Preparation method of reverse osmosis membrane based on plasma polymerization, reverse osmosis membrane and application
Through plasma polymerization process and oxidation protection modification treatment, the safety hazards of flammable and explosive solvents in the production process and the problem of insufficient chlorine resistance of reverse osmosis membranes are solved, and higher membrane performance and environmentally friendly reverse osmosis are achieved. Film preparation.
Patent Information
- Application Number
- CN202411342587.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The existing reverse osmosis membranes use flammable and explosive organic solvents during the production process, resulting in safety hazards and environmental pollution. At the same time, they have poor chlorine resistance, which affects the service life and performance of the membrane.
The reverse osmosis membrane is prepared by a plasma polymerization process. Through multi-stage plasma polymerization and oxidation protection modification treatment, the requirements for the substrate are reduced, the use of flammable and explosive solvents are avoided, and the chlorine resistance of the membrane is improved.
It improves the chlorine resistance and stability of the film, reduces production costs and environmental protection impact, expands the selection range of substrates, and enhances the commercial value of the film.
Smart Images

Figure BDA0005060120030000161 
Figure BDA0005060120030000171
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of reverse osmosis membrane preparation, and in particular to a reverse osmosis membrane preparation method based on plasma polymerization, a reverse osmosis membrane and applications. Background Art
[0002] Reverse osmosis membrane separation technology has become one of the most effective water treatment methods in the world due to its good separation performance for inorganic salt ions. It plays an increasingly important role in the fields of household water purification, industrial water treatment, municipal sewage treatment, seawater desalination, zero discharge and separation and concentration. Conventional reverse osmosis membranes are composed of three layers of materials, namely the bottom layer of non-woven fabric, the middle layer of polysulfone and the upper layer of polymer desalination layer. The desalination layer, as the core functional material, plays the role of separating salt and water.
[0003] At present, almost all reverse osmosis membranes on the market are asymmetric reverse osmosis membranes, which require specific wet non-woven fabrics and casting processes. The base membrane material selection required for interfacial polymerization is high, especially the flatness and uniformity of non-woven fabrics. Only the wet process can meet the requirements for reverse osmosis membranes. However, the membrane using plasma polymerization technology has greatly reduced requirements for the base material, and even without casting, it is possible to directly polymerize on PP or PE film to prepare reverse osmosis membranes, and there are more choices in base materials.
[0004] Since conventional reverse osmosis membranes are prepared by interfacial polymerization, the base membrane is first passed through or coated with an aqueous phase, and then coated with an oil phase to form a polymer desalting layer through an interfacial polycondensation reaction. In this technology, an organic phase must be used as a solvent to dissolve the acyl chloride monomer. Commonly used substances include Isopar E / G / H / L, n-hexane, n-decane and other substances. These substances are flammable and explosive. At the same time, when the organic phase on the surface of the membrane is dried in an oven, a large amount of high-VOC concentration gas will be generated, which must be treated with RTO and meet the standards before it can be discharged. On the one hand, the use of flammable and explosive organic phases puts higher requirements on the safety control of production, and it also needs to be equipped with exhaust gas post-treatment equipment, which will increase the investment cost of the production line. Otherwise, it will pollute the environment. The use of plasma polymerization can completely avoid such problems.
[0005] On the other hand, the reverse osmosis membrane material prepared by interfacial polymerization has benzene rings connected by amide bonds. Aromatic polyamides are highly sensitive to active chlorine. When exposed to active chlorine for a long time, hypochlorite will first replace the hydrogen atoms on the amide bonds with chlorine atoms, destroying the hydrogen bonds between the polymer chains. Subsequently, the Orton rearrangement reaction will occur, causing the amide bonds in the desalination layer of the reverse osmosis membrane to break. The polyamide layer of the reverse osmosis membrane will change from a regular crystalline state to an amorphous state, the free volume of the polymer membrane will increase, the membrane will become loose, and the retention rate will decrease. This is also one of the main usage problems currently faced by commercial reverse osmosis membranes.
[0006] Therefore, in view of the high requirements of existing membrane materials on the substrate, the interfacial polymerization process must be used for preparation, and the prepared membrane has poor chlorine resistance and has high requirements on production and environmental protection issues. This patent proposes a new plasma polymerization method for preparing reverse osmosis, which has better market advantages than membranes prepared using the interfacial polymerization process.
[0007] At present, the application of plasma polymerization technology to prepare reverse osmosis membranes is more focused on using the gases of monomer components as polymerization materials, or conducting discharge polymerization in an inert gas, resulting in the overall performance of membranes prepared by this process being less than ideal. Summary of the invention
[0008] In order to solve at least one of the above technical problems, a method for preparing a reverse osmosis membrane based on plasma polymerization is developed. The present application provides a method for preparing a reverse osmosis membrane based on plasma polymerization, a reverse osmosis membrane and applications.
