Modified calcium-based desulfurizing agent and preparation method thereof
Through the combination of calcium hydroxide and modified zeolite, the zeolite is treated with a modifier, which improves the specific surface area and effective test time of the desulfurizer, solves the problems of low utilization rate and frequent material replacement of existing desulfurizers, and achieves efficient The flue gas desulfurization effect and reduces operating costs.
Patent Information
- Application Number
- CN202411064811.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing desulfurizer has a small specific surface area and low effective utilization rate. It requires frequent material replacement, which increases operating costs and also causes waste of resources. The preparation steps are complex, energy consumption is high and cost-effective.
Modified calcium-based desulfurization agent made of calcium hydroxide and modified zeolite, and pretreat the zeolite by aqueous modification solution to enhance its specific surface area and effective testing time. The modification agent is selected from acid modifiers and alkali modifiers. With the inorganic salt modifier, the weight ratio of calcium hydroxide to zeolite is 40-80:40-80, the aqueous solution concentration of the modifier is more than 3 wt%, the drying temperature is 100-200°C, and the amount of wetting added to wet is 1- 30 wt%.
It improves the specific surface area and effective test time of the desulfurizer, enhances the adsorption capacity, reduces equipment investment and operation costs, simplifies the process flow, extends the use cycle, and solves the problems of low utilization rate of the desulfurizer and frequent material replacement.
Abstract
Description
Technical Field
[0001] The invention relates to a modified calcium-based desulfurizing agent and a preparation method thereof. Background Art
[0002] There are three types of desulfurization: before combustion, during combustion and after combustion. With the development of industry and the improvement of people's living standards, the demand for energy continues to increase, and SO2 in coal-fired flue gas has become the main cause of air pollution.
[0003] Reducing SO2 pollution has become a top priority for today's atmospheric environmental governance. Many flue gas desulfurization processes have been widely used in industry, among which fixed-bed dry flue gas desulfurization technology has attracted much attention due to its high efficiency, simple process and no wastewater discharge. However, existing desulfurizers generally have problems such as small specific surface area and low effective utilization rate, requiring frequent material changes, which increases operating costs and also causes waste of resources.
[0004] CN117865513A discloses a method for preparing a functionalized graphene-modified calcium hydroxide desulfurizer, comprising: mixing quicklime and amino-functionalized graphene uniformly, adding water, and reacting to obtain a modified calcium hydroxide desulfurizer. The specific surface area of the modified calcium hydroxide desulfurizer obtained in the patent document is 45 to 60 m 2 / g, still needs to be further improved.
[0005] CN116459664A discloses a cement desulfurizer, including a desulfurizer and a catalyst, wherein the desulfurizer is calcium hydroxide powder, and the catalyst preparation steps include: preparing a rare earth modified zeolite desulfurizer matrix; obtaining an iridium oxide layer coated matrix; treating the iridium oxide layer coated matrix with a hydrogen peroxide solution and ozone to obtain a catalyst component I; synthesizing a catalyst component II; and uniformly mixing the catalyst component I and the catalyst component II to obtain a catalyst. Although the specific surface area of the cement desulfurizer has been improved, its effective test time still needs to be improved. In addition, its preparation steps are relatively cumbersome, the energy consumption is high, and the cost is high.
[0006] CN113750759A discloses a method for preparing a combined desulfurizer, comprising: selecting activated alumina as a carrier, preparing a mixed solution A, and spraying the mixed solution A onto the carrier to obtain a semi-finished product; activating the semi-finished product to obtain a DHS-1 desulfurizer; preparing a mixed solution B, and mixing with alumina powder A to obtain a powder B; using the powder B to make particles, and performing a roasting treatment to obtain a semi-finished product; reducing and heating the roasted semi-finished product to obtain a DHS-2 desulfurizer. The specific surface area and effective test time of the obtained desulfurizer still need to be improved. In addition, the process of the preparation method is slightly complicated. Summary of the invention
[0007] In view of this, one object of the present invention is to provide a modified calcium-based desulfurizer, which has a larger specific surface area, a longer effective test time, and a higher desulfurization rate. Another object of the present invention is to provide a method for preparing the modified calcium-based desulfurizer as described above.
