Nitrogen oxide and sulfur dioxide solid absorbent and preparation method thereof

By modifying the desulfurization wastewater and gypsum of thermal power plants, the preparation of nitrogen oxides and sulfur dioxide solid absorbers is solved, and the problem of low removal efficiency of nitrogen oxides and sulfur dioxide in the prior art is achieved, and high-efficiency removal of low concentrations of nitrogen oxides and sulfur dioxide is achieved. Reduced emission concentration and operating costs.

CN118904026APending Publication Date: 2024-11-08CHINA HUADIAN ENG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085318.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art removes nitrogen oxides and sulfur dioxide in thermal power plants in low efficiency, and there are problems such as large equipment investment, high operating costs, large resource consumption and secondary pollution. Especially under low concentration emission standards, SCR and wet desulfurization Process costs increase.

Method used

By modifying the desulfurization wastewater and gypsum of thermal power plants, a nitrogen oxide and sulfur dioxide solid absorber is prepared, including desulfurization wastewater, calcium hypochlorite, nano-alumina, silicate cement and desulfurization gypsum, and is treated with flocculant The mixture is prepared by using the disc granulation mechanism to form a suspension of nano-alumina coated calcium hypochlorite, and a solid absorbent is obtained by drying.

Benefits of technology

Highly efficient removal of low concentrations of nitrogen oxides and sulfur dioxide is achieved, with removal rates reaching 94% and 92.3%, reducing the emission concentration of NOX and SO2, reducing cumulative damage to the environment, and reducing operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904026A_ABST
    Figure CN118904026A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of treatment of gas containing NOX and SO2, in particular to a nitrogen oxide and sulfur dioxide solid absorbent and a preparation method thereof, and the nitrogen oxide and sulfur dioxide solid absorbent is prepared from the following raw materials in parts by weight: 80-120 parts of desulfurization wastewater, 8-12 parts of calcium hypochlorite, 50-72 parts of nano aluminum oxide, 10-12 parts of Portland cement and 25-45 parts of desulfurization gypsum. Researches show that the prepared solid absorbent has an excellent removal effect on low-concentration nitrogen oxides and sulfur dioxide, the nitrogen oxide removal rate of the solid absorbent can reach 94%, the absorption rate of the solid absorbent can reach 0.8 g / (100g. S), the sulfur dioxide removal rate of the solid absorbent can reach 92.3%, the absorption rate of the solid absorbent can reach 0.72 g / (100g. S), and the solid absorbent can be recycled. The catalyst can be used as an auxiliary means of SCR and wet desulphurization to carry out advanced treatment on low-concentration NOX and SO2 of a thermal power plant, so that the emission concentration of NOX and SO2 is further reduced, and accumulative damage to the environment caused by long-term continuous emission of low-concentration nitrogen oxide and sulfur dioxide is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a NO X The technical field of gas treatment, in particular, relates to a solid absorbent for nitrogen oxides and sulfur dioxide and a preparation method thereof. Background Art

[0002] Sulfur dioxide (SO2) and nitrogen oxides (NO X ) are the gaseous pollutants with the largest content and widest impact among the current atmospheric pollutants. They mainly come from the combustion process of industrial fuel coal. In large-scale production enterprises such as thermal power plants, metal smelters, furnaces, etc., a large amount of waste gas (commonly known as flue gas) containing sulfide and nitrogen oxides is generated. Sulfur dioxide and nitrogen oxides form sulfuric acid mist, chemical smog and acid rain, which will bring serious harm to the ecological environment and human production and life.

[0003] For the removal of nitrogen oxides, the selective catalytic reduction denitrification technology (Selective Catalytic Reduction, SCR) and the selective non-catalytic reduction denitrification technology (Selective Non-Catalytic Reduction, SNCR) are generally used. The former has the advantages of high denitrification efficiency and low secondary pollution, but it has problems such as large equipment investment, high operating costs and high technical difficulty, especially when installing a waste heat boiler system, it is easy to cause waste heat waste. The latter does not use a catalyst and has low equipment operating costs, but it has problems such as low denitrification efficiency and large NH3 usage. It is difficult to ensure the reaction temperature and residence time, and it is easy to cause secondary pollution due to NH3 escape.