[0009] On the one hand, the present application provides a method for preparing a reverse osmosis membrane based on plasma polymerization, comprising the following steps:
[0010] S1, treating the reverse osmosis membrane base film with an aqueous solution to remove excess aqueous solution from the reverse osmosis membrane base film surface, and introducing a first polymerization chamber gas into the first polymerization chamber under the first polymerization chamber atmosphere to perform a first step of plasma polymerization;
[0011] S2. During the polymerization process, after 2 to 9 minutes of polymerization deposition, the back of the base film is attached to a back plate with a heating function, the heating temperature is 40 to 70° C., and plasma polymerization is continued. After 2 to 8 minutes, the polymerization is stopped and the film is placed in an oven to dry the moisture inside the film;
[0012] S3, placing the film treated by S2 in a second polymerization chamber, introducing the second polymerization chamber gas under the atmosphere of the second polymerization chamber to carry out second step plasma polymerization; after a period of reaction, introducing the second polymerization chamber supplementary gas to continue the second step plasma polymerization;
[0013] S4, subjecting the membrane sheet treated in S3 to oxidation protection modification treatment, and then immersing it in a mixed solution containing sodium bisulfite and glycerol, taking it out after immersion, and drying it to obtain a reverse osmosis membrane.
[0014] Optionally, the reverse osmosis membrane base film is surface treated in the water phase for 5 to 40 seconds;
[0015] And / or, the aqueous phase is obtained by mixing component a, component b, sodium lauryl sulfate and water in a weight ratio of 0.25-4.5:0.5-5:0.05-0.75:95-99;
[0016] And / or, the component a is at least one of sodium bicarbonate, sodium bisulfite, ammonium chloride, sodium carbonate, calcium bicarbonate, and potassium carbonate;
[0017] And / or, component b is at least one of sodium camphorsulfonate, sodium sulfite, sodium lactate, sodium citrate, sodium dihydrogen phosphate, sodium phosphate, and triethylamine hydrochloride.
[0018] Optionally, the first step of plasma polymerization is dielectric barrier discharge, bias voltage is 150V, flow rate of each monomer is 1-8mg / s, gas pressure value of polymerization chamber is set to 50-500pa, plasma polymerization power is 20-120W, plasma polymerization electrode spacing is 13-30mm, and polymerization chamber temperature is 25°C-45°C.
[0019] Optionally, the first polymerization chamber atmosphere is: a gas atmosphere having at least one of argon, helium, oxygen, nitrogen, carbon dioxide, water vapor, sulfur hexafluoride, and ammonia;
[0020] And / or, the first polymerization chamber gas is at least two of triethylamine, ethylenediamine, propylenediamine, butylenediamine, 1,3-dimethylbutylamine, di-n-butylamine, n-propylamine, isopropylamine, diisopropylamine, 2-allylamine, 3-aminopropylene, 3-butene-1-amine, 3-butene-2-amine, and 2-butene-1-amine.
[0021] Optionally, the atmosphere of the second polymerization chamber is: a gas atmosphere having at least one of argon, helium, oxygen, nitrogen, carbon dioxide, nitric oxide, and nitrogen dioxide;
[0022] And / or, the second polymerization chamber gas is at least two of: aniline, benzylamine, phenylethylamine, styrene, benzyl alcohol, toluidine, ethylaniline, N,N-dimethylaniline, m-xylylenediamine, p-xylylenediamine, and 4-vinylpyridine;
[0023] And / or, the second polymerization chamber supplementary gas is at least one of acrylic acid, hydroxyethyl acrylate, methyl crotonate, propionic acid, butyric acid, methyl acrylate, allyl alcohol, and butenol.
[0024] Optionally, the second step plasma polymerization is dielectric barrier discharge, bias voltage is 150V, each monomer flow rate is 2-9mg / s, and the polymerization chamber is at normal pressure. The plasma polymerization power is 30-150W, the plasma polymerization electrode spacing is 10-40mm, the polymerization time is 4-18min, the polymerization time of the supplementary gas introduced into the second polymerization chamber is 4-12min, and the polymerization chamber temperature is 25-45°C.
[0025] Optionally, the oxidation protection modification treatment is to immerse the membrane in an oxidation protection modification solution, wherein the oxidation protection modification solution is composed of a mixture of component c, component d and component e in a weight ratio of 0.35-1.85:1.5-4.5:0.25-1.25:92-98;
[0026] And / or, the component c is at least one of selenium dioxide, sodium periodate, Dess-Martin periodinane, iodosobenzene, sodium chlorite, diacetoxyiodobenzene, and bis(trifluoroacetoxyiodobenzene);
[0027] and / or, the component d is at least one of 2-methyl-2-butene, 3-methyl-1-butene, 2-methyl-1-butene, 1-pentene, 2-pentene, cyclopentene, and 1,3-butadiene;
[0028] And / or, the component e is at least one of sodium dihydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate, potassium phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate;
[0029] And / or, the pH of the oxidation protection modification solution is 3-7, the temperature is 30±2° C., and the membrane is immersed in the oxidation modification solution for 0.5 to 5 minutes.