[0008] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.
[0009] In one aspect, the present invention provides a modified calcium-based desulfurizer, which is made of the following raw materials: calcium hydroxide and modified zeolite.
[0010] The modified zeolite is obtained by pre-treating the zeolite with a modifier aqueous solution, and the weight ratio of the zeolite to the modifier in the modifier aqueous solution is 40-80:3-20; the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier;
[0011] Wherein, the weight ratio of the calcium hydroxide to the zeolite is 40-80:40-80, and the weight of the calcium hydroxide is greater than or equal to the weight of the zeolite.
[0012] According to the modified calcium-based desulfurizer of the present invention, preferably, the acid modifier is selected from one of boric acid, phosphoric acid, citric acid and oxalic acid; the alkali modifier is selected from at least one of sodium hydroxide and potassium hydroxide; the inorganic salt modifier is selected from at least one of sodium chloride, potassium chloride and ammonium chloride.
[0013] According to the modified calcium-based desulfurizer of the present invention, preferably, the acid modifier is selected from one of boric acid and oxalic acid; the alkali modifier is potassium hydroxide; and the inorganic salt modifier is potassium chloride.
[0014] According to the modified calcium-based desulfurizer of the present invention, preferably, the modified zeolite is obtained by pretreatment comprising the following steps: immersing the zeolite in an aqueous solution of the modifier, standing for 1.5 to 6 hours, separating the solid and the liquid, drying the separated solid, and then crushing to obtain the modified zeolite.
[0015] According to the modified calcium-based desulfurizer of the present invention, preferably, the concentration of the modifying agent aqueous solution is above 3 wt %.
[0016] According to the modified calcium-based desulfurizer of the present invention, preferably, the drying temperature is 100-200° C., and the drying time is 0.5-3 h.
[0017] The modified calcium-based desulfurizer according to the present invention is preferably made of only the following raw materials: calcium hydroxide and modified zeolite.
[0018] The modified zeolite is obtained by pre-treating the zeolite with a modifier aqueous solution, and the weight ratio of the zeolite to the modifier in the modifier aqueous solution is 40-80:3-20; the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier;
[0019] Wherein, the weight ratio of the calcium hydroxide to the zeolite is 40-80:40-80, and the weight of the calcium hydroxide is greater than or equal to the weight of the zeolite.
[0020] On the other hand, the present invention also provides a method for preparing the modified calcium-based desulfurizer as described above, comprising the following steps:
[0021] 1) pretreating zeolite with a modifier aqueous solution to obtain modified zeolite;
[0022] 2) stirring and mixing the modified zeolite and calcium hydroxide, adding water to moisten the mixture during the stirring and mixing process to obtain a mixture; kneading the mixture into a molded semi-finished product; drying the molded semi-finished product to obtain a modified calcium-based desulfurizer; wherein the amount of water added for moistening is 1 to 30 wt% of the sum of the weight of the modified zeolite and the calcium hydroxide.
[0023] According to the preparation method of the present invention, preferably, step 1) includes the following specific steps: immersing the zeolite in a modifier aqueous solution, standing for 1.5 to 6 hours, separating the solid and the liquid, drying the obtained solid, and then crushing it to obtain a modified zeolite; wherein the concentration of the modifier aqueous solution is above 3wt%.
[0024] According to the preparation method of the present invention, preferably, in step 2), the drying temperature is 100-200° C., and the drying time is 1-3 h.
[0025] The modified calcium-based desulfurizer of the present invention has a large specific surface area, a long effective test time, a high desulfurization rate, and a long service life, and can basically solve the problems of low desulfurizer utilization and frequent material changes. The preparation method of the present invention is relatively simple and is conducive to popularization and application. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0027] The modified calcium-based desulfurizer of the present invention is made of calcium hydroxide and modified zeolite, wherein the modified zeolite is obtained by pre-treating the zeolite with a specific modifier, and the weight ratio of calcium hydroxide to zeolite is within a specific range. The present invention has found through a large number of studies and experiments that such a modified calcium-based desulfurizer has a larger specific surface area, a longer effective test time, and a higher desulfurization rate. Although there are several common methods for the modification of zeolite, it is not conventional to select what kind and what amount of modifier is used to modify the zeolite and the modified zeolite obtained after the modified zeolite is used in conjunction with what amount of calcium hydroxide so that the formed desulfurizer has a larger specific surface area, a longer effective test time, and a higher desulfurization rate. Moreover, in the prior art, there is no report on the use of an excellent desulfurizer formed by modifying the zeolite with an acid modifier, an alkali modifier, or an inorganic salt modifier and then using it in conjunction with calcium hydroxide.
