COF-5 / 6FBD mixed matrix membrane as well as preparation method and application thereof

By dispersing COF-5 in 6FBD polymer and preparing COF-5/6FBD hybrid matrix membrane, the problem of insufficient helium flux and selectivity in the prior art was solved, and a more efficient helium separation effect was achieved.

CN118904103APending Publication Date: 2024-11-08ZINGKE (CHONGQING) ADVANCED MATERIALS RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410947839.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing mixed matrix membranes are used for helium separation with a smaller helium flux and a lower helium selectivity.

Method used

Using COF-5/6FBD mixed matrix membrane, the helium selectivity of the mixed matrix membrane is optimized by dispersing COF-5 in 6FBD polymer, and the ultra-high specific surface area and unique pore structure of COF-5 are used, and the helium selectivity of the mixed matrix membrane is optimized by solution casting method. Prepare membranes to increase helium flux and selectivity.

Benefits of technology

It significantly improved the helium flux and selectivity, with the maximum helium flux reaching 296GPU, and the selectivity of He/CH4, He/N2 and He/CO2 reached 588, 572, and 391 respectively, improving the helium mass transfer resistance and selectivity .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904103A_ABST
    Figure CN118904103A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of gas separation membrane materials, in particular to a COF-5 / 6FBD mixed matrix membrane as well as a preparation method and application thereof. The COF-5 / 6FBD mixed matrix membrane comprises a 6FBD polymer and COF-5 dispersed in the 6FBD polymer, and the dosage of the COF-5 is 5 wt%-20 wt% of that of the 6FBD polymer. The ultrahigh specific surface area, the unique pore structure and the good compatibility of the COF-5 are utilized, the selectivity of the mixed matrix membrane to He is optimized, meanwhile, the two materials of COF-5 and 6FBD with different fluxes and selectivity are used, the gas separation membrane with better performance, namely the COF-5 / 6FBD mixed matrix membrane is designed, and the helium flux and the helium selectivity are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas separation membrane materials, and in particular to a COF-5 / 6FBD mixed matrix membrane and a preparation method and application thereof. Background Art

[0002] Helium is an important strategic rare gas resource, and plays an irreplaceable role in the fields of national defense, military industry, high-end medical treatment, electronic manufacturing and large scientific facilities. my country is short of helium resources, and most of the helium is imported. The existing resources are of low grade and difficult to extract. Therefore, the development of efficient and low-cost helium extraction technology is of great significance to ensure the security of my country's helium resources. Gas separation membrane technology has the advantages of high energy efficiency, low investment and simple operation, and is considered to be an effective way to achieve efficient and low-cost helium extraction. Membrane separation technology has the advantages of high efficiency, greenness and energy saving, and is recognized as a highly potential gas filtration method that can replace existing technologies. At present, mixed matrix membranes combine the advantages of polymer membranes and inorganic membranes, are widely concerned by researchers, and show good application prospects in the field of gas separation.

[0003] Mixed matrix membranes are an effective way to improve the performance of polymer membranes. The microstructure of traditional mixed matrix membranes is filled with an inorganic material, which exists in the form of micrometer or nanometer particles (discrete phase) in the polymer matrix (continuous phase), which significantly improves the gas permeation separation performance compared with pure polymer membranes. At present, there are few studies on mixed matrix membranes for helium separation, and the existing mixed matrix membranes used for helium separation have the problems of small helium flux and low helium selectivity. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a COF-5 / 6FBD mixed matrix membrane and a preparation method and application thereof, so as to at least solve the problems of small helium flux and low helium selectivity in existing mixed matrix membranes for helium separation.

[0005] The present invention solves the above technical problems by the following technical means:

[0006] In a first aspect, the present invention provides a COF-5 / 6FBD mixed matrix membrane, comprising a 6FBD polymer and COF-5 dispersed in the 6FBD polymer, wherein the amount of COF-5 is 5 wt % to 20 wt % of the 6FBD polymer.

[0007] In combination with the first aspect, in some embodiments, the amount of COF-5 used is 10 wt % of the 6FBD polymer.

[0008] In a second aspect, the present invention provides a method for preparing a COF-5 / 6FBD mixed matrix membrane, comprising the following steps:

[0009] Weigh 6FBD polymer and dissolve it in dimethylacetamide to obtain a polymer solution;

[0010] Weigh COF-5 and disperse it in dimethylacetamide, stir and disperse it by ultrasonic for the first time to obtain a COF-5 solution, wherein the amount of COF-5 is 5wt% to 20wt% of the 6FBD polymer;

[0011] The COF-5 solution and the polymer solution are mixed, stirred for the second time, and ultrasonically dispersed. The obtained mixed solution is allowed to stand for 30 to 60 minutes, poured onto a polytetrafluoroethylene plate, and coated with a scraper to a thickness of 40 to 70 μm. Subsequently, the film is dried in a forced air drying oven at 60 to 80°C for 4 to 6 hours, and then the film is scraped off the polytetrafluoroethylene plate and immersed in anhydrous methanol for 10 to 24 hours, and dried at 60 to 100°C for 4 to 8 hours to obtain a COF-5 / 6FBD mixed matrix membrane.