[0030] Optionally, in the mixed solution, the mass fraction of sodium bisulfite is 0.3%, the mass fraction of glycerol is 8%, the temperature is 25±2° C., and the time for the membrane to be immersed in the sodium bisulfite solution is 0.5 to 3 minutes.
[0031] In a second aspect, the present application provides a reverse osmosis membrane prepared by the above-mentioned preparation method.
[0032] In a third aspect, the present application provides the application of the above-mentioned reverse osmosis membrane in the field of water treatment.
[0033] In summary, the present application includes at least one of the following beneficial technical effects:
[0034] 1. The reverse osmosis composite membrane is directly prepared by plasma polymerization process. In order to change the problem of poor desalination performance of the reverse osmosis membrane prepared by conventional plasma polymerization, the present invention polymerizes multiple monomers and controls the type of polymerization monomers and the degree of reaction at different stages. The staged plasma polymerization and secondary plasma polymerization process are used to make the performance of the reverse osmosis membrane more commercially valuable. The process described in the patent of the present invention is operable for various types of reverse osmosis substrates.
[0035] 2. The present invention uses a desalination layer morphology shaping process while performing plasma polymerization. The desalination layer of conventional membrane products using plasma polymerization is a relatively smooth or rough layer. When the salt retention rate of the desalination layer is high enough, it is not conducive to the improvement of the overall flux. According to the method provided by the present invention, while performing plasma polymerization deposition in the first stage, the morphology of the desalination layer can be shaped by decomposing the salt components in the base membrane, so that the surface of the desalination layer has a vesicle or spine structure, which increases the specific surface area of water passing through the desalination layer of the reverse osmosis membrane, and maintains the membrane desalination rate while having a higher flux;
[0036] 3. In order to solve the problem of unstable performance of membranes and fluctuation of batch performance in plasma polymerization process, the present invention performs modification in the post-treatment oxidation modification tank, removes the phenomenon of unstable performance of membranes caused by free radicals remaining in the desalination layer or substrate, and makes the performance of membranes in plasma polymerization process reach a stable state in advance;
[0037] 4. The plasma polymerization process provided by the present invention changes the current state of reverse osmosis membrane materials being mainly polyamide, making the selectivity and functionality of reverse osmosis membrane materials more diversified. The developed reverse osmosis membrane is stronger than the chemical bonds formed by interfacial polymerization because the chemical bonds are formed by free radical polymerization under ionization. The overall performance of the membrane material is changed, and the chlorine resistance is better than that of the traditional polyamide reverse osmosis membrane. It also provides a new way to develop better chlorine-resistant reverse osmosis membranes. DETAILED DESCRIPTION
[0038] The present application is further described in detail below with reference to the embodiments.
[0039] The present application designs a method for preparing a reverse osmosis membrane. Different from the commonly used interfacial polymerization process in the prior art, the present application prepares the reverse osmosis membrane through a plasma polymerization process;
[0040] The specific steps include:
[0041] S1, treating the reverse osmosis membrane base film with water phase to remove excess water phase droplets on the reverse osmosis membrane base film surface, and introducing the first polymerization chamber gas into the first polymerization chamber under the first polymerization chamber atmosphere to perform the first step of plasma polymerization;
[0042] S2. During the polymerization process, after 2 to 9 minutes of polymerization deposition, the back of the base film is attached to a back plate with a heating function, the heating temperature is 40 to 70° C., and plasma polymerization is continued. After 2 to 8 minutes, the polymerization is stopped and the film is placed in an oven to dry the moisture inside the film;
[0043] S3, placing the film treated by S2 in a second polymerization chamber, introducing the second polymerization chamber gas under the atmosphere of the second polymerization chamber to carry out second step plasma polymerization; after a period of reaction, adding the second polymerization chamber supplementary gas, and continuing the second step plasma polymerization;
[0044] S4, subjecting the membrane sheet treated in S3 to oxidation protection modification treatment, and then immersing it in a mixed solution containing sodium bisulfite and glycerol, taking it out after immersion, and drying it to obtain a reverse osmosis membrane.
[0045] The present application also provides a reverse osmosis membrane prepared by the above preparation method, and the application of the reverse osmosis membrane in the field of water treatment.
[0046] When designing the technical solution of the present application for preparing a reverse osmosis membrane through a plasma polymerization process, the inventors adopted the idea of gradually constructing a desalination layer. First, the "skeleton" of the desalination layer is shaped on the surface of the substrate through preliminary plasma polymerization, and at the same time, the substrate is heated by a back plate, and the morphology of the desalination layer is shaped by the release of gas during the reaction.
