Preparation method of light, thin and environment-friendly running wind coat
By using specific specifications of nylon yarn and spandex yarn interwoven technology, the problem of running windbreakers being airtight, non-hygroscopic, and sticky to skin is solved, and the effect of lightness, breathability and windproof is achieved, and the fabric is dry and comfortable to wear is ensured. Experience.
Patent Information
- Application Number
- CN202410988143.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing running windbreaker has problems such as airtight, non-hygroscopic, sticky skin and stuffy, resulting in poor wearing experience.
The composite yarn of 20D/24F FD FDY, the second nylon yarn of 40D/34F SD DTY and the composite yarn of spandex yarn are coated with the first nylon yarn, and the composite structure is formed by interweaving, combined with oil removal treatment, Dyeing and ironing process to prepare a light and light environmentally friendly running windbreaker.
It achieves excellent soft feel of the fabric, low moisture rebate, good dry and wet balance effect, and prevents itchy sensation caused by excessive drying, providing a cool wearing experience, and at the same time has certain wind resistance and breathability.
Smart Images

Figure CN118902189A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of clothing, and in particular to a method for preparing a light and environmentally friendly running windbreaker. Background Art
[0002] Running is a simple, convenient sport with a low entry threshold, so more and more people are taking running as a daily exercise. In summer, people can go out for a run by wearing only a running T-shirt on their upper body. In spring and autumn, the weather turns cooler, the temperature difference between morning and evening is large, and the wind increases. People sweat all over after running. At this time, it is not suitable to blow the wind or expose the sweaty skin for too long. Therefore, it is very important to carry a running windbreaker when running in spring and autumn. In order to pursue the ultimate lightweight, the running windbreakers on the market currently use ultra-fine yarns and high-density weaving to make the whole windbreaker extremely light, but there are problems such as stuffiness, airtightness, non-hygroscopicity, stickiness to the skin, and poor wearing experience.
[0003] In terms of yarn, most running windbreakers on the market are woven with polyester and nylon yarns, with yarn fineness ranging from 7D to 50D. Polyester yarn has good moisture absorption and quick-drying properties, but because woven fabrics are thinner and have a higher weaving density than knitted fabrics, their moisture absorption capacity is limited and they feel rough. After the human body warms up and sweats, they will feel stuffy and sticky, and the wearing experience is poor. Nylon has improved feel and moisture absorption compared to polyester, but it has poor quick-drying properties, and also has the discomfort of sticking to the skin and stuffiness after sweating.
[0004] Chinese patent application No. 201720766788.6 discloses a breathable running suit, comprising: a top and a hat connected to the top of the top, characterized in that the top is made of a three-layer structure, and the top is composed of an inner compression garment, a middle breathable garment and an outer protective garment from the inner layer to the outer layer, the inner compression garment is woven from a composite fiber composed of high-elastic polyester and spandex, the middle breathable garment has a grid-like breathable fabric structure as a whole, the outer protective garment comprises a front garment, a back garment and sleeves, the connection between the front garment, the back garment and the sleeves is connected by knitting, the outer layer of the outer protective garment is coated with a glass fiber light-absorbing particle coating, the outer protective garment is made of a waterproof material as a whole, a butterfly-hole mesh is provided at the connection between the sleeves and the front garment or the back garment, and a butterfly-hole mesh is provided on the back garment. The running suit uses a composite fiber composed of high-elastic polyester and spandex to weave an inner compression garment. After the human body heats up and sweats, it will produce a stuffy and sticky feeling, and the wearing experience is poor.
[0005] In terms of fabrics, there are currently two types of woven fabrics for running windbreakers: one is single-layer woven plain or small square fabrics, and the other is film-type fabrics. Woven single-layer fabrics are often woven with ultra-fine yarns for extreme lightness, and the weight of the finished garment can be as low as 20g, but this type of windbreaker has problems such as not being windproof, not keeping warm, and sticking to the skin; film-type fabrics can greatly improve the windproof and waterproof properties of clothing, but have problems such as poor skin affinity, high weight, and stuffiness and airtightness.