[0012] In conjunction with the second aspect, in some embodiments, the preparation method of the 6FBD polymer is as follows:

[0013] 2-(4-aminophenyl)-5-aminobenzimidazole and 2,4,6-trimethyl-1,3-phenylenediamine are mixed, and then N-methylpyrrolidone is added, and after dissolving under a N2 atmosphere, 6FDA is added at a temperature of 0 to 5°C, and the obtained reaction mixture is stirred at room temperature for 10 to 24 hours to obtain a polyamic acid reaction mixture;

[0014] 3-Methylpyridine and acetic anhydride are added to the polyamic acid reaction mixture and stirred for 10 to 24 hours for imidization reaction. The obtained reactant is precipitated in methanol, washed, and vacuum dried to obtain 6FBD polymer.

[0015] In combination with the second aspect, in some embodiments, the molar ratio of 6FDA, 2-(4-aminophenyl)-5-aminobenzimidazole and 2,4,6-trimethyl-1,3-phenylenediamine is 1:(0.5~1):(0.5~1), and the molar ratio of 6FDA, 3-methylpyridine and acetic anhydride is 1:1:(1~20).

[0016] In combination with the second aspect, in some embodiments, the preparation method of COF-5 is as follows: 1,4-phenylenediboronic acid, 2,3,6,7,10,11-hexahydroxytriphenylene, mesitylene and 1,4-dioxane are mixed evenly to obtain a mixture, the mixture is ultrasonically treated with an ultrasonic cell crusher for 2 to 4 hours, and then centrifuged at 6000 to 8000 rpm for 10 to 30 minutes. The separated powder is washed with acetone and vacuum dried at 60 to 80°C overnight to obtain COF-5.

[0017] In combination with the second aspect, in some embodiments, the molar ratio of 1,4-phenylenediboronic acid to 2,3,6,7,10,11-hexahydroxytriphenylene is (1.4-2.8):1, and the molar ratio of 1,4-phenylenediboronic acid, mesitylene and dioxane is 1:(1-3):1.

[0018] In combination with the second aspect, in some embodiments, the mass concentration of 6FBD polymer in the polymer solution is 0.5% to 2%, and the mass concentration of COF-5 in the COF-5 solution is 0.2% to 1%.

[0019] In combination with the second aspect, in some embodiments, the first stirring time is 1 to 5 hours, and the second stirring time is 1 to 8 hours; the ultrasonic dispersion operation is 3 to 8 times, each time for 3 to 8 minutes, and each time the ultrasonic dispersion is allowed to stand for 3 to 5 minutes before the next ultrasonic dispersion.

[0020] In a third aspect, the present invention provides the use of the COF-5 / 6FBD mixed matrix membrane described in the first aspect or the COF-5 / 6FBD mixed matrix membrane prepared by the preparation method described in the second aspect in helium separation.

[0021] The present invention utilizes the ultra-high specific surface area, unique pore structure and good compatibility of COF-5 to optimize the selectivity of the mixed matrix membrane for He. At the same time, by using two materials with different flux and selectivity, COF-5 and 6FBD, a gas separation membrane with better performance is designed, namely the COF-5 / 6FBD mixed matrix membrane, which significantly improves the helium flux and helium selectivity.

[0022] After testing, COF-5 has a fixed pore size of 2.7nm and a specific surface area of ​​up to 964.9m 2 .g -1 The gas separation test results of the COF-5 / 6FBD mixed matrix membrane of the present invention show that the maximum helium flux of the COF-5 / 6FBD mixed matrix membrane reaches 296GPU, and the He / CH4, He / N2 and He / CO2 selectivities reach 588, 572 and 391 respectively, indicating that the introduction of COF-5 greatly improves the helium mass transfer resistance and improves the helium selectivity by utilizing its own structural characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the specific surface area and pore size of COF-5 prepared in Example 2;

[0024] Figure 2 This is the thermal decomposition performance of the COF-5 / 6FBD mixed matrix membrane prepared in Example 2. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The raw materials, equipment or instruments used, if no manufacturer is specified, are all conventional products that can be purchased on the market.

[0027] The English letters in the present invention are interpreted as follows:

[0028] 6FDA: hexafluorodianhydride; DMAc: dimethylacetamide; BI: 2-(4-aminophenyl)-5-aminobenzimidazole; DAM: 2,4,6-trimethyl-1,3-phenylenediamine; NMP: N-methylpyrrolidone; BDBA: 1,4-phenylenediboronic acid; HHTP: 2,3,6,7,10,11-hexahydroxytriphenylene.