[0047] The second step is plasma polymerization, which modifies and improves the desalination layer formed in the first step of plasma polymerization to ensure the integrity of the membrane desalination layer.
[0048] The hydrophilicity of the membrane surface is changed by adding supplementary gas into the second polymerization chamber to carry out polymerization.
[0049] Finally, the oxidation modification protection process is used to convert the residual free radicals and other unreacted groups in advance to stabilize the performance of the membrane.
[0050] The above reverse osmosis membrane preparation process of the present application is operable for base membranes made of PP, PE, PSF (PSU), PTFE, PVC, PPS and other materials. Single-layer hydrophobic substrates such as PP and PE require corona treatment to ensure the effect, but reverse osmosis membranes that meet the requirements can be produced.
[0051] Compared with the conventional method of preparing reverse osmosis membrane by interfacial polymerization, the present invention directly and only uses the plasma polymerization process, and gradually shapes the desalination layer through different stages of plasma polymerization, providing a new preparation process for reverse osmosis membrane, expanding the range of options for reverse osmosis substrates, not only limited to traditional polysulfone ultrafiltration membranes, and greatly simplifying the reverse osmosis membrane coating process. It solves the safety and environmental protection issues of the need to dry flammable and explosive organic solvents at high temperatures during the production of reverse osmosis membranes;
[0052] The plasma polymerization process for preparing reverse osmosis membranes is more advantageous than interfacial polymerization products in terms of overall performance stability. This is because interfacial polymerization requires substances such as m-phenylenediamine. If the amino functional groups are not cleaned thoroughly, it will easily lead to color differences on the membrane surface during storage, which will also affect the performance of the membrane. Plasma polymerization membranes can completely avoid such problems because they do not contain m-phenylenediamine substances.
[0053] The present invention can also greatly reduce the energy consumption of the production line by preparing the reverse osmosis membrane by plasma polymerization, and the overall performance can be controlled by controlling the conditions of the polymerization chamber. The requirements for manufacturing equipment and auxiliary equipment are also lower than those for interfacial polymerization equipment.
[0054] In the following embodiments of the present application, polysulfone (PSF) is used as the reverse osmosis membrane base membrane.
[0055] In the following examples of the present application, unless otherwise specified, the main components involved were purchased from commercially available products.
[0056] Preparation of reverse osmosis membrane base membrane in the embodiment:
[0057] After heating N,N-dimethylformamide to 70° C., polysulfone is added and stirred for more than 12 hours to obtain a casting solution; the casting solution contains 15.5% polysulfone and 84.5% solvent. Specific embodiments
[0059] Example 1
[0060] Prepare aqueous solution:
[0061] Sodium bicarbonate, triethylamine hydrochloride, sodium dodecyl sulfate and pure water were prepared into an aqueous phase solution in a mass ratio of 0.95:2:0.15:96.9.
[0062] Preparation of oxidation modification protection solution:
[0063] Sodium chlorite, 2-methyl-2-butene, sodium dihydrogen phosphate and pure water were prepared into an oxidation modification protection solution in a mass ratio of 0.85:2:0.35:96.8, with a temperature of 30±2 degrees and a pH of 4.5.
[0064] Prepare sodium bisulfite solution:
[0065] A mixed solution with a mass fraction of 0.3% sodium bisulfite and a mass fraction of 8% glycerol was prepared using 25°C pure water.
[0066] Preparation of reverse osmosis membrane:
[0067] The reverse osmosis membrane base film was immersed in the aqueous solution for 25 seconds, and the excess aqueous solution on the surface and the back of the membrane was removed with an air knife, and then the membrane was placed on the heating plate in the first polymerization chamber.
[0068] Argon gas was introduced into the first polymerization chamber, and the gas pressure was set to 150 Pa, the discharge power to 80 W, the bias voltage to 150 V, the electrode spacing to 20 mm, and the polymerization chamber temperature to 30°C.
[0069] 1,3-dimethylbutylamine was vaporized at 140°C in a vaporization chamber, and the monomer flow rate was set to 4 mg / s. 3-Butene-1-amine was vaporized at 90°C in a vaporization chamber, and the monomer flow rate was set to 3 mg / s. 1,3-dimethylbutylamine and 3-butene-1-amine gases were mixed for 20 seconds and then plasma polymerization was performed.
[0070] After 6 minutes of polymerization deposition, the back of the film was attached to a back plate heated at 45°C, and the discharge power was reduced to 70W. The plasma polymerization was continued for 8 minutes and then the reaction was stopped.
[0071] The film was dried in an oven at 70°C for 2 min to remove excess moisture from the base film.
[0072] Helium gas at normal pressure was introduced into the second polymerization chamber, the discharge power was 90 W, the bias voltage was 150 V, the electrode spacing was 35 mm, and the polymerization chamber temperature was 35°C.