[0028] <Modified calcium-based desulfurizer>
[0029] The modified calcium-based desulfurizer of the present invention is made of the following raw materials: calcium hydroxide and modified zeolite, wherein the modified zeolite is obtained by pre-treating the zeolite with a modifier aqueous solution, and the weight ratio of the zeolite to the modifier in the modifier aqueous solution is 40-80:3-20; the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier;
[0030] The weight ratio of calcium hydroxide to zeolite is 40-80:40-80, and the weight of calcium hydroxide is greater than or equal to the weight of the zeolite. Preferably, the weight of calcium hydroxide is greater than the weight of the zeolite.
[0031] In the present invention, the zeolite may be clinoptilolite or mordenite.
[0032] In the present invention, the modified zeolite is obtained by pre-treating the zeolite with a modifier aqueous solution. Specifically, the zeolite is soaked with a modifier aqueous solution, the solid-liquid separation is performed, the separated solid is dried, and then the modified zeolite is obtained by crushing. In this way, the performance of the zeolite can be improved, and then the performance of the desulfurizer can be improved. The present invention believes that the zeolite has excellent holes and channels after pretreatment, and the specific surface area is significantly increased, which can greatly improve the adsorption capacity. At the same time, the change in the pore structure is conducive to the exposure of the active center of the adsorption reaction inside the zeolite, further improving the adsorption performance, and promoting the diffusion and adsorption of sulfur dioxide and water molecules. In addition, the aluminum oxide and silicon dioxide in the modified zeolite will react chemically with calcium hydroxide during the composite process to change the inherent structure and composition of the material, and the specific surface area can be increased while the active components can be stimulated, the dispersibility of calcium hydroxide can be improved, the adsorption capacity of sulfur dioxide can be enhanced, the desulfurization reaction speed can be promoted, and the effective utilization rate of the desulfurizer can be improved, and the equipment investment and operating costs of the flue gas desulfurization system can be effectively reduced. In addition, since the zeolite itself has a certain viscosity, there is no need to use an additional binder during the preparation process, which saves costs.
[0033] In the present invention, the weight ratio of zeolite to modifier may be 40-80:3-20, preferably 40-80:7-20, more preferably 40-80:13-20. The weight of the modified zeolite obtained in the present invention is not the sum of the weights of zeolite and modifier.
[0034] In the present invention, the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier. In certain embodiments, the modifier is an acid modifier, and the acid modifier is selected from one of boric acid, phosphoric acid, citric acid and oxalic acid, preferably selected from one of boric acid and oxalic acid, and more preferably oxalic acid. In other embodiments, the modifier is an alkali modifier, and the alkali modifier is selected from at least one of sodium hydroxide and potassium hydroxide, preferably potassium hydroxide. In still other embodiments, the modifier is an inorganic salt modifier, and the inorganic salt modifier is selected from at least one of sodium chloride, potassium chloride and ammonium chloride, preferably potassium chloride.
[0035] When preparing the modified calcium-based desulfurizer, the modifier is used in the form of a modifier aqueous solution. In the present invention, the weight of the modifier does not include the weight of water. The concentration of the modifier aqueous solution can be 3wt% or more, preferably 10wt% or more, and more preferably 15wt% or more.
[0036] In some specific embodiments, the concentration of the acid modifier aqueous solution can be 3-30wt%, preferably 7-25wt%, more preferably 12-20wt%. The time for soaking the zeolite in the acid modifier aqueous solution can be 1.5-6h, preferably 1.5-5h, more preferably 2-4h.
[0037] In other specific embodiments, the concentration of the aqueous solution of the alkaline modifier can be 3-65wt%, preferably 7-45wt%, more preferably 12-35wt%, and further preferably 15-20wt%. The time for soaking the zeolite in the aqueous solution of the alkaline modifier can be 1-6h, preferably 2-5h, and more preferably 2.5-4.5h.