[0029] The COF-5 / 6FBD mixed matrix membrane of the present invention comprises a 6FBD polymer and COF-5 dispersed in the 6FBD polymer, wherein the amount of COF-5 is 5wt% to 20wt% of the 6FBD polymer. The present invention utilizes the ultra-high specific surface area, unique pore structure, and good compatibility of COF-5 to optimize the selectivity of the mixed matrix membrane to He, and simultaneously uses two different flux and selectivity materials, COF-5 and 6FBD, to design a gas separation membrane with better performance, thereby significantly improving the helium flux.

[0030] The preparation method of the COF-5 / 6FBD mixed matrix membrane of the present invention comprises the following steps:

[0031] (1) Synthesis of 6FBD polymer

[0032] Weigh 6FBD polymer and dissolve it in dimethylacetamide to obtain a polymer solution. The mass concentration of 6FBD polymer in the polymer solution is 0.5% to 2%.

[0033] In some embodiments, the preparation method of 6FBD polymer is as follows:

[0034] 2-(4-aminophenyl)-5-aminobenzimidazole and 2,4,6-trimethyl-1,3-phenylenediamine are mixed, and then N-methylpyrrolidone is added. After dissolving under N2 atmosphere, 6FDA is added at a temperature of 0 to 5°C, and the obtained reaction mixture is stirred at room temperature for 10 to 24 hours to obtain a polyamic acid reaction mixture; 3-methylpyridine and acetic anhydride are added to the polyamic acid reaction mixture and stirred for 10 to 24 hours to induce the imidization reaction of the polyamic acid, and the obtained reactant is precipitated in methanol, washed, and vacuum dried to obtain a 6FBD polymer. The molar ratio of 6FDA, 2-(4-aminophenyl)-5-aminobenzimidazole and 2,4,6-trimethyl-1,3-phenylenediamine is 1:(0.5 to 1):(0.5 to 1), and the molar ratio of 6FDA, 3-methylpyridine and acetic anhydride is 1:1:(1 to 20).

[0035] (2) Preparation of COF-5

[0036] Weigh COF-5 and disperse it in dimethylacetamide, stir and disperse it by ultrasonic for the first time to obtain a COF-5 solution. The mass concentration of COF-5 in the COF-5 solution is 0.2% to 1%, and the amount of COF-5 used is 5wt% to 20wt% of the 6FBD polymer.

[0037] In some embodiments, the preparation method of COF-5 is as follows: 1,4-phenylenediboronic acid, 2,3,6,7,10,11-hexahydroxytriphenylene, mesitylene and 1,4-dioxane are mixed uniformly to obtain a mixture, and the mixture is ultrasonically treated for 2 to 4 hours at a constant power of 30% and a temperature of 28°C using an ultrasonic cell crusher, and the ultrasonic treatment is conducive to promoting the uniform mixing of slightly soluble BDBA and HHTP in the mixture. Subsequently, the mixture is centrifuged at 6000 to 8000 rpm for 10 to 30 minutes, and the separated powder is washed with acetone and vacuum dried overnight at 60 to 80°C to obtain COF-5. Among them, the molar ratio of 1,4-phenylenediboronic acid to 2,3,6,7,10,11-hexahydroxytriphenylene is (1.4 to 2.8):1, and the molar ratio of 1,4-phenylenediboronic acid, mesitylene and dioxane is 1:(1 to 3):1.

[0038] (3) Preparation of mixed matrix membranes

[0039] The COF-5 solution and the polymer solution are mixed, stirred for the second time, and ultrasonically dispersed. The obtained mixed solution is allowed to stand for 30 to 60 minutes, poured onto a polytetrafluoroethylene plate, and coated with a scraper to a thickness of 40 to 70 μm. Subsequently, the film is dried in a forced air drying oven at 60 to 80°C for 4 to 6 hours, and then the film is scraped off the polytetrafluoroethylene plate and immersed in anhydrous methanol for 10 to 24 hours, and dried at 60 to 100°C for 4 to 8 hours to obtain a COF-5 / 6FBD mixed matrix membrane.

[0040] For details, please refer to Examples 1-6:

[0041] Example 1

[0042] The preparation method of the COF-5 / 6FBD mixed matrix membrane of this embodiment is as follows:

[0043] (1) Synthesis of 6FBD polymer

[0044] The synthesis of 6FBD polymer is a two-step reaction condensation. The first step is to prepare high molecular weight polyamic acid (PAA) at low temperature, add 0.01 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI), and 0.01 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) into a round-bottom flask, and then add 45 mL N-methylpyrrolidone (NMP), after dissolving under N2 atmosphere, add 0.02 mol 6FDA at low temperature 0°C, and stir the reaction mixture at room temperature for 24 hours to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 1:0.5:0.5).