[0073] Meta-xylylenediamine was vaporized at 270°C in the vaporization chamber, and the monomer flow rate was set to 5 mg / s. Styrene was vaporized at 180°C in the vaporization chamber, and the monomer flow rate was set to 3 mg / s. Hydroxyethyl acrylate was vaporized at 240°C in the vaporization chamber, and the monomer flow rate was set to 4 mg / s.
[0074] The membrane was placed in the second polymerization chamber, and vaporized m-xylylenediamine and styrene were introduced and mixed for 20 seconds before the second step of plasma polymerization. After polymerization deposition for 12 minutes, vaporized hydroxyethyl acrylate was introduced to continue polymerization for 10 minutes.
[0075] Immerse the membrane in the oxidation modification protection solution for 3 minutes, take it out and use an air knife to remove excess water droplets on the surface.
[0076] The membrane was immersed in a sodium bisulfite glycerol mixed solution for 1 min, taken out and the water droplets on the surface were removed with an air knife, and dried in an oven at 70°C for 2 min to obtain a finished reverse osmosis membrane.
[0077] Example 2
[0078] The difference between this embodiment and embodiment 1 is that the aqueous phase solution is prepared in this embodiment:
[0079] Sodium bicarbonate, triethylamine hydrochloride, sodium dodecyl sulfate and pure water were prepared into an aqueous phase solution in a mass ratio of 0.25:2:0.15:97.6.
[0080] Example 3
[0081] The difference between this embodiment and embodiment 1 is that the aqueous phase solution is prepared in this embodiment:
[0082] Sodium bicarbonate, triethylamine hydrochloride, sodium dodecyl sulfate and pure water were prepared into an aqueous phase solution in a mass ratio of 0.95:0.5:0.15:98.4.
[0083] Example 4
[0084] The difference between this embodiment and embodiment 1 is that the atmosphere of the first polymerization chamber of this embodiment is a carbon dioxide gas atmosphere.
[0085] Example 5
[0086] The difference between this embodiment and embodiment 1 is that the gas in the first polymerization chamber of this embodiment is gasified triethylamine and diisopropylamine.
[0087] Example 6
[0088] The difference between this embodiment and embodiment 1 is that in this embodiment, after the polymerization deposition for 4 minutes, the back of the film is attached to a back plate heated at 45°C.
[0089] Example 7
[0090] The difference between this embodiment and embodiment 1 is that:
[0091] The back of the film was attached to a back plate heated to 45°C, and the discharge power was increased to 100W.
[0092] Example 8
[0093] The difference between this embodiment and embodiment 1 is that in this embodiment, the atmosphere of the second polymerization chamber is a nitrogen dioxide gas atmosphere.
[0094] Example 9
[0095] The difference between this embodiment and embodiment 1 is that in this embodiment, the gas in the second polymerization chamber is gasified aniline and p-phenylenediamine.
[0096] Example 10
[0097] The difference between this embodiment and embodiment 1 is that in this embodiment, the supplementary gas in the second polymerization chamber is gasified butyric acid.
[0098] Embodiment 11
[0099] The difference between this embodiment and embodiment 1 is that: in this embodiment,
[0100] After the vaporized m-xylylenediamine and styrene were introduced and mixed for 20 seconds, the second step of plasma polymerization was carried out. After the polymerization deposition for 18 minutes, the vaporized hydroxyethyl acrylate was introduced to continue the polymerization.
[0101] Example 12
[0102] The difference between this embodiment and embodiment 1 is that in this embodiment, vaporized hydroxyethyl acrylate is introduced to continue polymerization, and the polymerization time is 5 minutes.
[0103] Embodiment 13
[0104] The difference between this embodiment and embodiment 1 is that in this embodiment, the oxidation modification protection liquid component used is iodobenzoylbenzene, 2-methyl-2-butene, sodium dihydrogen phosphate and pure water mixed in a mass ratio of 0.85:2:0.35:96.8.
[0105] Embodiment 14
[0106] The difference between this embodiment and embodiment 1 is that in this embodiment, the membrane is immersed in the oxidation modification protection solution for 0.5 min.
[0107] Comparative Example 1
[0108] The difference between this comparative example and Example 1 is that this comparative example adopts the interfacial polymerization method in the prior art to prepare the reverse osmosis membrane; the details are as follows:
[0109] Prepare aqueous solution:
[0110] Metaphenylenediamine, triethylamine hydrochloride and pure water were prepared into an aqueous phase solution in a mass ratio of 2:2:96.
[0111] Prepare oil phase solution:
[0112] Trimesoyl chloride, tributyl phosphate and n-hexane were prepared into an oil phase solution in a mass ratio of 0.15:0.35:99.5.
[0113] Prepare sodium carbonate solution:
[0114] Prepare a 0.3% sodium carbonate solution.
[0115] Prepare sodium bisulfite solution:
[0116] Prepare a 0.3% sodium bisulfite solution.