[0004] For the removal of sulfur dioxide, wet desulfurization, dry desulfurization and ammonia desulfurization are generally used. Among them, coal chemical plants and coal-fired power plants generally use limestone-gypsum method for flue gas desulfurization. This method has the characteristics of high desulfurization efficiency, reliable operation and high absorbent utilization rate, but the process has a large demand for limestone, and there are problems such as large resource consumption, large water consumption and secondary pollution of wastewater. Dry desulfurization mainly includes furnace calcium injection method, which has low investment, small land occupation, no sewage and waste acid discharge, and small equipment corrosion, but the problem of this method is low desulfurization efficiency, slow desulfurization reaction rate, and long-term use requires the renewal of dust removal system. Ammonia desulfurization is mainly a flue gas purification technology that uses ammonia water as an absorbent to remove pollutants such as SO2 in flue gas. It has the advantages of high absorption efficiency and fast reaction rate. However, since the price of ammonia is much higher than that of absorbents such as limestone, high operating cost is the biggest factor hindering the widespread application of ammonia desulfurization process.

[0005] At the same time, NO X Ultra-low emission standards have been controlled at 30mg / m 3 Some local domestic standards are even controlled at 25mg / m3 The ultra-low emission standard of SO2 has been controlled at 35mg / m 3 Within, common SCR denitrification can reduce NO X Emissions are controlled at 50mg / m 3 Even 30 mg / m 3 Flue gas wet desulfurization can control SO2 emissions to 20-30mg / m 3 However, as emission standards become more stringent, the cost of SCR denitrification process and wet desulfurization will also increase by multiples.

[0006] Therefore, among the many emission reduction technologies, solid absorbents have gradually become a research hotspot in the field of nitrogen oxide and sulfur dioxide control in thermal power plants due to their advantages such as high efficiency, stability and easy recovery.

[0007] The present invention proposes a novel solid absorbent for nitrogen oxides and sulfur dioxide by modifying the desulfurization wastewater and desulfurization gypsum in thermal power plants, which can be used as an auxiliary means for SCR and wet desulfurization to treat low-concentration NO in thermal power plants. X and SO2 for deep treatment to further reduce NO X and SO2 emission concentration. Summary of the invention

[0008] The object of the present invention is to provide a nitrogen oxide and sulfur dioxide solid absorbent and a preparation method thereof. The nitrogen oxide and sulfur dioxide solid absorbent prepared by the present invention has an excellent removal effect on low-concentration nitrogen oxides and sulfur dioxide.

[0009] In a first aspect, the present invention provides a solid absorbent for nitrogen oxides and sulfur dioxide, comprising the following raw materials in parts by weight:

[0010] 80-120 parts of desulfurization wastewater, 8-12 parts of calcium hypochlorite, 50-72 parts of nano-alumina, 10-12 parts of silicate cement and 5-45 parts of desulfurization gypsum.

[0011] As a preferred embodiment of the present technical solution, 0.004-0.008 parts of flocculant is also included; the flocculant includes any one of ferric chloride, aluminum sulfate, polyaluminum chloride, polyacrylamide, polyacrylic acid, starch, lignin and chitosan, and is preferably polyacrylamide.

[0012] The present invention uses a flocculant to flocculate desulfurized wastewater, so as to effectively form a large-volume, high-density, fast-sedimenting flocculent body through a polymerization reaction from suspended matter (such as granular colloid) in the desulfurized wastewater, thereby significantly reducing the content of suspended matter in the wastewater; secondly, the flocculant can also effectively remove harmful substances such as sulfate and sulfite, COD and fluoride in the desulfurized wastewater; furthermore, the desulfurized wastewater often has a high chroma, and the flocculation treatment of the flocculant can significantly reduce the chroma of the wastewater and improve the appearance of the water quality. In addition, since the amount of the flocculant used in the present invention is relatively small, the use of the flocculant will not affect the oxidizability of calcium hypochlorite at all.

[0013] As a preferred embodiment of the present technical solution, the nano-alumina is preferably γ-Al2O3, and its particle size is 10-20nm. Compared with nano-alumina of other crystal forms, γ-Al2O3 has a larger specific surface area and higher activity.

[0014] As a preferred embodiment of the present technical solution, the desulfurized gypsum of the present invention can directly use the desulfurized gypsum powder produced by coal-fired power plants, the particle size of which is preferably 30-60 μm, and the moisture content is preferably 10%-15%.