[0045] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.2 mol acetic anhydride are added to the reaction mixture of the first step above, and stirred for 24 h to induce the imidization reaction of the polyamic acid to form PI. The PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0046] (2) Preparation of COF-5

[0047] 0.79 mmol 1,4-phenylenediboronic acid (BDBA), 0.56 mmol 2,3,6,7,10,11-hexahydroxytriphenylene (HHTP) were added to a beaker, 0.79 mmol mesitylene and 0.79 mmol 1,4-dioxane were mixed evenly, and then the mixture was ultrasonically treated for several hours at constant power (30%) and temperature (28°C) using an ultrasonic cell crusher. Then, the powder at the bottom of the reactor was separated by centrifugation at 8000 rpm for 10 minutes, thoroughly washed with acetone and dried at 80°C overnight, and the gray-purple solid powder finally obtained was COF-5.

[0048] (3) Preparation of mixed matrix membranes

[0049] The COF-5 / 6FBD mixed matrix membrane was prepared by conventional solution casting. 0.1 g of COF-5 was dispersed in 50 ml of DMAc, stirred for 1 h, ultrasonicated 3 times, each ultrasonication for 3 min, and each ultrasonication was completed and then the next ultrasonic dispersion was performed to make it uniformly dispersed. (The loading percentage is the mass ratio of COF-5 to 6FBD is 5 wt%). Weigh 2 g of 6FBD polymer, dissolve it in 200 ml of DMAc, and after it is completely dissolved, mix and stir it with the COFs solution for 2 h, ultrasonicated 3 times, each ultrasonication for 3 min, and each ultrasonication was completed and then the next ultrasonic dispersion was performed. Finally, the mixed solution was allowed to stand for half an hour to remove bubbles, poured on preheated polytetrafluoroethylene, scraped with a scraper to a thickness of 40-70 μm, and dried in a blast drying oven at 80 ° C for 5 h. The film was scraped off the polytetrafluoroethylene plate, immersed in anhydrous methanol for 24 h, and dried in a vacuum oven at 100 °C for 12 h to obtain a COF-5 / 6FBD mixed matrix membrane.

[0050] Example 2

[0051] The preparation method of the COF-5 / 6FBD mixed matrix membrane of this embodiment is as follows:

[0052] (1) Synthesis of 6FBD polymer

[0053] The synthesis of the polymer is a two-step reaction condensation. In the first step, high molecular weight polyamic acid (PAA) is prepared at low temperature. 0.01 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI) and 0.01 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) are added to a round-bottom flask, and then 45 mL N-methylpyrrolidone (NMP) is added. After dissolving under N2 atmosphere, 0.02 mol 6FDA is added at low temperature 0°C, and the reaction mixture is stirred at room temperature for 24 h to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 1:0.5:0.5).

[0054] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.2 mol acetic anhydride are added to the above reaction mixture and stirred for 24 h to induce the imidization reaction of polyamic acid to form PI. PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0055] (2) Preparation of COF-5

[0056] 0.79 mmol 1,4-phenylenediboronic acid (BDBA), 0.56 mmol 2,3,6,7,10,11-hexahydroxytriphenylene (HHTP) were added to a beaker, 0.79 mmol mesitylene and 0.79 mmol 1,4-dioxane were mixed evenly, and then the mixture was ultrasonically treated for several hours at constant power (30%) and temperature (28°C) using an ultrasonic cell crusher. Then, the powder at the bottom of the reactor was separated by centrifugation at 8000 rpm for 10 minutes, thoroughly washed with acetone and dried at 80°C overnight, and the gray-purple solid powder finally obtained was COF-5.

[0057] (3) Preparation of mixed matrix membranes

[0058] The COF-5 / 6FBD mixed matrix membrane was prepared by conventional solution casting. 0.2g of COF-5 was dispersed in 50ml DMAc, stirred for 1h, ultrasonicated 3 times, each ultrasonication for 3min, and each ultrasonication was allowed to stand for 3min before the next ultrasonic dispersion to make it uniformly dispersed. (The loading percentage is the mass ratio of COF-5 to 6FBD is 10wt%). 2g of 6FBD polymer was weighed and dissolved in 200ml DMAc. After complete dissolution, it was mixed and stirred with the COFs solution for 2h, ultrasonicated 3 times, each ultrasonication for 3min, and each ultrasonication was allowed to stand for 3min before the next ultrasonic dispersion. Finally, the mixed solution was allowed to stand for half an hour to remove bubbles, poured on preheated polytetrafluoroethylene, scraped with a scraper to a thickness of 40-70μm, and dried in a blast drying oven at 80°C for 5h. The film was scraped off the polytetrafluoroethylene plate, immersed in anhydrous methanol for 24 h, and dried in a vacuum oven at 100 °C for 12 h to obtain a COF-5 / 6FBD mixed matrix membrane.

[0059] Example 3

[0060] This embodiment provides a method for preparing a COF-5 / 6FBD mixed matrix membrane, the steps are as follows:

[0061] (1) Synthesis of 6FBD polymer

[0062] The synthesis of the polymer is a two-step reaction condensation. In the first step, high molecular weight polyamic acid (PAA) is prepared at low temperature. 0.01 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI) and 0.01 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) are added to a round-bottom flask, and then 45 mL N-methylpyrrolidone (NMP) is added. After dissolving under N2 atmosphere, 0.02 mol 6FDA is added at low temperature 0°C, and the reaction mixture is stirred at room temperature for 24 h to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 1:0.5:0.5).