[0006] Chinese patent application No. 202322043234.1 discloses a wear-resistant woven fabric, including a base layer, the base layer including weft yarns and skin-contacting warp yarns and wear-resistant warp yarns arranged alternately at intervals, the skin-contacting warp yarns and the wear-resistant warp yarns respectively forming a first satin system and a second satin system with the weft yarns, the skin-contacting warp yarns forming skin-contacting floating long lines on one side of the weft yarns, and the wear-resistant warp yarns forming wear-resistant floating long lines on the other side of the weft yarns. The utility model improves the skin-friendliness of the fabric on the side close to the skin and the wear resistance of the fabric on the side away from the skin by forming skin-contacting floating long lines with the skin-contacting warp yarns and wear-resistant floating long lines with the wear-resistant warp yarns. The single-layer setting of the fabric makes the fabric relatively light and thin, the softness and hygroscopicity of the fabric are improved by modal fibers, the ductility and elasticity of the fabric are improved by polyester fibers, and the wear resistance and strength of the fabric on the side away from the skin are improved by nylon fibers, that is, the service life of the fabric is improved. However, the windbreaker made of woven single-layer fabrics has problems such as not being windproof, not keeping warm, and sticking to the skin. Summary of the invention
[0007] Therefore, in view of the above problems, the present invention provides a method for preparing a lightweight and environmentally friendly running windbreaker to solve the problems that the existing windbreakers are not breathable, do not absorb moisture, stick to the skin, are easy to get stuffy when worn, and have a poor user experience.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] A method for preparing a lightweight and environmentally friendly running windbreaker comprises the following steps:
[0010] S1. Selection of raw materials: the raw materials include a first nylon yarn with a specification of 20D / 24F FD FDY, a second nylon yarn with a specification of 40D / 34F SDDTY, and a composite yarn of the first nylon yarn coated with spandex yarn, wherein the specification of the spandex yarn is 20-50D;
[0011] S2, the warp yarn is the first nylon yarn, the weft yarn is the second nylon yarn and the composite yarn of nylon yarn covered with spandex yarn, and the warp and weft yarns are interwoven to obtain a grey cloth;
[0012] S3, degreasing the grey cloth obtained in step S2, and then dyeing it;
[0013] S4, after post-processing and plate-making, the grey cloth is cut according to the pattern design, and then the light and environmentally friendly running windbreaker is obtained after sewing and ironing.
[0014] Furthermore, the minimum circulation unit of the grey fabric in the transverse direction includes six weaving rows, and the minimum circulation unit of the grey fabric in the longitudinal direction includes eight weaving rows, wherein rows 1-6 are all weaved with composite yarns, and rows 7-8 are all weaved with second nylon yarns.
[0015] Further, the grey cloth is formed by a composite structure, the warp structure points of the composite structure are floating, the weft structure points are sinking, and the structure cycle from left to right and from bottom to top is:
[0016] Ups and downs;
[0017] Ups and downs;
[0018] Ups and downs;
[0019] Ups and downs;
[0020] Ups and downs;
[0021] Ups and downs;
[0022] Floating and floating;
[0023] Ups and downs.
[0024] Furthermore, the density of the grey cloth is 274T*203T, and the weight is 64g / m 2 .
[0025] Furthermore, the coating process of the composite yarn is as follows: using the spandex yarn as the core yarn and the first nylon yarn as the coating yarn, the core yarn and the coating yarn are respectively wound onto a double-sided bobbin dedicated to the coating machine, the yarn is passed from bottom to top through the tension clamp and the yarn guide hook and fixed on the double-sided bobbin for coating on the machine, and the coating direction of the coating yarn is Z twist.