[0038] In some specific embodiments, the concentration of the inorganic salt modifier aqueous solution can be 10-40wt%, preferably 15-35wt%, more preferably 20-25wt%. The time for soaking the zeolite in the inorganic salt modifier aqueous solution can be 0.5-3h, preferably 1.5-3h, more preferably 2.5-3h.
[0039] According to one embodiment of the present invention, the modified calcium-based desulfurizer of the present invention is made of only the following raw materials: calcium hydroxide and modified zeolite, wherein the modified zeolite is obtained by pre-treating zeolite with an aqueous solution of a modifier, and the weight ratio of the zeolite to the modifier in the aqueous solution of the modifier is 40-80:3-20; the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier; wherein the weight ratio of the calcium hydroxide to the zeolite is 40-80:40-80, and the weight of the calcium hydroxide is greater than or equal to the weight of the zeolite.
[0040] <Preparation method>
[0041] The present invention also provides a method for preparing the modified calcium-based desulfurizer as described above, comprising the following steps: (1) a step of forming a modified zeolite; (2) a step of mixing the modified zeolite and calcium hydroxide; (3) a step of kneading and molding; and (4) a step of forming a modified calcium-based desulfurizer.
[0042] Steps for forming modified zeolite
[0043] The zeolite is pretreated with an aqueous solution of a modifier to obtain a modified zeolite. Specifically, the zeolite is soaked with an aqueous solution of a modifier, the solid and the liquid are separated, the separated solid is dried, and then crushed to obtain the modified zeolite. The present invention believes that the pretreatment can achieve the modulation of the pore size of the zeolite, can enhance the adsorption and diffusion mass transfer capacity of the zeolite to the adsorbate, improve the performance of the zeolite, and then improve the performance of the desulfurizer. The type and amount of zeolite, the type and amount of the modifier, the concentration of the aqueous solution of the modifier, and more specific pretreatment steps have been described in detail above and will not be repeated here.
[0044] Mixing steps of modified zeolite and calcium hydroxide
[0045] The modified zeolite and calcium hydroxide are stirred and mixed, and water is added during the stirring and mixing process to obtain a mixture; the amount of water added for wetting is 1 to 30 wt% of the total weight of the modified zeolite and calcium hydroxide, which is conducive to uniform mixing and effectively improves the performance of the desulfurizer.
[0046] The amount of water added for wetting can be 1-30wt% of the total weight of the modified zeolite and calcium hydroxide, preferably 3-20wt%, for example 3wt%, 5wt%, 7wt%, 8wt%, 10wt%, 15wt%, 18wt%, 20wt%. The mixing time can be 20-30min.
[0047] Kneading and molding steps
[0048] The mixture is kneaded into a shape to obtain a semi-finished product.
[0049] In the present invention, the kneading molding can be performed by extrusion molding using a granulating extruder or tablet molding using a tablet press.
[0050] The semi-finished product may be in the shape of a column, a four-leaf clover or a sheet. According to one embodiment of the present invention, the semi-finished product is in the shape of a column.
[0051] Formation steps of modified calcium-based desulfurizer
[0052] The formed semi-finished product is dried to obtain a modified calcium-based desulfurizer.
[0053] The drying temperature is 100 to 200° C., preferably 150 to 190° C., more preferably 150 to 180° C. The drying time is 1 to 3 hours, preferably 1.5 to 3 hours, more preferably 2 to 2.5 hours.
[0054] In the present invention, a drying device such as a mesh belt kiln or a rotary kiln can be used for drying to obtain a modified calcium-based desulfurizer.
[0055] The modified calcium-based desulfurizer product of the present invention has a high desulfurization reaction speed and a lasting effective utilization rate during the desulfurization process due to its high specific surface area, which can improve the desulfurization effect while further reducing equipment operating costs, and is suitable for fixed bed or moving bed dry flue gas desulfurization.
[0056] Unless otherwise specified, in the following examples, the parts mentioned are parts by weight.
[0057] In the following examples, the zeolite is commercially available clinoptilolite.