[0063] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.2 mol acetic anhydride are added to the above reaction mixture and stirred for 24 h to induce the imidization reaction of polyamic acid to form PI. PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0064] (2) Preparation of COF-5

[0065] 0.79 mmol 1,4-phenylenediboronic acid (BDBA), 0.56 mmol 2,3,6,7,10,11-hexahydroxytriphenylene (HHTP) were added to a beaker, 0.79 mmol mesitylene and 0.79 mmol 1,4-dioxane were mixed evenly, and then the mixture was ultrasonically treated for several hours at constant power (30%) and temperature (28°C) using an ultrasonic cell crusher. Then, the powder at the bottom of the reactor was separated by centrifugation at 8000 rpm for 10 minutes, thoroughly washed with acetone and dried at 80°C overnight, and the gray-purple solid powder finally obtained was COF-5.

[0066] (3) Preparation of mixed matrix membranes

[0067] The COF-5 / 6FBD mixed matrix membrane was prepared by conventional solution casting. 0.3 g of COF-5 was dispersed in 50 ml of DMAc, stirred for 1 h, and ultrasonicated 3 times for 3 min each time to make it evenly dispersed. (The loading percentage is 15 wt% of the mass ratio of COF-5 to 6FBD). 2 g of polymer was weighed and dissolved in 200 ml of DMAc. After complete dissolution, it was mixed and stirred with the COFs solution for 2 h, ultrasonicated 3 times for 3 min each time. Finally, the mixed solution was allowed to stand for half an hour to remove bubbles, poured on preheated polytetrafluoroethylene, and scraped with a scraper to a thickness of 40-70 μm, and dried in a blast drying oven at 80 ° C for 5 h. The film was scraped off the polytetrafluoroethylene plate, soaked in anhydrous methanol for 24 h, and dried in a vacuum oven at 100 ° C for 12 h to obtain a COF-5 / 6FBD mixed matrix membrane.

[0068] Example 4

[0069] This embodiment provides a method for preparing a COF-5 / 6FBD mixed matrix membrane, the steps are as follows:

[0070] (1) Synthesis of 6FBD polymer

[0071] The synthesis of the polymer is a two-step reaction condensation. In the first step, high molecular weight polyamic acid (PAA) is prepared at low temperature. 0.01 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI) and 0.01 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) are added to a round-bottom flask, and then 45 mL N-methylpyrrolidone (NMP) is added. After dissolving under N2 atmosphere, 0.02 mol 6FDA is added at low temperature 0°C, and the reaction mixture is stirred at room temperature for 24 h to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 2:1:1).

[0072] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.2 mol acetic anhydride are added to the above reaction mixture and stirred for 24 h to induce the imidization reaction of polyamic acid to form PI. PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0073] (2) Preparation of COF-5

[0074] 0.79 mmol 1,4-phenylenediboronic acid (BDBA), 0.56 mmol 2,3,6,7,10,11-hexahydroxytriphenylene (HHTP) were added to a beaker, 0.79 mmol mesitylene and 0.79 mmol 1,4-dioxane were mixed evenly, and then the mixture was ultrasonically treated for several hours at constant power (30%) and temperature (28°C) using an ultrasonic cell crusher. Then, the powder at the bottom of the reactor was separated by centrifugation at 8000 rpm for 10 minutes, thoroughly washed with acetone and dried at 80°C overnight, and the gray-purple solid powder finally obtained was COF-5.

[0075] (3) Preparation of mixed matrix membranes

[0076] The COF-5 / 6FBD mixed matrix membrane was prepared by conventional solution casting. 0.4 g of COFs was dispersed in 50 ml DMAc, stirred for 1 h, and ultrasonicated 3 times for 3 min each time to make it evenly dispersed. (The loading percentage is 20% of the mass ratio of COF-5 to 6FBD). Weigh 2 g of 6FBD polymer, dissolve 0.5 g of 6FBD polymer in 200 ml DMAc, and after complete dissolution, mix and stir with the COFs solution for 2 h, ultrasonicate 3 times for 3 min each time. Add the remaining polymer in two batches (0.5 g and 1 g) to the above mixed solution, and repeat the stirring and ultrasonication steps three times. Finally, let the mixed solution stand for half an hour to remove bubbles, pour it on the preheated polytetrafluoroethylene, apply a scraper to a thickness of 40-70 μm, and dry it in a blast drying oven at 80 ° C for 5 h. The film was scraped off the polytetrafluoroethylene plate, immersed in anhydrous methanol for 24 h, and dried in a vacuum oven at 100 °C for 12 h to obtain a COF-5 / 6FBD mixed matrix membrane.