[0015] In a second aspect, the present invention also provides a method for preparing the above-mentioned solid absorbent, comprising the following steps:

[0016] S1. flocculating the desulfurization wastewater using a flocculant, mixing the supernatant with calcium hypochlorite, stirring and dissolving, and obtaining a mixed solution;

[0017] S2, adding nano-alumina to the mixed solution, stirring evenly, to obtain a suspension of nano-alumina-coated calcium hypochlorite;

[0018] S3, adding silicate cement and desulfurized gypsum to the suspension of nano-alumina-coated calcium hypochlorite in sequence, stirring evenly to obtain a viscous liquid mixture;

[0019] S4. Press the viscous liquid mixture into a honeycomb shape and then dry it to obtain a solid absorbent.

[0020] In the preparation method of the present invention, first, a certain amount of flocculant is added to the desulfurization wastewater, and after stirring and standing, the supernatant is taken for standby use to reduce the content of suspended matter in the wastewater and the chromaticity of the wastewater and improve the appearance of water quality; then, calcium hypochlorite is added to the supernatant of the desulfurization wastewater. Since the desulfurization wastewater itself is weakly acidic and contains relatively rich chloride ions, under acidic conditions, the chloride ions can greatly improve the oxidizability of calcium hypochlorite to oxidize nitrogen oxides and sulfur dioxide into nitrates and sulfates. On this basis, nano-alumina is added to the mixed solution of the desulfurization wastewater supernatant and calcium hypochlorite, and a suspension of calcium hypochlorite coated with nano-alumina is prepared by stirring or the like. At this time, the oxide film in the porous structure of nano-alumina can not only provide a physical barrier for calcium hypochlorite, reducing the chance of direct contact between calcium hypochlorite and air, but also the chemical stability of nano-alumina itself helps to maintain the stability of the entire mixed system, preventing calcium hypochlorite from failing due to reaction with other chemical substances. Moreover, the porous structure and wear resistance of nano-alumina will also produce synergistic effects with other components, further enhancing the protective effect of calcium hypochlorite, so that calcium hypochlorite can continuously exert a high oxidizability. In order to further improve the stability of the solid absorbent and prevent the solid absorbent from having problems such as ash falling and dust scattering during use, the present invention further adds silicate cement and desulfurized gypsum to the suspension of calcium hypochlorite coated with nano-alumina in sequence, and promotes the hydration reaction of silicate cement by utilizing the alkaline substances such as calcium carbonate or calcium hydroxide remaining in the desulfurized gypsum, thereby enhancing the strength and viscosity of the entire system. Finally, the prepared viscous liquid mixture is pressed and dried to obtain a solid absorbent having an excellent removal effect on low-concentration nitrogen oxides and sulfur dioxide.

[0021] As a preferred embodiment of the present technical solution, in step S1, during the flocculation treatment, a flocculant is added to the desulfurization wastewater and stirred for 1-10 minutes, and then allowed to settle for 1-2 hours.

[0022] As a preferred embodiment of the present technical solution, in step S2, the mixed solution and nano-alumina are placed in a disc granulator for stirring and dispersion to obtain a suspension of nano-alumina-coated calcium hypochlorite;

[0023] Wherein, the rotation speed of the disc granulator is 15-30rpm, and the processing time is 60-120min.

[0024] The present invention adopts the method of a disc granulator to prepare a suspension of calcium hypochlorite coated with nano-alumina. Since the disc granulator forms a uniform material layer on the disc through the action of rotation and centrifugal force, and gradually forms particles during the diffusion process, the method can ensure that the particle size of the calcium hypochlorite coated with nano-alumina is uniform, thereby improving the stability and consistency of the suspension; in addition, during the disc granulation process, the nano-alumina can more effectively coat the calcium hypochlorite particles to form a dense coating layer, which not only protects the activity of calcium hypochlorite, but also improves its stability and durability in water. Therefore, the nano-alumina coated calcium hypochlorite suspension prepared by the disc granulator of the present invention has more optimized particle morphology and surface properties, which helps to improve the dispersibility, solubility and use effect of the product. Compared with the traditional mechanical stirring method, the nano-alumina coated calcium hypochlorite product prepared by the disc granulator has consistent particle morphology and excellent surface properties, which helps to improve the overall quality and stability of the product.

[0025] As a preferred embodiment of the present technical solution, in step S3, after adding silicate cement and stirring evenly, desulfurized gypsum is immediately added and stirring is continued for 20-40 minutes.

