrode slurry to which the magnetic field is applied is dried and roll-pressed to form a negative electrode active layer. The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1: [Equation 1] 0.5≤[OI a ] / [OI r ]<1.0 In equation 1, OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation, OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and The arrangement value (OI) represents the ratio of the area integral value of the peak at 2θ=54.7±0.2° representing the (0,0,4) plane to the peak at 2θ=77.5±0.2° representing the (1,1,0) plane in the X-ray diffraction spectrum analysis of the negative electrode active layer. 9 . The method for manufacturing a negative electrode for a lithium secondary battery according to claim 8 , wherein the step of applying a magnetic field is performed at a magnetic field strength of 3000 G to 9000 G. 10 . The method for manufacturing a negative electrode for a lithium secondary battery according to claim 8 , wherein the step of applying a magnetic field is performed for 1 second to 30 seconds. 11 . The method for producing a negative electrode for a lithium secondary battery according to claim 8 , wherein the roll pressing is performed at a temperature of 20° C. to 35° C. and a pressure of 50 MPa to 200 MPa.
12. A lithium secondary battery provided with an electrode assembly, the electrode assembly comprising: positive electrode, The negative electrode according to claim 1, and A separator is disposed between the positive electrode and the negative electrode.
13. The lithium secondary battery of claim 12, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active layer, the positive electrode active layer being disposed on at least one side of the positive electrode current collector and comprising at least one positive electrode active material of lithium metal oxides represented by the following Chemical Formula 1 and Chemical Formula 2: [Chemical formula 1] Li x [Ni y Co z Mr w M 1 v ]O2 [Chemical formula 2] LiM 2 p Mn 1-p O4 In Chemical Formula 1 and Chemical Formula 2, M 1 is at least one element selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, x, y, z, w, and v are respectively 1.0 ≤ x ≤ 1.30, 0.5 ≤ y < 1, 0 < z ≤ 0.3, 0 < w ≤ 0.3, and 0 ≤ v ≤ 0.1, where y + z + w + v = 1, M 2 is Ni, Co or Fe, and p is 0.05 ≤ p ≤ 1.
0.
14. A method for manufacturing a lithium secondary battery, comprising: Activating a lithium secondary battery including an electrode assembly, the electrode assembly including a positive electrode, the negative electrode according to claim 1, and a separator disposed between the positive electrode and the negative electrode; The arrangement value (OI) of the activated carbon-based negative electrode active material of the negative electrode active layer a ) is less than 3, and satisfies the following equation 1: [Equation 1] 0.5≤[OI a ] / [OI r ]<1.0 In Equation 1, OI r represents the arrangement value (OI) of the carbon-based negative electrode active material measured before activation, OI a represents the arrangement value (OI) of the carbon-based negative electrode active material measured after activation, and wherein the arrangement value (O.I) represents the ratio of the area integral value of the peak at 2θ = 54.7 ± 0.2° representing the (0,0,4) plane to the peak at 2θ = 77.5 ± 0.2° representing the (1,1,0) plane in the X-ray diffraction spectrum analysis of the negative electrode active layer.
15. The method for manufacturing a lithium secondary battery according to claim 14, wherein the activation process is performed by charging and discharging at a rate of 0.01C to 0.9C at least twice.
Citation Information
Cited By
Negative electrode sheet and preparation method therefor, cylindrical battery, and electronic cigarette
WO2026148790A1