[0026] Furthermore, the degreasing process is as follows:
[0027] c. First, loosen and inspect the grey cloth, soak it at 40-50℃, and then oscillate and scour it in a scouring tank at 90-95℃;
[0028] d. The grey cloth treated in step a is sequentially subjected to hot water washing, acid neutralization treatment, and cold water washing treatment.
[0029] Furthermore, the dyeing process is as follows: dyeing is carried out using a one-bath dyeing method with a bath ratio of 1:200-220, cationic dyes and auxiliaries are added at room temperature, the temperature is raised to 85°C, the holding time is 10 minutes, the degreased grey cloth is dyed, the holding time is 40 minutes, the temperature is increased stepwise, the temperature is increased to 100°C at a rate of 1°C / min, the holding time is 30 minutes, and then the temperature is decreased to about 50°C at a rate of 1°C / min, and then cold washed and dried.
[0030] Furthermore, the impregnation is carried out in an impregnation tank for 15-30 minutes, and the impregnation solution comprises: 2 g / L of degreasing agent, 1 g / L of soda ash, and 1 g / L of chelating agent; the oscillation refining is carried out in a refining tank with an oscillation frequency of 30-40 Hz and a time of 15-30 minutes, and the refining solution comprises: 6 g / L of degreasing agent, 4 g / L of soda ash, and 1 g / L of chelating agent.
[0031] Furthermore, the temperature of the hot water washing treatment is 75-85°C, the temperature of the acid neutralization treatment is 50-60°C, and the temperature of the cold water washing treatment is 30-40°C.
[0032] Furthermore, the auxiliary agent includes: 1g / L high temperature leveling agent, 1g / L buffer acid NX-306, 0.5g / L chelating dispersant and 2g / L sodium sulfate; before dyeing, the pH value of the auxiliary solution is adjusted to 4.5-5 using acetic acid; the drying is carried out in an oven at a temperature of 90-100°C for 30-60min.
[0033] By adopting the above technical solution, the beneficial effects of the present invention are:
[0034] 1. The present invention uses nylon 56 nylon yarn as raw material. Nylon 56 is different from traditional petroleum-based nylon 6 yarn. It is obtained by fermenting and extracting lysine from plant crops, synthesizing pentamethylenediamine, and polymerizing pentamethylenediamine with dibasic acid to obtain nylon 56 masterbatch, and then through the spinning process, nylon 56 yarns of different specifications are obtained. Compared with traditional nylon 6 yarn, the production process of nylon 56 is carried out at room temperature and pressure, and the energy consumption is lower than that of hexamethylenediamine and caprolactam produced by chemical methods, realizing "three lows" production, low water consumption, low energy consumption, and low carbon emissions; and compared with traditional nylon 6, nylon The nylon 56 molecule has more unsaturated hydrogen bonds, which makes the fabric woven from it have an excellent soft and smooth feel, and the moisture regain is about 5.5-6%, providing a more balanced dry-wet balance effect. The moisture regain is lower than cotton fiber (about 8.5%) and cellulose fiber (about 13%), which can ensure that the fabric always remains dry and avoids the situation of only absorbing moisture without dissipating moisture. At the same time, the moisture regain is much higher than polyester fiber (0.7-0.9%), which reduces the itching and static electricity caused by excessive drying. Nylon 56 has a higher thermal conductivity, rapid heat conduction, and a contact coolness coefficient higher than the national standard. At the same time, the "active" structure of the nylon 56 molecular chain enables it to absorb moisture faster and conduct heat to the outside of the fabric, so that it can maintain a cool body feeling even after long-term wear.