[0026] The present invention adds silicate cement first and then desulfurized gypsum to the suspension of calcium hypochlorite coated with nano-alumina, which can promote the hydration reaction of silicate cement and enhance the strength and viscosity of the whole system. If the order of adding silicate cement and desulfurized gypsum is reversed, firstly, desulfurized gypsum may react with the water and part of calcium hypochlorite in the system first (although the stability of calcium hypochlorite in water may be protected by the coating layer), but this may consume part of the water and may affect the subsequent hydration reaction rate and degree of silicate cement, and finally affect the strength of the system; secondly, the addition of desulfurized gypsum may form a thin film covering the surface of part of the particles, hindering the direct contact between silicate cement particles and water, thereby delaying the start of hydration reaction, and further leading to the delay of system strength development; finally, desulfurized gypsum may also react with the hydration product of silicate cement to form a more complex mineral phase, thereby affecting the overall performance of the system.

[0027] As a preferred embodiment of the present technical solution, in step S4, during the drying, the temperature is controlled to be 90-120° C. and the time is 1-3 hours.

[0028] In a third aspect, the present invention also discloses the use of the above solid absorbent in the removal of low-concentration nitrogen oxides and sulfur dioxide, wherein the initial concentration of the nitrogen oxides is 2-20 mg / m 3 The initial concentration of sulfur dioxide is 2-20 mg / m 3 , and should also belong to the protection scope of the present invention.

[0029] The solid absorbent for nitrogen oxides and sulfur dioxide of the present invention and the preparation method thereof have at least the following characteristics:

[0030] Beneficial effects:

[0031] The nitrogen oxide and sulfur dioxide solid absorbent of the present invention is mainly prepared from desulfurization wastewater, desulfurization gypsum, calcium hypochlorite, silicate cement and nano-alumina, wherein the desulfurization wastewater itself is weakly acidic and contains relatively rich chloride ions. Under acidic conditions, chloride ions can greatly improve the oxidizability of calcium hypochlorite to oxidize nitrogen oxide and sulfur dioxide into nitrate and sulfate. At the same time, the oxide film in the porous structure of nano-alumina provides a physical barrier for calcium hypochlorite, reducing the chance of direct contact between calcium hypochlorite and air, and the chemical stability of nano-alumina itself also helps to maintain the stability of the entire mixed system, preventing calcium hypochlorite from failing due to reaction with other chemical substances. In addition, the porous structure and wear resistance of nano-alumina will also produce synergistic effects with other components, further enhancing the protective effect on calcium hypochlorite, so that calcium hypochlorite can continuously exert a high oxidizability. Finally, by introducing silicate cement and desulfurized gypsum, the alkaline substances such as calcium carbonate or calcium hydroxide remaining in the desulfurized gypsum can promote the hydration reaction of silicate cement and enhance the strength and viscosity of the entire system. Therefore, the structure of nano-alumina-coated calcium hypochlorite can be evenly adhered to the silicate cement, thereby effectively avoiding the problem of powder falling easily after the solid absorbent is formed.

[0032] Studies have shown that the solid absorbent prepared by the present invention has excellent removal effects on low-concentration nitrogen oxides and sulfur dioxide. The solid absorbent has a nitrogen oxide removal rate of up to 94% and an absorption rate of up to 0.8 g / (100 g·s). The solid absorbent has a sulfur dioxide removal rate of up to 92.3% and an absorption rate of up to 0.72 g / (100 g·s). It can be used as an auxiliary means for SCR and wet desulfurization to remove low-concentration NO in thermal power plants. X and SO2 for deep treatment to further reduce NO X and SO2 emission concentrations, and reduce the cumulative damage to the environment caused by long-term continuous emissions of low-concentration nitrogen oxides and sulfur dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1The present invention is a flow chart of the preparation method of the solid absorbent for nitrogen oxides and sulfur dioxide. DETAILED DESCRIPTION

[0035] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] Reference Figure 1 Preparation method flow chart of nitrogen oxide and sulfur dioxide solid absorbent The following solid absorbent is prepared:

[0040] S1. Take 100 ml of desulfurization wastewater, add 0.06 g of polyacrylamide to the desulfurization wastewater, stir thoroughly for 1-10 min, let it stand for 1-2 h, add 10 g of calcium hypochlorite to the supernatant, stir and dissolve to obtain a mixed solution;

[0041] S2. Add 60 g of 10-20 nm γ-type nano-alumina to the mixed solution, and place it in a disc granulator for stirring and dispersion to obtain a suspension of calcium hypochlorite coated with nano-alumina, wherein the rotation speed of the disc granulator is 30 rpm and the processing time is 60 min;

[0042] S3, add 11g of Portland cement to the suspension of nano-alumina-coated calcium hypochlorite, stir evenly, and immediately add 35g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15%, continue stirring for 20-40min, and after stirring evenly, obtain a viscous liquid mixture;

[0043] S4. Place the viscous liquid mixture in a honeycomb mold, press it into a honeycomb shape, and place it in a 90-120°C oven for curing for 1-3 hours to obtain a solid absorbent having a size of 11x10x5cm and a pore size of 2mm.