[0077] Example 5

[0078] The preparation method of the COF-5 / 6FBD mixed matrix membrane of this embodiment is as follows:

[0079] (1) Synthesis of 6FBD polymer

[0080] The synthesis of 6FBD polymer is a two-step reaction condensation. In the first step, high molecular weight polyamic acid (PAA) is prepared at low temperature. 0.02 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI) and 0.01 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) are added to a round-bottom flask, and then 45 mL N-methylpyrrolidone (NMP) is added. After dissolving under N2 atmosphere, 0.02 mol 6FDA is added at low temperature of 5°C, and the reaction mixture is stirred at room temperature for 10 h to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 1:1:0.5).

[0081] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.02 mol acetic anhydride are added to the reaction mixture of the first step above, and stirred for 10 h to induce the imidization reaction of the polyamic acid to form PI. The PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0082] (2) Preparation of COF-5

[0083] 1.568mmol 1,4-phenylenediboronic acid (BDBA), 0.56mmol 2,3,6,7,10,11-hexahydroxytriphenylene (HHTP) were added to a beaker, 3.136mmol mesitylene and 1.568mmol 1,4-dioxane were mixed evenly, and then the mixture was ultrasonically treated for several hours at constant power (30%) and temperature (28°C) using an ultrasonic cell crusher. Then, the powder at the bottom of the reactor was separated by centrifugation at 6000rpm for 30min, thoroughly washed with acetone and dried at 70°C overnight, and the gray-purple solid powder finally obtained was COF-5.

[0084] (3) Preparation of mixed matrix membranes

[0085] COF-5 / 6FBD mixed matrix membrane was prepared by conventional solution casting. 0.2g of COF-5 was dispersed in 50ml DMAc, stirred for 2h, ultrasonicated 4 times, each ultrasonication for 5min, and each ultrasonication was completed and then stood for 4min before the next ultrasonic dispersion to make it evenly dispersed. (The loading percentage is the mass ratio of COF-5 to 6FBD is 10wt%). 2g of 6FBD polymer was weighed and dissolved in 200ml DMAc. After complete dissolution, it was mixed and stirred with COFs solution for 1h, ultrasonicated 4 times, each ultrasonication for 5min, and each ultrasonication was completed and then stood for 4min before the next ultrasonic dispersion. Finally, the mixed solution was allowed to stand for half an hour to remove bubbles, poured on preheated polytetrafluoroethylene, scraped with a scraper to a thickness of 40-70μm, and dried in a blast drying oven at 80°C for 5h. The film was scraped off the polytetrafluoroethylene plate, immersed in anhydrous methanol for 10 h, and dried in a vacuum oven at 80 °C for 8 h to obtain a COF-5 / 6FBD mixed matrix membrane.

[0086] Example 6

[0087] The preparation method of the COF-5 / 6FBD mixed matrix membrane of this embodiment is as follows:

[0088] (1) Synthesis of 6FBD polymer

[0089] The synthesis of 6FBD polymer is a two-step reaction condensation. In the first step, high molecular weight polyamic acid (PAA) is prepared at low temperature. 0.02 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI) and 0.02 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) are added to a round-bottom flask, and then 45 mL N-methylpyrrolidone (NMP) is added. After dissolving under N2 atmosphere, 0.02 mol 6FDA is added at low temperature of 3°C, and the reaction mixture is stirred at room temperature for 20 h to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 1:1:1).

[0090] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.4 mol acetic anhydride are added to the reaction mixture of the first step above, and stirred for 20 h to induce the imidization reaction of the polyamic acid to form PI. The PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0091] (2) Preparation of COF-5

[0092] 1.12mmol 1,4-phenylenediboronic acid (BDBA), 0.56mmol 2,3,6,7,10,11-hexahydroxytriphenylene (HHTP), 3.36mmol mesitylene and 1.12mmol 1,4-dioxane were added to a beaker and mixed evenly, and then the mixture was ultrasonically treated for several hours at constant power (30%) and temperature (28°C) using an ultrasonic cell crusher. Then, the powder at the bottom of the reactor was separated by centrifugation at 7000rpm for 20min, thoroughly washed with acetone and dried at 60°C overnight, and the gray-purple solid powder finally obtained was COF-5.

[0093] (3) Preparation of mixed matrix membranes

[0094] The COF-5 / 6FBD mixed matrix membrane was prepared by conventional solution casting. 0.2g of COF-5 was dispersed in 50ml DMAc, stirred for 5h, ultrasonicated 8 times, each ultrasonication for 8min, and each ultrasonication was allowed to stand for 5min before the next ultrasonic dispersion to make it uniformly dispersed. (The loading percentage is the mass ratio of COF-5 to 6FBD is 10wt%). 2g of 6FBD polymer was weighed and dissolved in 100ml DMAc. After complete dissolution, it was mixed and stirred with the COFs solution for 5h, ultrasonicated 8 times, each ultrasonication for 8min, and each ultrasonication was allowed to stand for 5min before the next ultrasonic dispersion. Finally, the mixed solution was allowed to stand for half an hour to remove bubbles, poured on preheated polytetrafluoroethylene, scraped with a scraper to a thickness of 40-70μm, and dried in a blast drying oven at 60°C for 4h. The film was scraped off the polytetrafluoroethylene plate, immersed in anhydrous methanol for 10 h, and dried in a vacuum oven at 60 °C for 8 h to obtain a COF-5 / 6FBD mixed matrix membrane.