[0117] Adopting interfacial polymerization process, the reverse osmosis base membrane is first passed through the above-prepared aqueous phase solution for 30 seconds, and after removing excess water droplets on the surface with a roller and an air knife, the above-prepared oil phase solution is coated on the base membrane, and after reacting for 30 seconds, the excess oil phase on the membrane surface is poured out or removed, and the oil phase on the membrane surface and the water inside are dried in an oven at 100°C;
[0118] The membrane was immersed in 0.3% sodium carbonate solution for 30 seconds, then rinsed with pure water, and then soaked in 70°C pure water for 3 minutes. The membrane was taken out and soaked in 0.3% sodium bisulfite solution for 30 seconds, and then dried in an oven at 70°C to obtain a finished reverse osmosis membrane.
[0119] Comparative Example 2
[0120] The difference between this comparative example and Example 1 is that in this comparative example, the aqueous phase solution does not contain sodium bicarbonate.
[0121] Comparative Example 3
[0122] The difference between this comparative example and Example 1 is that in this comparative example, the aqueous phase solution does not contain triethylamine hydrochloride.
[0123] Comparative Example 4
[0124] The difference between this comparative example and Example 1 is that in this comparative example, the first polymerization chamber gas is 3-butene-1-amine gas.
[0125] Comparative Example 5
[0126] The difference between this comparative example and Example 1 is that in this comparative example, no back plate heating film is used.
[0127] Comparative Example 6
[0128] The difference between this comparative example and Example 1 is that in this comparative example, single m-xylylenediamine is used for plasma polymerization without introducing styrene.
[0129] Comparative Example 7
[0130] The difference between this comparative example and Example 1 is that in this comparative example, only m-xylylenediamine is used for plasma polymerization, and hydroxyethyl acrylate is no longer introduced.
[0131] Comparative Example 8
[0132] The difference between this comparative example and Example 1 is that in this comparative example, there is no 2-methyl-2-butene in the components of the oxidative modification protection solution.
[0133] The finished reverse osmosis membranes prepared in the above Examples 1 to 14 and Comparative Examples 1 to 8 were subjected to membrane performance testing: the performance data measured under the conditions of 500 ppm NaCl as the test solution, 25° C., pH=7-8, and an applied pressure of 72.5 psi are shown in Table 1.
[0134] Table 1
[0135] Reverse Osmosis Membrane Differences from Example 1 Membrane flux / LMH Membrane desalination / % Example 1 / 43.35 99.20 Example 2 Sodium bicarbonate concentration decreased 40.24 99.14 Example 3 Triethylamine hydrochloride concentration decreases 26.99 98.80 Example 4 Change of atmosphere in the first aggregation room 42.22 99.24 Example 5 Change of gas composition in the first polymerization chamber 47.85 98.87 Example 6 First polymerization time decreases 45.48 98.82 Example 7 First aggregation power increase 40.34 99.24 Example 8 Change of atmosphere in the second aggregation room 41.24 99.27 Example 9 Change of gas composition in the second polymerization chamber 43.35 99.03 Example 10 Change of the gas composition in the second polymerization chamber 39.67 99.20 Embodiment 11 The second polymerization time is extended 41.19 99.31 Example 12 Adding polyacrylic acid reduces polymerization time 40.29 99.23 Embodiment 13 Changes in the composition of the oxidation protection modified liquid 42.29 99.24 Embodiment 14 Oxidative modification protection time is reduced 40.24 99.25 Comparative Example 1 Interfacial Polymerization Process 45.00 99.19 Comparative Example 2 The aqueous phase does not contain sodium bicarbonate 35.78 99.29 Comparative Example 3 The aqueous phase does not contain triethylamine hydrochloride 29.47 99.17 Comparative Example 4 The first polymerization was changed to a single component polymerization 39.49 99.17 Comparative Example 5 The first polymer film back is not heated 38.46 99.11 Comparative Example 6 The second polymerization was changed to a single component polymerization 44.01 99.02 Comparative Example 7 No second polymerization chamber to supplement gas 39.02 99.23 Comparative Example 8 Oxidative modification protection component reduction 40.08 99.28
[0136] According to the data of Examples 1 to 14, Comparative Examples 1 to 8 and Table 1, it can be seen that:
[0137] The flux of Example 2 is lower than that of Example 1. This is because the content of the sodium bicarbonate component is reduced, fewer bubbles are generated by heating, the morphology shaping ability of the desalination layer is reduced, and the specific surface area of water passing through the membrane surface is reduced.
[0138] The decrease in flux in Example 3 is obviously due to the decrease in the concentration of triethylamine hydrochloride. The pore-preserving ability of the salt decreases when the base film is dried, resulting in a decline in the overall flux.
[0139] It can be seen from Examples 4 and 8 that the change in polymerization atmosphere has little performance fluctuation without affecting the overall polymerization efficiency.