[0035] 2. The materials of common running windbreakers on the market are mostly woven plain or small square structures in pursuit of lightness. The overall structure is relatively flat, and the warp density and weft density are relatively dense, which makes this type of windbreaker very easy to get hot and sticky when worn for running. To address this problem, the present invention uses a relatively thick second nylon yarn (specification is 40D / 34F SD DTY) to form a weft floating line structure on the back of the fabric. After the composite yarn (specification is 20D / 24F FD FDY nylon coated with 20D spandex) forms a 6-row plain weave, the second nylon yarn forms a weft floating line spanning 5 vertical columns; and because the weft yarn is relatively thick and is DTY yarn, regular raised horizontal stripes are formed on the back of the fabric, and the front of the fabric is mainly 20D / 24F FD FDY nylon yarn is relatively smooth and delicate, with a striped appearance. The raised horizontal stripes can transfer sweat to the surface of the garment using the wicking structure the moment the sweat touches the garment, keeping the inside dry. On the other hand, the raised horizontal stripes form a microclimate with the skin, ensuring air circulation and preventing the skin from sticking.
[0036] 3. Material density is 274T*203T, weight is 64g / m 2 It has certain windproof properties while also being breathable and lightweight, which can reduce the burden during exercise. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1is a front view of a running windbreaker according to an embodiment of the present invention;
[0038] Figure 2 is a schematic diagram of the back side of a running windbreaker according to an embodiment of the present invention;
[0039] Figure 3 Schematic diagram of the structure of the composite structure of the grey cloth in the embodiment of the present invention;
[0040] Figure 4 is a front view of the actual fabric of the running windbreaker in an embodiment of the present invention;
[0041] Figure 5 It is a back view of the actual fabric of the running windbreaker in the embodiment of the present invention. DETAILED DESCRIPTION
[0042] Example 1
[0043] refer to Figures 1 to 5 A method for preparing a lightweight and environmentally friendly running windbreaker comprises the following steps:
[0044] (1) Selection of raw materials
[0045] The raw materials include a first nylon yarn of 20D / 24F FD FDY, a second nylon yarn of 40D / 34F SD DTY, and a composite yarn of the first nylon yarn covered with spandex yarn;
[0046] The coating process of the composite yarn is as follows: the spandex yarn is used as the core yarn and the first nylon yarn is used as the coating yarn, the core yarn and the coating yarn are respectively wound onto a double-sided bobbin dedicated to the coating machine, the yarn is passed from bottom to top through a tension clamp and a yarn guide hook and fixed on the double-sided bobbin for coating on the machine, and the coating direction of the coating yarn is Z twist;
[0047] (2) Woven fabric
[0048] The warp yarn is the first nylon yarn, the weft yarn is the second nylon yarn and the composite yarn of nylon coated with spandex, the specification of the spandex yarn is 20D, the warp and weft yarns are interwoven to form a grey cloth, the density of the grey cloth is 274T*203T, and the gram weight is 64g / m 2 The minimum horizontal cycle unit of the grey fabric includes six rows of weaving, and the minimum longitudinal cycle unit of the grey fabric includes eight rows of weaving, wherein the 1-6 rows are all weaved with composite yarns, and the 7-8 rows are all weaved with second nylon yarns. The grey fabric is formed by a composite tissue, and the warp tissue points of the composite tissue are floating and the weft tissue points are sinking. The warp tissue point a is represented by ■, and the weft tissue point b is represented by □. The tissue cycle of the composite tissue from left to right and from bottom to top is:
[0049] Ups and downs;
[0050] Ups and downs;
[0051] Ups and downs;
[0052] Ups and downs;
[0053] Ups and downs;
[0054] Ups and downs;
[0055] Floating and floating;
[0056] Ups and downs;
[0057] (3) Degreasing treatment