[0095] Comparative Example 1

[0096] This embodiment is a pure polymer film, and the preparation method of the pure polymer film is as follows:

[0097] (1) Synthesis of 6FBD polymer

[0098] The synthesis of the polymer is a two-step reaction condensation. In the first step, high molecular weight polyamic acid (PAA) is prepared at low temperature. 0.01 mol 2-(4-aminophenyl)-5-aminobenzimidazole (BI) and 0.01 mol 2,4,6-trimethyl-1,3-phenylenediamine (DAM) are added to a round-bottom flask, and then 45 mL N-methylpyrrolidone (NMP) is added. After dissolving under N2 atmosphere, 0.02 mol 6FDA is added at low temperature 0°C, and the reaction mixture is stirred at room temperature for 24 h to form the corresponding polyamic acid (the molar ratio of 6FDA to BI and DAM is 1:0.5:0.5).

[0099] The second step is cyclodehydration imidization, 0.02 mol 3-methylpyridine and 0.2 mol acetic anhydride are added to the above reaction mixture and stirred for 24 h to induce the imidization reaction of polyamic acid to form PI. PI is precipitated in methanol, washed, and then vacuum dried at 100 ° C for 24 h to obtain 6FBD polymer.

[0100] (2) Preparation of polymer films

[0101] Weigh 2g of 6FBD polymer and dissolve it in 200ml DMAc. After it is completely dissolved, let the solution stand for half an hour to remove bubbles, pour it on the preheated polytetrafluoroethylene, and use a scraper to scrape it to a thickness of 40-70μm, and dry it in a forced air drying oven at 80℃ for 5h. Scrape the film off the polytetrafluoroethylene plate, soak it in anhydrous methanol for 24h, and dry it in a vacuum oven at 100℃ for 12h to obtain a pure polymer film.

[0102] Comparative Example 2

[0103] The difference between this embodiment and embodiment 2 is that step (3) is prepared by solution casting, where COF-5 and 6FBD are simply mixed and pressed into a film, and the loading percentage is 10 wt % of the mass ratio of COF-5 to 6FBD. The other steps and conditions are the same.

[0104] Performance Test:

[0105] The COF-5 / 6FBD mixed matrix membranes prepared in Examples 1-6 and the membranes prepared in Comparative Examples 1-2 were used as samples to perform gas separation performance tests, as follows:

[0106] The COF-5 / 6FBD mixed matrix membranes prepared in Examples 1-6 and the membranes prepared in Comparative Examples 1-2 were respectively encapsulated in components, and their performances were tested under conditions of a pressure of 1 MPa and a room temperature. The test gases included CH4, CO2, He, and N2. The test results are shown in Table 1.

[0107]

[0108] Table 1

[0109] As can be seen from the data in Table 1, the helium flux and selectivity of the membrane without COF-5 are relatively poor, while the helium flux and selectivity of the COF-5 / 6FBD mixed matrix membrane are greatly improved, the maximum helium flux reaches 296GPU, and the He / CH4, He / N2 and He / CO2 selectivities reach 588, 572, and 391, respectively. Therefore, it can be explained that the introduction of COF-5 greatly improves the helium mass transfer resistance, and improves the helium selectivity by utilizing its own structural characteristics, wherein the effect prepared by adding 10wt% COF-5 is the best. Therefore, the COF-5 / 6FBD mixed matrix membrane of the present invention can be used in helium separation.

[0110] In addition, combining the data of Example 2 and Comparative Example 2 in Table 1, it can be seen that the mixing method of COF-5 and 6FBD polymers has a certain influence on the permeability of the membrane, and the COF-5 / 6FBD mixed matrix membrane prepared by solution casting has stronger permeability to helium.

[0111] The COF-5 prepared in Example 2 was used as a sample to detect its pore size and specific surface area. The test method was to activate the sample at 120°C for 4 hours and then use a Bayer adsorption instrument to test under liquid nitrogen freezing conditions to obtain the test results. The results are shown in Figure 1 .from Figure 1 It can be seen that the COF-5 of the present invention has a fixed pore size of 2.7 nm, and its specific surface area is as high as 964.9 m 2 .g -1 , which is conducive to its excellent performance in gas adsorption.

[0112] The COF-5 / 6FBD mixed matrix membrane prepared in Example 2 was used as a sample to test its heat resistance. The test was performed using a Mettler thermogravimeter at a test temperature of 30-800°C and a heating rate of 10°C / min. The test results are shown in FIG. Figure 2 . Figure 2 The data show that the COF-5 / 6FBD mixed matrix membrane prepared in the present invention has excellent heat resistance, and its heat resistance temperature is as high as 230°C.

