Preparation method of high-flux titanium oxide ceramic nanofiltration membrane

The preparation of titanium oxide ceramic nanofiltration membranes through sol-microwave hydrothermal method solves the problems of high moisture content and large particle size in traditional methods, and achieves efficient preparation of high-quality ceramic nanofiltration membranes, with excellent separation performance and low Cost characteristics.

CN118904107APending Publication Date: 2024-11-08SUNTAR MEMBRANE TECHNOLOGY (XIAMEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964185.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

Smart Images

  • Figure CN118904107A_ABST
    Figure CN118904107A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-flux titanium oxide ceramic nanofiltration membrane, which comprises the following steps: preparing a titanium oxide film in situ by a sol-microwave hydrothermal method, and drying and calcining to directly obtain a titanium oxide nanofiltration membrane layer; a dispersing agent is added into titanium oxide sol, a titanium oxide thin film loaded on an aluminum oxide ceramic membrane supporting body is prepared in a short time through microwave hydrothermal treatment, and the defect-free, high-quality and high-flux titanium oxide nanofiltration membrane is prepared through the steps of drying and calcining.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiltration membrane preparation, and specifically relates to a method for preparing a high-flux titanium oxide ceramic nanofiltration membrane. Background Art

[0002] Ceramic nanofiltration membranes have remarkable chemical stability, thermal stability and solvent resistance, and they have excellent separation and purification capabilities for nanoscale substances in harsh chemical environments, such as high temperature, strong acid and alkali, and organic solvent systems. These characteristics provide broad prospects for the application of ceramic nanofiltration membranes in the fields of chemical industry, energy, electronics, food, and medicine.

[0003] Among the existing nanoparticle preparation technologies, including chemical precipitation, sol-gel, hydrothermal and microemulsion, the sol-gel method has become the most important method due to its advantages in preparing titanium dioxide nanoparticles in the liquid phase method. However, this method also has some limitations. The titanium dioxide nanoparticles obtained by the sol-gel method have a high water content and insufficient crystallinity. These problems lead to severe volume shrinkage during the calcination process of preparing wet ceramic nanofiltration membranes, and then multiple coatings are required to form a complete membrane layer, which undoubtedly increases the complexity and cost of the process.

[0004] In contrast, the hydrothermal method has attracted attention for its unique advantages. Generally, the hydrothermal method can directly obtain crystalline powders without high-temperature sintering, which not only saves the grinding step, but also reduces the impurities introduced thereby. The powders prepared by the hydrothermal method have the advantages of good crystallization, less agglomeration, high purity, narrow particle size distribution, and in most cases the morphology can be controlled. However, when preparing powders by the traditional hydrothermal reaction method, the particle size is large and the reaction time is long, which limits its application in the rapid preparation of ceramic nanofiltration membranes. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a high-flux titanium oxide ceramic nanofiltration membrane.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing a high-flux titanium oxide ceramic nanofiltration membrane comprises the following steps:

[0008] (1) mixing an organic titanium salt, diethanolamine and water in a molar ratio of 1:1:10-100, stirring at room temperature for 10-30 minutes, and then performing solid-liquid separation, adding water to the obtained solid and stirring it evenly, adding nitric acid, adjusting the pH to 1-2, continuing to stir for 30 minutes, and then heating and stirring at 75-85° C. for 2-4 hours to obtain a transparent titanium oxide sol;

[0009] (2) placing the titanium oxide sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 50-80%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, performing microwave hydrothermal reaction at a pressure of 0.5-2 MPa for 1-3 hours, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0010] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 80-120° C. at a humidity of 10-20%, and then heat-dried for 2-5 hours, and then heated to 350-600° C. and heat-calcined for 2-5 hours, and then cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0011] In a preferred embodiment of the present invention, the organic titanium salt is n-butyl titanate or isopropyl titanate.

[0012] More preferably, the organic titanium salt is n-butyl titanate.

[0013] In a preferred embodiment of the present invention, in step (1), the organic titanium salt, diethanolamine and water are mixed in a molar ratio of 1:1:50.

[0014] In a preferred embodiment of the present invention, in step (3): the wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 80-120°C at a rate of 1-3°C / min at a humidity of 10-20% and then kept dry for 2-5 hours.

[0015] Further preferably, in the step (3), the wet titanium oxide ceramic nanofiltration membrane obtained in the step (2) is heated to 100° C. at a rate of 1° C. / min at a humidity of 10-20%, and then kept warm and dried for 3 hours.