[0058] (3-1) First, the grey cloth is loosened and preliminarily inspected, and then immersed in an immersion solution at 40° C., the immersion is carried out in an immersion tank for 15 minutes, and the immersion solution comprises: 2 g / L of degreasing agent, 1 g / L of soda ash, and 1 g / L of chelating agent, and then oscillated and refined in a refining solution at 90° C., the oscillation refining is carried out in a refining tank with an oscillation frequency of 30 Hz for 15 minutes, and the refining solution comprises: 6 g / L of degreasing agent, 4 g / L of soda ash, and 1 g / L of chelating agent;
[0059] (3-2) subjecting the grey cloth treated in step (3-1) to hot water washing, acid neutralization and cold water washing in sequence, wherein the hot water washing temperature is 75° C., the acid neutralization temperature is 50° C. and the cold water washing temperature is 30° C.;
[0060] (4) Dyeing treatment
[0061] The dyeing is performed by a one-bath dyeing method with a bath ratio of 1:200, and cationic dyes and auxiliaries are added at room temperature, wherein the auxiliaries include: 1 g / L high-temperature leveling agent, 1 g / L buffer acid NX-306, 0.5 g / L chelating dispersant and 2 g / L sodium sulfate. Before dyeing, the pH value of the auxiliary solution is adjusted to 4.5-5 using acetic acid, the temperature is increased to 85°C, the holding time is 10 minutes, the degreased grey cloth is dyed, the holding time is 40 minutes, the temperature is increased stepwise, the temperature is increased to 100°C at a speed of 1°C / min, the holding time is 30 minutes, and then the temperature is decreased to about 50°C at a speed of 1°C / min, and then the cold water washing is performed at 30°C and then the drying is performed in an oven at a temperature of 90°C for 60 minutes;
[0062] (5) After post-processing and plate making, the grey cloth is cut according to the plate design, and then sewn and ironed to obtain the light and environmentally friendly running windbreaker.
[0063] Example 2
[0064] A method for preparing a lightweight and environmentally friendly running windbreaker comprises the following steps:
[0065] (1) Selection of raw materials
[0066] The raw materials include a first nylon yarn of 20D / 24F FD FDY, a second nylon yarn of 40D / 34F SD DTY, and a composite yarn of the first nylon yarn covered with spandex yarn;
[0067] The coating process of the composite yarn is as follows: the spandex yarn is used as the core yarn and the first nylon yarn is used as the coating yarn, the core yarn and the coating yarn are respectively wound onto a double-sided bobbin dedicated to the coating machine, the yarn is passed from bottom to top through a tension clamp and a yarn guide hook and fixed on the double-sided bobbin for coating on the machine, and the coating direction of the coating yarn is Z twist;
[0068] (2) Woven fabric
[0069] The warp yarn is the first nylon yarn, the weft yarn is the second nylon yarn and the composite yarn of nylon coated with spandex, the specification of the spandex yarn is 30D, the warp and weft yarns are interwoven to form a grey cloth, the density of the grey cloth is 274T*203T, and the gram weight is 64g / m 2 The minimum horizontal circulation unit of the grey fabric includes six rows of weaving, and the minimum vertical circulation unit of the grey fabric includes eight rows of weaving, wherein the 1st to 6th rows are all weaved with composite yarns, and the 7th to 8th rows are all weaved with second nylon yarns. The grey fabric is formed by a composite structure, and the warp structure point of the composite structure is floating, and the weft structure point is sinking. The structure cycle from left to right and from bottom to top is:
[0070] Ups and downs;
[0071] Ups and downs;
[0072] Ups and downs;
[0073] Ups and downs;
[0074] Ups and downs;
[0075] Ups and downs;
[0076] Floating and floating;
[0077] Ups and downs;
[0078] (3) Degreasing
[0079] (3-1) First, the grey cloth is loosened and preliminarily inspected, and then immersed in an immersion solution at 45° C., the immersion is carried out in an immersion tank for 20 minutes, and the immersion solution includes: 2 g / L of degreasing agent, 1 g / L of soda ash, and 1 g / L of chelating agent, and then oscillated and refined in a refining solution at 90° C., the oscillation refining is carried out in a refining tank with an oscillation frequency of 35 Hz for 20 minutes, and the refining solution includes: 6 g / L of degreasing agent, 4 g / L of soda ash, and 1 g / L of chelating agent;