[0140] Since the reaction of the second polymerization chamber is to strengthen the integrity of the membrane and improve the hydrophilicity of the membrane surface, the desalination performance of the membrane fluctuates after changing the composition of the gas in the second polymerization chamber. The decrease in the desalination performance of Example 9 is due to the replacement of styrene, which reduces the unsaturated bond content during polymerization and affects part of the polymerization efficiency.
[0141] The change in the composition of the supplementary gas introduced into the second polymerization chamber in Example 10 is due to the fact that butyric acid produces fewer oxygen-containing free radicals, especially hydrophilic groups, than hydroxyethyl acrylate, and the hydrophilic groups on the surface of the membrane are also fewer, resulting in a decrease in flux; this is similar to the phenomenon in Example 12.
[0142] Example 13 shows that the change of the oxidation protection liquid component has little effect on the performance of the membrane under the condition of having the same function. However, the change of time has a certain effect. This is because there are still a certain amount of free radicals or charges on the surface of the membrane to fully oxidize. The overall desalination rate is high, but this is not the final stable state.
[0143] Compared with the interfacial polymerization process, the process according to the present invention has similar performances, but the safety, environmental protection and convenience of the plasma polymerization process will be increased. Comparative Examples 2 to 3 show that the salt of the aqueous phase component and the heating of the membrane back in Comparative Example 5 have a great effect on maintaining the membrane flux. Comparative Examples 4 and 6 show that changes in the polymerization gas components can significantly affect the desalination rate, because the type or amount of the polymerized gas directly affects the type of free radicals generated and the polymerization efficiency. Although the desalination rate is higher when the oxidative modification protection component is reduced, the stability will deviate, which is consistent with the data in Example 14.
[0144] After the reverse osmosis membranes of some embodiments and comparative examples were stored as dry films in a sealed and light-proof environment for one month, the performance data were measured under the conditions of 500 ppm NaCl as the test liquid, 25° C., pH=7-8, and an applied pressure of 72.5 psi as shown in Table 2.
[0145] Table 2
[0146]
[0147] From the data in the table, it can be seen that compared with the preservation performance of the reverse osmosis membrane prepared by the normal interfacial polymerization process in Comparative Example 1, the desalination reduction of most embodiments of the reverse osmosis membrane using the plasma polymerization process is relatively small. However, some are larger, which shows that the influence of the component gas on the membrane when the reverse osmosis membrane is prepared by the plasma polymerization process is very large, which is also a key point in the preparation of plasma reverse osmosis membranes.
[0148] The data of Examples 13 to 14 show that the change of the components of the oxidation-modified protection solution has a great influence on the overall stability of the membrane, especially the high degree of flux change. This is because the oxidation-modified protection solution can reduce or convert the unreacted free radicals in advance, and at the same time, due to the protective function of the buffer component, it will not be excessively oxidized, resulting in changes in other chemical bonds. Therefore, converting the active groups of the desalination layer in advance is the basis for stabilizing the performance of the membrane.
[0149] The membranes of some embodiments and comparative examples were immersed in a NaClO solution at 25°C, 250ppm, pH=8 for 24h, and then tested in 500ppm NaCl as the test solution, 25°C, pH=7-8, and an applied pressure of 72.5psi. The performance data are shown in Table 3.
[0150] Table 3
[0151]
[0152] In terms of overall chlorine resistance, it can be found from the data in Table 3 that, under the condition that the initial performance is not much different, the desalination rate of the reverse osmosis membrane prepared by plasma polymerization after long-term chlorine resistance is higher than that of the membrane of the interfacial polymerization process under almost all conditions. Prolonging the time of plasma polymerization can make the desalination layer more resistant to chlorine, and the data of Example 11 just illustrates this point. Therefore, in terms of chlorine resistance, the plasma polymerization process has a more obvious advantage over the conventional interfacial polymerization process.
[0153] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a reverse osmosis membrane based on plasma polymerization, characterized in that: The following steps are involved: S1, treating the reverse osmosis membrane base film with an aqueous solution to remove excess aqueous solution from the reverse osmosis membrane base film surface, and introducing a first polymerization chamber gas into the first polymerization chamber under the first polymerization chamber atmosphere to perform a first step of plasma polymerization; S2. During the polymerization process, after 2 to 9 minutes of polymerization deposition, the back of the base film is attached to a back plate with a heating function, the heating temperature is 40 to 70° C., and plasma polymerization is continued. After 2 to 8 minutes, the polymerization is stopped and the film is placed in an oven to dry the moisture inside the film; S3, placing the film treated by S2 in a second polymerization chamber, introducing the second polymerization chamber gas under the atmosphere of the second polymerization chamber to carry out second step plasma polymerization; after a period of reaction, introducing the second polymerization chamber supplementary gas to continue the second step plasma polymerization; S4, subjecting the membrane sheet treated in S3 to oxidation protection modification treatment, and then immersing it in a mixed solution containing sodium bisulfite and glycerol, taking it out after immersion, and drying it to obtain a reverse osmosis membrane.