[0016] In a preferred embodiment of the present invention, in step (3), the temperature is raised to 350-600°C at a rate of 1-5°C / min, then kept warm and calcined for 2-5h, and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0017] Further preferably, in the step (3), the temperature is raised to 400°C at a rate of 2°C / min, then kept warm and calcined for 3 hours, and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0018] In a preferred embodiment of the present invention, the step (3) is as follows: the wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 80-120°C at a rate of 1-3°C / min at a humidity of 10-20%, and then heat-dried for 2-5 hours, and then heated to 350-600°C at a rate of 1-5°C / min, and then heat-calcined for 2-5 hours, and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0019] Further preferably, the step (3) is: heating the wet titanium oxide ceramic nanofiltration membrane obtained in step (2) to 100°C at a rate of 1°C / min at a humidity of 10-20%, and then keeping warm and drying for 3 hours, and then heating to 400°C at a rate of 2°C / min, and then keeping warm and calcining for 3 hours, and cooling to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0020] The beneficial effects of the present invention are:

[0021] 1. The present invention adopts the sol-microwave hydrothermal method, prepares nanoparticles with smaller particle size in the sol, and uses microwave hydrothermal technology to quickly heat up, accelerates the reaction rate, and significantly shortens the reaction time. Compared with the traditional sol-gel method and hydrothermal method, the present invention can directly load nanoparticles with fine grains, uniform particle size, and complete crystal development on the ceramic membrane support. After drying and calcination steps, high-quality titanium oxide ceramic nanofiltration membranes are successfully prepared.

[0022] 2. The present invention adds a dispersant to the titanium oxide sol, so that the nanoparticles are more evenly dispersed during the microwave hydrothermal process, avoiding agglomeration, thereby forming a uniform, defect-free titanium oxide film on the alumina ceramic membrane support. After the titanium oxide film is dried and calcined, a titanium oxide nanofiltration membrane with excellent separation performance can be prepared.

[0023] 3. Compared with the traditional sol-gel method, the present invention avoids the problems of high water content and low crystallinity, reduces the volume shrinkage during calcination, and thus forms a complete film layer without multiple coatings.

[0024] 4. Compared with the hydrothermal method, the present invention greatly shortens the reaction time while maintaining the high crystallinity and narrow particle size distribution of the powder, and the particle size is smaller, making it easier to form a uniform film layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope photograph of the high-flux titanium oxide ceramic nanofiltration membrane prepared in Example 1 of the present invention.

[0026] Figure 2 This is a scanning electron microscope photograph of the comparative titanium oxide ceramic nanofiltration membrane prepared in Comparative Example 1 of the present invention.

[0027] Figure 3 This is a scanning electron microscope photograph of the comparative titanium oxide ceramic nanofiltration membrane prepared in Comparative Example 2 of the present invention.

[0028] Figure 4 This is a scanning electron microscope photograph of the comparative titanium oxide ceramic nanofiltration membrane prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0030] Example 1

[0031] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, and then nitric acid solution was added to adjust the pH to 1.5. The mixture was stirred for 30 minutes and then heated and stirred at 80° C. for 3 hours to obtain a transparent titanium oxide sol.

[0032] (2) placing the titanium oxide sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, and performing microwave hydrothermal reaction at a pressure of 0.5 MPa for 2 hours, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0033] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0034] The high flux titanium oxide ceramic nanofiltration membrane has a complete membrane layer (such as Figure 1 As shown), under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 96% and the flux is 70 LHM.

[0035] Example 2

[0036] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, and then nitric acid solution was added to adjust the pH to 1.5. The mixture was stirred for 30 minutes and then heated and stirred at 80° C. for 3 hours to obtain a transparent titanium oxide sol.

[0037] (2) placing the titanium oxide sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, performing microwave hydrothermal reaction for 2 hours at a pressure of 1 MPa, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0038] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0039] Under the test conditions of room temperature and 0.69 MPa, the high-flux titanium oxide ceramic nanofiltration membrane has a retention rate of 92% and a flux of 74 LHM for a 0.1% PEG1000 solution.

[0040] Example 3

[0041] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, and then nitric acid solution was added to adjust the pH to 1.5. The mixture was stirred for 30 minutes and then heated and stirred at 80° C. for 3 hours to obtain a transparent titanium oxide sol.

[0042] (2) placing the titanium oxide sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 60%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, performing microwave hydrothermal reaction for 2 hours at a pressure of 2 MPa, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0043] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

[0044] Under the test conditions of room temperature and 0.69 MPa, the high-flux titanium oxide ceramic nanofiltration membrane has a retention rate of 90% and a flux of 80 LHM for a 0.1% PEG1000 solution.

[0045] Comparative Example 1

[0046] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, and then nitric acid solution was added to adjust the pH to 1.5. The mixture was stirred for 30 minutes and then heated and stirred at 80° C. for 3 hours to obtain a transparent titanium oxide sol.

[0047] (2) Titanium oxide sol was dip-coated onto a porous alumina ceramic membrane support with an average pore size of 5 nm. The temperature was raised to 100°C at a rate of 1°C / min at a humidity of 10-20%, and the mixture was kept warm and dried for 2-5 hours. The temperature was then raised to 400°C at a rate of 2°C / min, and the mixture was kept warm and calcined for 3 hours. The mixture was cooled to obtain a comparative ceramic nanofiltration membrane.