[0080] (3-2) subjecting the grey cloth treated in step (3-1) to hot water washing, acid neutralization and cold water washing in sequence, wherein the hot water washing temperature is 80° C., the acid neutralization temperature is 55° C., and the cold water washing temperature is 35° C.;
[0081] (4) Dyeing treatment
[0082] The dyeing is performed by a one-bath dyeing method, the bath ratio is 1:210, and cationic dyes and auxiliaries are added at room temperature, wherein the auxiliaries include: 1 g / L high-temperature leveling agent, 1 g / L buffer acid NX-306, 0.5 g / L chelating dispersant and 2 g / L sodium sulfate. Before dyeing, the pH value of the auxiliary solution is adjusted to 5 using acetic acid, the temperature is increased to 85°C, the holding time is 10 minutes, the degreased grey cloth is dyed, the holding time is 40 minutes, the temperature is increased stepwise, the temperature is increased to 100°C at a speed of 1°C / min, the holding time is 30 minutes, and then the temperature is decreased to about 50°C at a speed of 1°C / min, and then the cold water washing is performed at 35°C and then the drying is performed in an oven at a temperature of 95°C for 45 minutes;
[0083] (5) After post-processing and plate making, the grey cloth is cut according to the plate design, and then sewn and ironed to obtain the light and environmentally friendly running windbreaker.
[0084] Example 3
[0085] A method for preparing a lightweight and environmentally friendly running windbreaker comprises the following steps:
[0086] (1) Selection of raw materials
[0087] The raw materials include a first nylon yarn of 20D / 24F FD FDY, a second nylon yarn of 40D / 34F SD DTY, and a composite yarn of the first nylon yarn covered with spandex yarn;
[0088] The coating process of the composite yarn is as follows: the spandex yarn is used as the core yarn and the first nylon yarn is used as the coating yarn, the core yarn and the coating yarn are respectively wound onto a double-sided bobbin dedicated to the coating machine, the yarn is passed from bottom to top through a tension clamp and a yarn guide hook and fixed on the double-sided bobbin for coating on the machine, and the coating direction of the coating yarn is Z twist;
[0089] (2) Woven fabric
[0090] The warp yarn is the first nylon yarn, the weft yarn is the second nylon yarn and the composite yarn of nylon coated with spandex, the specification of the spandex yarn is 40D, the warp and weft yarns are interwoven to form a grey cloth, the density of the grey cloth is 274T*203T, and the gram weight is 64g / m 2 The minimum horizontal circulation unit of the grey fabric includes six rows of weaving, and the minimum vertical circulation unit of the grey fabric includes eight rows of weaving, wherein the 1st to 6th rows are all weaved with composite yarns, and the 7th to 8th rows are all weaved with second nylon yarns. The grey fabric is formed by a composite structure, and the warp structure point of the composite structure is floating, and the weft structure point is sinking. The structure cycle from left to right and from bottom to top is:
[0091] Ups and downs;
[0092] Ups and downs;
[0093] Ups and downs;
[0094] Ups and downs;
[0095] Ups and downs;
[0096] Ups and downs;
[0097] Floating and floating;
[0098] Ups and downs;
[0099] (4) Degreasing treatment
[0100] (3-1) First, the grey cloth is loosened and preliminarily inspected, and then immersed in an immersion solution at 50° C., the immersion is carried out in an immersion tank for 30 minutes, and the immersion solution includes: 2 g / L of degreasing agent, 1 g / L of soda ash, and 1 g / L of chelating agent, and then oscillated and refined in a refining solution at 95° C., the oscillation refining is carried out in a refining tank with an oscillation frequency of 40 Hz for 20 minutes, and the refining solution includes: 6 g / L of degreasing agent, 4 g / L of soda ash, and 1 g / L of chelating agent;
[0101] (3-2) subjecting the grey cloth treated in step (3-1) to hot water washing, acid neutralization and cold water washing in sequence, wherein the hot water washing temperature is 85° C., the acid neutralization temperature is 60° C. and the cold water washing temperature is 40° C.;