[0044] Example 2

[0045] S1. Take 80 ml of desulfurization wastewater, add 0.04 g of polyacrylamide and 0.02 g of polyaluminum chloride to the desulfurization wastewater, stir thoroughly for 1-10 min, let stand for 1-2 h, add 8 g of calcium hypochlorite to the supernatant, stir and dissolve to obtain a mixed solution;

[0046] S2. Add 50 g of 10-20 nm γ-type nano-alumina to the mixed solution, and place it in a disc granulator for stirring and dispersion to obtain a suspension of calcium hypochlorite coated with nano-alumina, wherein the rotation speed of the disc granulator is 15 rpm and the processing time is 120 min;

[0047] S3, add 10g of Portland cement to the suspension of nano-alumina-coated calcium hypochlorite, stir evenly, and immediately add 25g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15%, continue stirring for 20-40min, and after stirring evenly, obtain a viscous liquid mixture;

[0048] S4. Place the viscous liquid mixture in a honeycomb mold, press it into a honeycomb shape, and place it in a 90-120°C oven for curing for 1-3 hours to obtain a solid absorbent having a size of 11x10x5cm and a pore size of 2mm.

[0049] Example 3

[0050] S1. Take 120 ml of desulfurization wastewater, add 0.08 g of polyacrylic acid to the desulfurization wastewater, stir thoroughly for 1-10 min, let stand for 1-2 h, add 12 g of calcium hypochlorite to the supernatant, stir and dissolve to obtain a mixed solution;

[0051] S2. Add 72 g of 10-20 nm γ-type nano-alumina to the mixed solution, and place it in a disc granulator for stirring and dispersion to obtain a suspension of calcium hypochlorite coated with nano-alumina, wherein the rotation speed of the disc granulator is 30 rpm and the processing time is 60 min;

[0052] S3, add 12g of Portland cement to the suspension of nano-alumina-coated calcium hypochlorite, stir evenly, and immediately add 45g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15%, continue stirring for 20-40min, and after stirring evenly, obtain a viscous liquid mixture;

[0053] S4. Place the viscous liquid mixture in a honeycomb mold, press it into a honeycomb shape, and place it in a 90-120°C oven for curing for 1-3 hours to obtain a solid absorbent having a size of 11x10x5cm and a pore size of 2mm.

[0054] Example 4

[0055] S1. Take 100 ml of desulfurization wastewater, add 0.03 g of ferric chloride and 0.03 g of aluminum sulfate to the desulfurization wastewater, stir thoroughly for 1-10 min, let stand for 1-2 h, add 9 g of calcium hypochlorite to the supernatant, stir and dissolve to obtain a mixed solution;

[0056] S2. Add 65 g of 10-20 nm γ-type nano-alumina to the mixed solution, and place it in a disc granulator for stirring and dispersion to obtain a suspension of calcium hypochlorite coated with nano-alumina, wherein the rotation speed of the disc granulator is 30 rpm and the processing time is 60 min;

[0057] S3, add 11g of Portland cement to the suspension of nano-alumina-coated calcium hypochlorite, stir evenly, and immediately add 30g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15%, continue stirring for 20-40min, and after stirring evenly, obtain a viscous liquid mixture;

[0058] S4. Place the viscous liquid mixture in a honeycomb mold, press it into a honeycomb shape, and place it in a 90-120°C oven for curing for 1-3 hours to obtain a solid absorbent having a size of 11x10x5cm and a pore size of 2mm.