[0048] The ceramic nanofiltration membrane is prone to cracks (such as Figure 2 As shown), under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 0 and the flux is 110 LHM.

[0049] Comparative Example 2

[0050] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, and then nitric acid solution was added to adjust the pH to 1.5. The mixture was stirred for 30 minutes and then heated and stirred at 80° C. for 3 hours to obtain a transparent titanium oxide sol.

[0051] (2) placing the titanium oxide sol obtained in step (1) into a hydrothermal reactor with a filling degree of 60%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, and reacting at 200° C. for 3 h, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0052] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a comparative ceramic nanofiltration membrane.

[0053] The ceramic nanofiltration membrane is prone to microcracks (such as Figure 3 As shown), under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 15% and the flux is 88 LHM.

[0054] Comparative Example 3

[0055] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, and then nitric acid solution was added to adjust the pH to 1.5. The mixture was stirred for 30 minutes and then heated and stirred at 80° C. for 3 hours to obtain a transparent titanium oxide sol.

[0056] (2) placing the titanium oxide sol obtained in step (1) into a hydrothermal reactor with a filling degree of 60%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, reacting at 200° C. for 10 hours, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane;

[0057] (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and dried for 3 hours. Then, the temperature is raised to 400°C at a rate of 2°C / min, and calcined for 3 hours. The membrane is cooled to obtain a comparative ceramic nanofiltration membrane.

[0058] The membrane layer of the comparative ceramic nanofiltration membrane is intact (eg Figure 4 As shown), under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 82% and the flux is 58 LHM.

[0059] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing a high-flux titanium oxide ceramic nanofiltration membrane, Features: The steps include: (1) mixing an organic titanium salt, diethanolamine and water in a molar ratio of 1:1:10-100, stirring at room temperature for 10-30 minutes, and then performing solid-liquid separation, adding water to the obtained solid and stirring it evenly, adding nitric acid, adjusting the pH to 1-2, continuing to stir for 30 minutes, and then heating and stirring at 75-85° C. for 2-4 hours to obtain a transparent titanium oxide sol; (2) placing the titanium oxide sol obtained in step (1) into a microwave hydrothermal reaction device with a filling degree of 50-80%, and then immersing the ceramic membrane support in the titanium oxide sol in the microwave hydrothermal reaction device, performing microwave hydrothermal reaction at a pressure of 0.5-2 MPa for 1-3 hours, and cooling to obtain a wet titanium oxide ceramic nanofiltration membrane; (3) The wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 80-120° C. at a humidity of 10-20%, and then heat-dried for 2-5 hours, and then heated to 350-600° C. and heat-calcined for 2-5 hours, and then cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

2. The preparation method according to claim 1, Features: The organic titanium salt is n-butyl titanate or isopropyl titanate.

3. The preparation method according to claim 2, Features: The organic titanium salt is n-butyl titanate.

4. The preparation method according to any one of claims 1 to 3, Features: In the step (1), the organic titanium salt, diethanolamine and water are mixed in a molar ratio of 1:1:

50.

5. The preparation method according to claim 1, Features: In the step (3), the wet titanium oxide ceramic nanofiltration membrane obtained in the step (2) is heated to 80-120° C. at a rate of 1-3° C. / min at a humidity of 10-20%, and then kept warm and dried for 2-5 hours.

6. The preparation method according to claim 5, Features: In the step (3), the wet titanium oxide ceramic nanofiltration membrane obtained in the step (2) is heated to 100° C. at a rate of 1° C. / min at a humidity of 10-20%, and then kept warm and dried for 3 hours.

7. The preparation method according to claim 1, Features: In the step (3), the temperature is raised to 350-600° C. at a rate of 1-5° C. / min, then kept warm and calcined for 2-5 hours, and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

8. The preparation method according to claim 7, Features: In the step (3), the temperature is raised to 400° C. at a rate of 2° C. / min, then kept at that temperature for 3 hours and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

9. The preparation method according to claim 1, Features: The step (3) is as follows: the wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 80-120°C at a rate of 1-3°C / min at a humidity of 10-20%, and then heat-dried for 2-5 hours, and then heated to 350-600°C at a rate of 1-5°C / min, and then heat-calcined for 2-5 hours, and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.

10. The preparation method according to claim 9, Features: The step (3) is as follows: the wet titanium oxide ceramic nanofiltration membrane obtained in step (2) is heated to 100°C at a rate of 1°C / min at a humidity of 10-20%, and then heat-dried for 3 hours, and then heated to 400°C at a rate of 2°C / min, and then heat-calcined for 3 hours, and cooled to obtain a high-flux titanium oxide ceramic nanofiltration membrane.