[0102] (4) Dyeing treatment
[0103] The dyeing is performed by a one-bath dyeing method, the bath ratio is 1:220, and cationic dyes and auxiliaries are added at room temperature, wherein the auxiliaries include: 1 g / L high-temperature leveling agent, 1 g / L buffer acid NX-306, 0.5 g / L chelating dispersant and 2 g / L sodium sulfate. Before dyeing, the pH value of the auxiliary solution is adjusted to 5 using acetic acid, the temperature is increased to 85°C, the holding time is 10 minutes, the degreased grey cloth is dyed, the holding time is 40 minutes, the temperature is increased stepwise, the temperature is increased to 100°C at a speed of 1°C / min, the holding time is 30 minutes, and then the temperature is decreased to about 50°C at a speed of 1°C / min, and after cold water washing at 40°C, the cloth is dried in an oven at a temperature of 100°C for 30 minutes;
[0104] (5) After post-processing and plate making, the grey cloth is cut according to the plate design, and then sewn and ironed to obtain the light and environmentally friendly running windbreaker.
[0105] Comparative Example 1
[0106] The difference from Example 1 is that: the raw materials do not use the first nylon yarn of 20D / 24F FD FDY, the second nylon yarn of 40D / 34F SD DTY, and the composite yarn of the first nylon yarn covered with spandex yarn, wherein the spandex yarn is 20D, and the nylon yarn of the commercially available nylon 6 material is used; the weaving structure does not use the method of forming the weft floating line structure on the reverse side of the fabric of the present invention, but uses a woven plain weave. Other technical solutions are the same as those of Example 1.
[0107] The test results of the products of Example 1, Example 2, Example 3 and Comparative Example 1 are shown in Table 1.
[0108] Table 1
[0109] Test items Example 1 Example 2 Example 3 Comparative Example 1 Air permeability (mm / s) 190 183 196 168 Water absorption (%) 227 216 224 176 Moisture regain (%) 5.82 5.63 5.71 7.30
[0110] With reference to GB / T 5453-1997 “Determination of Air Permeability of Textile Fabrics”, the air permeability of the products of Example 1, Example 2, Example 3 and the product of Comparative Example 1 was measured.
[0111] With reference to GB / T 21655.1-2023 “Evaluation of the quick-drying property of textiles Part 1: Single combination test method”, the hygroscopic properties of the products of Example 1, Example 2, Example 3 and the product of Comparative Example 1 were measured.
[0112] Referring to GB / T 9994-2018 "Official Moisture Regains of Textile Materials", the moisture regains of the products of Example 1, Example 2, Example 3 and the product of Comparative Example 1 were measured.
[0113] It can be seen from the test results in Table 1 that the moisture absorption and air permeability of the products of Example 1, Example 2 and Example 3 are better than those of Comparative Example 1, and the moisture regain is lower than that of Comparative Example 1, indicating that the products of the present invention can not only ensure that the fabric remains dry at all times, but also avoid the situation of only absorbing moisture but not discharging moisture.
[0114] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A method for preparing a lightweight and environmentally friendly running windbreaker, characterized in that: The following steps are involved: S1. Selection of raw materials: the raw materials include a first nylon yarn with a specification of 20D / 24F FD FDY, a second nylon yarn with a specification of 40D / 34F SD DTY, and a composite yarn of the first nylon yarn coated with spandex yarn, wherein the specification of the spandex yarn is 20-50D; S2, the warp yarn is the first nylon yarn, the weft yarn is the second nylon yarn and the composite yarn of nylon yarn covered with spandex yarn, and the warp and weft yarns are interwoven to obtain a grey cloth; S3, degreasing the grey cloth obtained in step S2, and then dyeing it; S4, after post-processing and plate-making, the grey cloth is cut according to the pattern design, and then the light and environmentally friendly running windbreaker is obtained after sewing and ironing.