[0059] Example 5

[0060] S1. Take 100 ml of desulfurization wastewater, add 0.05 g of polyacrylamide and 0.02 g of starch to the desulfurization wastewater, stir thoroughly for 1-10 min, let stand for 1-2 h, add 11 g of calcium hypochlorite to the supernatant, stir and dissolve to obtain a mixed solution;

[0061] S2. Add 65 g of 10-20 nm γ-type nano-alumina to the mixed solution, and place it in a disc granulator for stirring and dispersion to obtain a suspension of calcium hypochlorite coated with nano-alumina, wherein the rotation speed of the disc granulator is 30 rpm and the processing time is 60 min;

[0062] S3, add 12g of Portland cement to the suspension of nano-alumina-coated calcium hypochlorite, stir evenly, and immediately add 40g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15%, continue stirring for 20-40min, and after stirring evenly, obtain a viscous liquid mixture;

[0063] S4. Place the viscous liquid mixture in a honeycomb mold, press it into a honeycomb shape, and place it in a 90-120°C oven for curing for 1-3 hours to obtain a solid absorbent having a size of 11x10x5cm and a pore size of 2mm.

[0064] Example 6

[0065] S1. Take 100 ml of desulfurization wastewater, add 0.07 g of polyacrylamide to the desulfurization wastewater, stir thoroughly for 1-10 min, let stand for 1-2 h, add 12 g of calcium hypochlorite to the supernatant, stir and dissolve to obtain a mixed solution;

[0066] S2. Add 70 g of 10-20 nm γ-type nano-alumina to the mixed solution, and place it in a disc granulator for stirring and dispersion to obtain a suspension of calcium hypochlorite coated with nano-alumina, wherein the rotation speed of the disc granulator is 30 rpm and the processing time is 60 min;

[0067] S3, add 11g of Portland cement to the suspension of nano-alumina-coated calcium hypochlorite, stir evenly, and immediately add 40g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15%, continue stirring for 20-40min, and after stirring evenly, obtain a viscous liquid mixture;

[0068] S4. Place the viscous liquid mixture in a honeycomb mold, press it into a honeycomb shape, and place it in a 90-120°C oven for curing for 1-3 hours to obtain a solid absorbent having a size of 11x10x5cm and a pore size of 2mm.

[0069] Comparative Example 1

[0070] This control example is basically the same as Example 1, except that tap water is used instead of the desulfurization wastewater supernatant in Example 1.

[0071] Comparative Example 2

[0072] This comparative example is basically the same as Example 1, except that manganese dioxide is used to replace the nano-aluminum oxide in Example 1.

[0073] Comparative Example 3

[0074] This comparative example is basically the same as Example 1, except that no nano-alumina is added.

[0075] Comparative Example 4

[0076] This comparative example is basically the same as Example 1, except that no desulfurized gypsum is added and only silicate cement is used as a viscosity agent.

[0077] Comparative Example 5

[0078] This control example is basically the same as Example 1, except that after adding nano-alumina to the mixed solution, a suspension of nano-alumina-coated calcium hypochlorite is prepared by mechanical stirring, wherein the speed of the mechanical stirring is 200 rpm and the stirring time is 60 min.

[0079] Comparative Example 6

[0080] This control example is basically the same as Example 1, except that: 35g of desulfurized gypsum with a particle size of 30-60μm and a moisture content of 10%-15% is first added to the suspension of nano-alumina-coated calcium hypochlorite, and then 11g of silicate cement is added, and stirring is continued for 20-40min. After stirring evenly, a viscous liquid mixture is obtained.

[0081] Test example

[0082] Test method:

[0083] Prepare a test chamber with a volume of 10 cubic meters and ensure that the inner wall of the test chamber is made of inert material to avoid adsorption or reaction to the test gas, while ensuring good sealing to prevent gas leakage.

[0084] According to the test requirements, the temperature in the experimental chamber is set and maintained at 25-30℃ to simulate the actual use environment.

[0085] According to the test requirements, a mixed gas containing nitrogen oxides and sulfur dioxide is prepared to ensure that the gas concentration is stable and controllable.

[0086] Prepare the solid absorbent according to certain specifications and quantities and place it at the designated location in the experimental chamber.

[0087] Test steps:

[0088] System inspection: Before the formal test, check the connection and working status of equipment such as the experimental cabin, composite gas detector and gaseous pollutant generating device to ensure that everything is normal.

[0089] Background concentration measurement: Turn off the gaseous pollutant generating device, turn on the composite gas detector, measure the background concentration in the experimental chamber (i.e. the concentration of nitrogen oxides and sulfur dioxide when no test gas is introduced), and record the data.

[0090] Introduce test gas: Turn on the gaseous pollutant generator and introduce a mixed gas containing nitrogen oxides and sulfur dioxide into the experimental chamber at a wind volume of 300m3 / h (the oxide film formed by this nano-aluminum oxide on the surface of calcium hypochlorite can isolate a certain amount of air. Therefore, only under a certain wind volume can the mixed gas pass through this film to react with calcium hypochlorite), so that the pollutants are fully in contact with the absorbent.