[0058] Example 1
[0059] The modified calcium-based desulfurizer is prepared according to the formula in Table 1, and the steps are as follows:
[0060] The modifier oxalic acid is dissolved in water to form an oxalic acid aqueous solution. The zeolite is soaked in the oxalic acid aqueous solution, stirred evenly, and allowed to stand at room temperature for 1.5 hours, and then the solid-liquid separation is performed, and the separated solid is placed in an oven and dried at 110°C for 0.5 hours, and then crushed to 100 meshes with a crusher to obtain a modified zeolite.
[0061] The modified zeolite and calcium hydroxide are placed in a mixer for mixing and stirring, and a proper amount of water is added during the stirring process to wet the mixture evenly to obtain a mixture. The mixture is then extruded and formed in a granulator to obtain a columnar semi-finished product. The columnar semi-finished product is placed in a mesh belt kiln and dried at 120°C for 2 hours to obtain a columnar modified calcium-based desulfurizer.
[0062] Example 2
[0063] Except for the following parameter settings, the rest are the same as Example 1: In this example, the modifier used is potassium hydroxide. During the process of forming the modified zeolite, it is left to stand at room temperature for 2.5 hours.
[0064] Example 3
[0065] Except for the following parameter settings, the rest are the same as Example 2: In this example, the modifier used is potassium chloride.
[0066] Example 4
[0067] Except for the following parameter settings, the rest are the same as Example 1: In this example, the modifier used is boric acid.
[0068] Example 5
[0069] Except for the following parameter settings, the rest are the same as Example 1: In this example, the modifier used is phosphoric acid.
[0070] Comparative Example 1
[0071] The difference from Example 1 is that the zeolite is not modified. The specific steps include: placing 40 parts of zeolite and 60 parts of calcium hydroxide in a mixer for mixing and stirring, adding an appropriate amount of water to wet evenly during the stirring process, and then extruding and molding in a granulator to obtain a columnar semi-finished product. The semi-finished product is placed in a mesh belt kiln and dried at 120° C. for 2 hours to obtain a columnar modified calcium-based desulfurizer.
[0072] Comparative Example 2
[0073] The difference from Example 1 is that no modified zeolite is added. The specific steps include: placing 100 parts of calcium hydroxide in a mixer for stirring, adding an appropriate amount of water to wet evenly during the stirring process, and then extruding and molding in a granulator to obtain a columnar semi-finished product. The semi-finished product is placed in a mesh belt kiln and dried at 120° C. for 2 hours to obtain a columnar calcium-based desulfurizer.
[0074] Comparative Example 3
[0075] Except for the following parameter settings, the rest are the same as Example 1: the modifier used is acetic acid.
[0076] Table 1
[0077] serial number Calcium hydroxide / part Zeolite / part Type and quantity of modifier Modifier aqueous solution concentration wt% Example 1 60 40 20 parts of oxalic acid 20 Example 2 60 40 20 parts potassium hydroxide 20 Example 3 60 40 20 parts potassium chloride 20 Example 4 60 40 Boric acid 20 parts 20 Example 5 60 40 Phosphoric acid 20 parts 20 Comparative Example 1 60 40 -- -- Comparative Example 2 100 0 -- -- Comparative Example 3 60 40 20 parts of acetic acid 20
[0078] The modified calcium-based desulfurizers obtained in the examples and comparative examples were tested for their performance.
[0079] Test method: Use JW-DX surface area meter to test surface area; use Testo 340 to test sulfur dioxide concentration. Simulate fixed bed reaction device, at temperature 140℃, oxygen content 10vol%, moisture content 3%, SO2 concentration 200mg / m 3 , reaction space velocity 800h -1 , detect the SO2 concentration of sulfur-containing flue gas before and after treatment with the above desulfurizer. When the SO2 concentration reaches 35mg / m 3 The test was stopped at 1 pm, and the test duration and desulfurization rate were calculated. The results are shown in Table 2.
[0080] Among them, desulfurization rate = (total SO2 content in raw gas - total SO2 content in tail gas) / total SO2 content in raw gas) × 100%.