2. The method for preparing a lightweight and environmentally friendly running windbreaker according to claim 1, characterized in that: The minimum circulation unit of the grey fabric in the transverse direction includes six rows of weaving, and the minimum circulation unit of the grey fabric in the longitudinal direction includes eight rows of weaving, wherein rows 1 to 6 are all weaved with composite yarns, and rows 7 to 8 are all weaved with second nylon yarns.
3. The method for preparing a light and environmentally friendly running windbreaker according to claim 1, characterized in that: The grey cloth is formed by a composite structure, the warp structure points of the composite structure are floating, the weft structure points are sinking, and the structure cycle from left to right and from bottom to top is: Ups and downs; Ups and downs; Ups and downs; Ups and downs; Ups and downs; Ups and downs; Floating and floating; Ups and downs.
4. The method for preparing a light and environmentally friendly running windbreaker according to claim 1, characterized in that: The density of the grey cloth is 274T*203T, and the weight is 64g / m 2 .
5. The method for preparing a light and environmentally friendly running windbreaker according to claim 1, characterized in that: The coating process of the composite yarn is as follows: using the spandex yarn as the core yarn and the first nylon yarn as the coating yarn, the core yarn and the coating yarn are respectively wound onto a double-sided bobbin dedicated to the coating machine, the yarn is passed from bottom to top through a tension clamp and a yarn guide hook and fixed on the double-sided bobbin for coating on the machine, and the coating direction of the coating yarn is Z twist.
6. The method for preparing a light and environmentally friendly running windbreaker according to claim 1, characterized in that: The degreasing process is as follows: a. First, loosen and inspect the grey cloth, immerse it in the impregnation liquid at 40-50℃, and then oscillate and scour it in the refining liquid at 90-95℃; b. The grey cloth treated in step a is sequentially subjected to hot water washing, acid neutralization treatment, and cold water washing treatment.
7. The method for preparing a light and environmentally friendly running windbreaker according to claim 1, characterized in that: The dyeing process is as follows: dyeing is performed using a one-bath dyeing method with a bath ratio of 1:200-220, cationic dyes and auxiliaries are added at room temperature, the temperature is raised to 85°C, the holding time is 10 minutes, the degreased grey cloth is dyed, the holding time is 40 minutes, the temperature is increased stepwise, the temperature is increased to 100°C at a speed of 1°C / min, the holding time is 30 minutes, and then the temperature is decreased to about 50°C at a speed of 1°C / min, cold water washing is performed, and then drying is performed.
8. The method for preparing a light and environmentally friendly running windbreaker according to claim 6, characterized in that: The impregnation is carried out in an impregnation tank for 15-30 minutes, and the impregnation liquid comprises: 2g / L of degreasing agent, 1g / L of soda ash, and 1g / L of chelating agent; the oscillation refining is carried out in a refining tank with an oscillation frequency of 30-40Hz for 15-30 minutes, and the refining liquid comprises: 6g / L of degreasing agent, 4g / L of soda ash, and 1g / L of chelating agent.
9. A method for preparing a light and environmentally friendly running windbreaker according to any one of claims 6-7, characterized in that: The temperature of the hot water washing treatment is 75-85°C, the temperature of the acid neutralization treatment is 50-60°C, and the temperature of the cold water washing treatment is 30-40°C.
10. The method for preparing a light and environmentally friendly running windbreaker according to claim 7, characterized in that: The auxiliary agent comprises: 1g / L high temperature leveling agent, 1g / L buffer acid NX-306, 0.5g / L chelating dispersant and 2g / L sodium sulfate; before dyeing, the pH value of the auxiliary agent solution is adjusted to 4.5-5 using acetic acid; the drying is carried out in an oven at a temperature of 90-100°C for 30-60 minutes.