[0091] Concentration monitoring: During the process of introducing the test gas, the composite gas detector is used to continuously monitor the changes in the concentrations of nitrogen oxides and sulfur dioxide in the experimental chamber and record the data.

[0092] Data recording and analysis: Based on the monitoring data, calculate the absorption efficiency of the absorbent for nitrogen oxides and sulfur dioxide, and perform data analysis.

[0093] Tables 1-14 show the immediate absorption effects of the solid absorbents obtained in Example 1 and Comparative Examples 1-6, as well as the absorption effects after being placed in the air for 1 week, 1 month, and 3 months after the first test.

[0094] Table 1 Absorption effect of solid absorbent in Example 1

[0095] Test gas <![CDATA[Initial concentration mg / m 3 > <![CDATA[Reaction concentration after 1 h, mg / m 3 > Absorption efficiency % <![CDATA[SO2]]> 5.03 0.37 92.6 <![CDATA[NO2]]> 2.45 0.14 94.3 NO 2.02 0.06 97.0

[0096] Table 2 Stability test data of solid absorbent of Example 1

[0097]

[0098] Table 3 Absorption effect of solid absorbent of comparative example 1

[0099] Test gas <![CDATA[Initial concentration mg / m 3 > <![CDATA[Reaction concentration after 1 h, mg / m 3 > Absorption efficiency % <![CDATA[SO2]]> 5.03 1.21 75.9 <![CDATA[NO2]]> 2.45 0.75 69.4 NO 2.02 0.69 65.8

[0100] Table 4 Stability test data of solid absorbent of comparative example 1

[0101]

[0102] Table 5 Absorption effect of solid absorbent of comparative example 2

[0103] Test gas <![CDATA[Initial concentration mg / m 3 > <![CDATA[Reaction concentration after 1 h, mg / m 3 > Absorption efficiency % <![CDATA[SO2]]> 5.03 0.72 85.7 <![CDATA[NO2]]> 2.45 0.45 81.6 NO 2.02 0.34 83.2

[0104] Table 6 Stability test data of solid absorbent of comparative example 2

[0105]

[0106] Table 7 Absorption effect of solid absorbent of comparative example 3

[0107] Test gas <![CDATA[Initial concentration mg / m 3 > <![CDATA[Reaction concentration after 1 h, mg / m 3 > Absorption efficiency % <![CDATA[SO2]]> 5.03 0.88 82.5 <![CDATA[NO2]]> 2.45 0.75 69.4 NO 2.02 0.67 66.8

[0108] Table 8 Stability test data of solid absorbent of comparative example 3

[0109]

[0110] Table 9 Absorption effect of solid absorbent of comparative example 4

[0111] Test gas <![CDATA[Initial concentration mg / m 3 > <![CDATA[Reaction concentration after 1 h, mg / m 3 > Absorption efficiency % <![CDATA[SO2]]> 5.03 0.56 88.9 <![CDATA[NO2]]> 2.45 0.38 84.5 NO 2.02 0.21 89.6

[0112] Table 10 Stability test data of solid absorbent of Comparative Example 4

[0113]

[0114] Table 11 Absorption effect of solid absorbent of comparative example 5

[0115] Test gas <![CDATA[Initial concentration mg / m 3 > <![CDATA[Concentration after 1-hour reaction, mg / m 3 > Absorption efficiency % <![CDATA[SO2]]> 5.03 0.52 89.66 <![CDATA[NO2]]> 2.45 0.35 85.71 NO 2.02 0.27 86.63

[0116] Table 12 Stability test data of solid absorbent of comparative example 5

[0117]

[0118] Table 13 Absorption effect of solid absorbent of comparative example 6

[0119]

[0120]

[0121] Table 14 Stability test data of solid absorbent of comparative example 6

[0122]

[0123] As shown in Table 1-14, compared with the control examples 1-6, the solid absorbent prepared in Example 1 of the present invention has excellent removal effect on low-concentration nitrogen oxides and sulfur dioxide, and calcium hypochlorite can exert high oxidizing stability for a long time. Therefore, the solid absorbent can be used as an auxiliary means of SCR and wet desulfurization to remove low-concentration NO in thermal power plants. X and SO2 for deep treatment to further reduce NO X and SO2 emission concentrations, and reduce the cumulative damage to the environment caused by long-term continuous emissions of low-concentration nitrogen oxides and sulfur dioxide.