[0081] The effective test time refers to: based on the ultra-low emission standard, from the time when the sulfur-containing flue gas is treated with the desulfurizer to the time when the SO2 concentration of the sulfur-containing flue gas after the desulfurizer treatment is detected to be 35mg / m 3 Length of time.
[0082] Table 2
[0083] serial number <![CDATA[Specific surface area m 2 / g]]> Desulfurization rate% Effective test time / h Example 1 89.41 >99 63.2 Example 2 102.52 >99 72.8 Example 3 76.86 >99 57.6 Example 4 87.01 >99 61.82 Example 5 85.69 >99 65.78 Comparative Example 1 39.63 >50 19.7 Comparative Example 2 21.29 >40 13.2 Comparative Example 3 41.07 >55 21.8
[0084] It can be seen from Table 2 that the modified calcium-based desulfurizer of the present invention has a larger specific surface area, a longer effective test time, a higher desulfurization rate, and can ensure high desulfurization reaction activity and effective utilization rate.
[0085] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A modified calcium-based desulfurizer, characterized in that: Made from the following raw materials: calcium hydroxide and modified zeolite, The modified zeolite is obtained by pre-treating the zeolite with a modifier aqueous solution, and the weight ratio of the zeolite to the modifier in the modifier aqueous solution is 40-80:3-20; the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier; Wherein, the weight ratio of the calcium hydroxide to the zeolite is 40-80:40-80, and the weight of the calcium hydroxide is greater than or equal to the weight of the zeolite.
2. The modified calcium-based desulfurizer according to claim 1, characterized in that: The acid modifier is selected from one of boric acid, phosphoric acid, citric acid and oxalic acid; the base modifier is selected from at least one of sodium hydroxide and potassium hydroxide; the inorganic salt modifier is selected from at least one of sodium chloride, potassium chloride and ammonium chloride.
3. The modified calcium-based desulfurizer according to claim 1, characterized in that: The acid modifier is selected from one of boric acid and oxalic acid; the base modifier is potassium hydroxide; and the inorganic salt modifier is potassium chloride.
4. The modified calcium-based desulfurizer according to claim 1, characterized in that: The modified zeolite is obtained by pretreatment including the following steps: soaking the zeolite in a modifier aqueous solution, standing for 1.5 to 6 hours, separating the solid from the liquid, drying the separated solid, and then crushing to obtain the modified zeolite.
5. The modified calcium-based desulfurizer according to claim 4, characterized in that: The concentration of the modifying agent aqueous solution is above 3 wt %.
6. The modified calcium-based desulfurizer according to claim 4, characterized in that: The drying temperature is 100-200°C and the drying time is 0.5-3h.
7. The modified calcium-based desulfurizer according to claim 1, characterized in that: Made from the following raw materials only: calcium hydroxide and modified zeolite, The modified zeolite is obtained by pre-treating the zeolite with a modifier aqueous solution, and the weight ratio of the zeolite to the modifier in the modifier aqueous solution is 40-80:3-20; the modifier is selected from one of an acid modifier, an alkali modifier and an inorganic salt modifier; Wherein, the weight ratio of the calcium hydroxide to the zeolite is 40-80:40-80, and the weight of the calcium hydroxide is greater than or equal to the weight of the zeolite.
8. A method for preparing a modified calcium-based desulfurizer according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) pretreating zeolite with a modifier aqueous solution to obtain modified zeolite; 2) stirring and mixing the modified zeolite and calcium hydroxide, adding water to moisten the mixture during the stirring and mixing process to obtain a mixture; kneading the mixture into a molded semi-finished product; drying the molded semi-finished product to obtain a modified calcium-based desulfurizer; wherein the amount of water added for moistening is 1 to 30 wt% of the sum of the weight of the modified zeolite and the calcium hydroxide.
9. The preparation method according to claim 8, characterized in that: Step 1) comprises the following specific steps: soaking zeolite in a modifier aqueous solution, standing for 1.5 to 6 hours, separating the solid and the liquid, drying the obtained solid, and then crushing it to obtain a modified zeolite; wherein the concentration of the modifier aqueous solution is above 3wt%.
10. The preparation method according to claim 9, characterized in that: In step 2), the drying temperature is 100-200° C. and the drying time is 1-3 hours.