2. The preparation method according to claim 1, characterized in that: The time for the reverse osmosis membrane base film to be surface treated by the aqueous solution is 5 to 40 seconds; And / or, the aqueous phase solution is obtained by mixing component a, component b, sodium lauryl sulfate and water in a weight ratio of 0.25-4.5:0.5-5:0.05-0.75:95-99; And / or, the component a is at least one of sodium bicarbonate, sodium bisulfite, ammonium chloride, sodium carbonate, calcium bicarbonate, and potassium carbonate; And / or, component b is at least one of sodium camphorsulfonate, sodium sulfite, sodium lactate, sodium citrate, sodium dihydrogen phosphate, sodium phosphate, and triethylamine hydrochloride.
3. The preparation method according to claim 1, characterized in that: The first step of plasma polymerization is dielectric barrier discharge, bias voltage is 150V, flow rate of each monomer is 1-8mg / s, pressure value of polymerization chamber is set to 50-500pa, plasma polymerization power is 20-120W, distance between plasma polymerization electrodes is 13-30mm, and temperature of polymerization chamber is 25℃-45℃.
4. The preparation method according to claim 1, characterized in that: The first polymerization chamber atmosphere is: a gas atmosphere having at least one of argon, helium, oxygen, nitrogen, carbon dioxide, water vapor, sulfur hexafluoride, and ammonia; And / or, the first polymerization chamber gas is at least two of triethylamine, ethylenediamine, propylenediamine, butylenediamine, 1,3-dimethylbutylamine, di-n-butylamine, n-propylamine, isopropylamine, diisopropylamine, 2-allylamine, 3-aminopropylene, 3-butene-1-amine, 3-butene-2-amine, and 2-butene-1-amine.
5. The preparation method according to claim 1, characterized in that: The atmosphere of the second polymerization chamber is: a gas atmosphere having at least one of argon, helium, oxygen, nitrogen, carbon dioxide, nitric oxide, and nitrogen dioxide; And / or, the second polymerization chamber gas is at least two of: aniline, benzylamine, phenylethylamine, styrene, benzyl alcohol, toluidine, ethylaniline, N,N-dimethylaniline, m-xylylenediamine, p-xylylenediamine, and 4-vinylpyridine; And / or, the second polymerization chamber supplementary gas is at least one of acrylic acid, hydroxyethyl acrylate, methyl crotonate, propionic acid, butyric acid, methyl acrylate, allyl alcohol, and butenol.
6. The preparation method according to claim 1, characterized in that: The second step plasma polymerization is dielectric barrier discharge, bias voltage is 150V, each monomer flow rate is 2-9mg / s, the polymerization chamber is at normal pressure, the plasma polymerization power is 30-150W, the plasma polymerization electrode spacing is 10-40mm, the polymerization time is 4-18min, the polymerization time of the supplementary gas in the second polymerization chamber is 4-12min, and the polymerization chamber temperature is 25-45°C.
7. The preparation method according to claim 1, characterized in that: The oxidation protection modification treatment is to immerse the membrane in an oxidation protection modification solution, wherein the oxidation protection modification solution is composed of a mixture of component c, component d and component e in a weight ratio of 0.35-1.85:1.5-4.5:0.25-1.25:92-98; And / or, the component c is at least one of selenium dioxide, sodium periodate, Dess-Martin periodinane, iodosobenzene, sodium chlorite, diacetoxyiodobenzene, and bis(trifluoroacetoxyiodobenzene); and / or, the component d is at least one of 2-methyl-2-butene, 3-methyl-1-butene, 2-methyl-1-butene, 1-pentene, 2-pentene, cyclopentene, and 1,3-butadiene; And / or, the component e is at least one of sodium dihydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate, potassium phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate; And / or, the pH of the oxidation protection modification solution is 3-7, the temperature is 30±2° C., and the membrane is immersed in the oxidation modification solution for 0.5 to 5 minutes.
8. The preparation method according to claim 1, characterized in that: In the mixed solution, the mass fraction of sodium bisulfite is 0.3%, the mass fraction of glycerol is 8%, the temperature is 25±2° C., and the membrane is immersed in the sodium bisulfite solution for 0.5 to 3 minutes.
9. A reverse osmosis membrane, characterized in that: The compound is prepared by the preparation method described in any one of claims 1 to 8.
10. Use of the reverse osmosis membrane according to claim 9 in the field of water treatment.
Citation Information
Patent Citations
Preparation process of epoxy modified reverse osmosis membrane, reverse osmosis membrane and application of reverse osmosis membrane
CN114146567A
Oxidation-resistant composite reverse osmosis membrane and preparation method thereof
CN116603393A
Composite reverse osmosis membrane and preparation method therefor
WO2022127637A1