[0124] Among them, in Control Example 1, tap water is used instead of the desulfurization wastewater supernatant of the present invention. Although the prepared solid absorbent has a certain oxidizing property to nitrogen oxides and sulfur dioxide in the initial stage, due to the extremely low chloride ion content in tap water, the oxidizing property of calcium hypochlorite cannot be effectively maintained, resulting in a significant decrease in the oxidizing property of the solid absorbent after being stored in the air for a period of time.

[0125] In Comparative Example 2, manganese dioxide is used to replace the nano-alumina in the present invention. Since it is unable to form a film to protect calcium hypochlorite from interference from gases in the environment, the solid absorbent cannot continuously and effectively maintain its oxidizing properties against nitrogen oxides and sulfur dioxide.

[0126] In Control Example 3, nano-alumina was not used to coat calcium hypochlorite, which greatly reduced the service life and stability of the solid absorbent.

[0127] In Comparative Example 4, only silicate cement was used as a binder, and the solid absorbent obtained after molding had problems such as dust and ash easily falling off.

[0128] In Comparative Example 5, a suspension of calcium hypochlorite coated with nano-alumina was prepared by mechanical stirring. Although the nano-alumina could coat calcium hypochlorite well to a certain extent, the dispersibility, solubility and use effect of the product were still slightly inferior to those of the disc granulation method. Therefore, the service life and stability of the prepared solid absorbent need to be further improved.

[0129] In Comparative Example 6, reversing the order of adding desulfurized gypsum and silicate cement will affect the hydration reaction rate and degree of silicate cement, and further affect the overall performance of the system. Therefore, the bonding performance of the prepared solid absorbent is poor.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A solid absorbent for nitrogen oxides and sulfur dioxide, characterized in that: The invention comprises the following raw materials in parts by weight: 80-120 parts of desulfurization wastewater, 8-12 parts of calcium hypochlorite, 50-72 parts of nano alumina, 10-12 parts of silicate cement and 25-45 parts of desulfurization gypsum.

2. The solid absorbent according to claim 1, characterized in that: Also includes 0.004-0.008 parts of flocculant; The flocculant includes any one of ferric chloride, aluminum sulfate, polyaluminum chloride, polyacrylamide, polyacrylic acid, starch, lignin and chitosan.

3. The solid absorbent according to claim 1, characterized in that: The nano-alumina is γ-Al2O3, and its particle size is 10-20nm.

4. The solid absorbent according to claim 1, characterized in that: The particle size of the desulfurized gypsum is 30-60 μm, and the moisture content is 10%-15%.

5. The method for preparing the solid absorbent according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. flocculating the desulfurization wastewater using a flocculant, mixing the supernatant with calcium hypochlorite, stirring and dissolving, and obtaining a mixed solution; S2, adding nano-alumina to the mixed solution, stirring evenly, to obtain a suspension of nano-alumina-coated calcium hypochlorite; S3, adding silicate cement and desulfurized gypsum to the suspension of nano-alumina-coated calcium hypochlorite in sequence, stirring evenly to obtain a viscous liquid mixture; S4. Press the viscous liquid mixture into a honeycomb shape and then dry it to obtain a solid absorbent.

6. The preparation method according to claim 5, characterized in that: In step S1, during the flocculation treatment, a flocculant is added to the desulfurization wastewater and stirred for 1-10 minutes, and then allowed to settle for 1-2 hours.

7. The preparation method according to claim 5, characterized in that: In step S2, the mixed solution and nano-alumina are placed in a disc granulator for stirring and dispersion to obtain a suspension of nano-alumina-coated calcium hypochlorite; Wherein, the rotation speed of the disc granulator is 15-30rpm, and the processing time is 60-120min.

8. The preparation method according to claim 5, characterized in that: In step S3, after adding silicate cement and stirring evenly, desulfurized gypsum is immediately added and stirring is continued for 20-40 minutes.

9. The preparation method according to claim 5, characterized in that: In step S4, during the drying, the temperature is controlled to be 90-120° C. and the time is 1-3 hours.

10. Use of the solid absorbent according to any one of claims 1 to 4, characterized in that: The solid absorbent is used in the removal of low-concentration nitrogen oxides and sulfur dioxide, wherein the initial concentration of the nitrogen oxides is 2-20 mg / m 3 The initial concentration of sulfur dioxide is 2-20 mg / m 3 .