[0113] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it should be understood by those skilled in the art that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention. The techniques, shapes, and structural parts not described in detail in the present invention are all known technologies.

Claims

1. COF-5 / 6FBD mixed matrix membrane, characterized in that The invention comprises 6FBD polymer and COF-5 dispersed in the 6FBD polymer, wherein the amount of the COF-5 is 5wt% to 20wt% of the 6FBD polymer.

2. The COF-5 / 6FBD mixed matrix membrane according to claim 1, characterized in that: The amount of COF-5 used is 10 wt % of the 6FBD polymer.

3. A method for preparing a COF-5 / 6FBD mixed matrix membrane, characterized in that: The steps include: Weigh 6FBD polymer and dissolve it in dimethylacetamide to obtain a polymer solution; Weigh COF-5 and disperse it in dimethylacetamide, stir and disperse it by ultrasonic for the first time to obtain a COF-5 solution, wherein the amount of COF-5 is 5wt% to 20wt% of the 6FBD polymer; The COF-5 solution and the polymer solution are mixed, stirred for the second time, and ultrasonically dispersed. The obtained mixed solution is allowed to stand for 30 to 60 minutes, poured onto a polytetrafluoroethylene plate, and coated with a scraper to a thickness of 40 to 70 μm. Subsequently, the film is dried in a forced air drying oven at 60 to 80°C for 4 to 6 hours, and then the film is scraped off the polytetrafluoroethylene plate and immersed in anhydrous methanol for 10 to 24 hours, and dried at 60 to 100°C for 4 to 8 hours to obtain a COF-5 / 6FBD mixed matrix membrane.

4. The method for preparing the COF-5 / 6FBD mixed matrix membrane according to claim 3, characterized in that: The preparation method of the 6FBD polymer is as follows: 2-(4-aminophenyl)-5-aminobenzimidazole and 2,4,6-trimethyl-1,3-phenylenediamine are mixed, and then N-methylpyrrolidone is added, and after dissolving under a N2 atmosphere, 6FDA is added at a temperature of 0 to 5°C, and the obtained reaction mixture is stirred at room temperature for 10 to 24 hours to obtain a polyamic acid reaction mixture; 3-Methylpyridine and acetic anhydride are added to the polyamic acid reaction mixture and stirred for 10 to 24 hours for imidization reaction. The obtained reactant is precipitated in methanol, washed, and vacuum dried to obtain 6FBD polymer.

5. The method for preparing the COF-5 / 6FBD mixed matrix membrane according to claim 4, characterized in that: The molar ratio of 6FDA, 2-(4-aminophenyl)-5-aminobenzimidazole and 2,4,6-trimethyl-1,3-phenylenediamine is 1:(0.5-1):(0.5-1), and the molar ratio of 6FDA, 3-methylpyridine and acetic anhydride is 1:1:(1-20).

6. The method for preparing the COF-5 / 6FBD mixed matrix membrane according to claim 3, characterized in that: The preparation method of the COF-5 is as follows: 1,4-phenylenediboronic acid, 2,3,6,7,10,11-hexahydroxytriphenylene, mesitylene and 1,4-dioxane are mixed uniformly to obtain a mixture, and the mixture is ultrasonically treated with an ultrasonic cell crusher for 2 to 4 hours, followed by centrifugation at 6000 to 8000 rpm for 10 to 30 minutes. The separated powder is washed with acetone and vacuum dried at 60 to 80° C. overnight to obtain COF-5.

7. The method for preparing the COF-5 / 6FBD mixed matrix membrane according to claim 6, characterized in that: The molar ratio of the 1,4-phenylenediboronic acid to 2,3,6,7,10,11-hexahydroxytriphenylene is (1.4-2.8):1, and the molar ratio of the 1,4-phenylenediboronic acid, mesitylene and dioxane is 1:(1-3):

1.

8. The method for preparing the COF-5 / 6FBD mixed matrix membrane according to claim 3, characterized in that: The mass concentration of 6FBD polymer in the polymer solution is 0.5% to 2%, and the mass concentration of COF-5 in the COF-5 solution is 0.2% to 1%.

9. The method for preparing a COF-5 / 6FBD mixed matrix membrane according to claim 3, characterized in that: The first stirring time is 1 to 5 hours, and the second stirring time is 1 to 8 hours; the ultrasonic dispersion operation is 3 to 8 times, each time for 3 to 8 minutes, and each ultrasonic dispersion is allowed to stand for 3 to 5 minutes before the next ultrasonic dispersion.

10. Use of the COF-5 / 6FBD mixed matrix membrane according to claim 1 or 2 or the COF-5 / 6FBD mixed matrix membrane prepared by the preparation method according to any one of claims 3 to 9 in helium separation.

Citation Information

Cited By

  • Covalent organic framework membrane based on regulation and control of multifunctional catalyst as well as preparation method and application of covalent organic framework membrane

    CN119838452A