Bi-polyethylene polyamine functionalized solid amine carbon trapping material as well as preparation method and application thereof
By grafting polyethylene polyamine chains on a polystyrene resin carrier in solid amine carbon capture materials, and forming a bispolyethylene polyamine functionalized material with high amine content through chloroacetylation and ring-opening polymerization reaction, the solution is to solve the problem of The problems of uneven distribution of amine groups and easy shedding in the prior art have been achieved, efficient CO2 capture and cycle stability are achieved, and adsorption performance is significantly improved.
Patent Information
- Application Number
- CN202411246152.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
AI Technical Summary
The existing solid amine carbon capture materials have shortcomings in adsorption performance and cycle stability, especially the uneven distribution of amine groups and easy shedding, which leads to low CO2 adsorption and low grafting rate, which affects its application effect. .
Using bispolyethylene polyamine functionalized solid amine carbon capture material, grafting the polyethylene polyamine chain through chemical bonds on the polystyrene resin carrier, combining chloroacetylation and ring-opening polymerization reaction, further condensation and reduction to form a high amine content solid-state materials enhance their CO2 capture capability and cycle stability.
The CO2 capture capacity and cycle stability of the material are significantly improved. The capacity remains unchanged after 20 adsorption-desorption cycles, and the amine loading and CO2 adsorption volume are greatly increased, making it suitable for engineering utilization.
Smart Images

Figure CN118904294A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gas capture materials, and in particular relates to a bis(ethylene polyamine) functionalized solid amine carbon capture material and a preparation method and application thereof. Background Art
[0002] Today's energy structure is dominated by fossil fuels, which inevitably produces a large amount of industrial flue gas, and the resulting global warming, ocean acidification and other issues have attracted great attention. The large-scale emission of greenhouse gases such as carbon dioxide is considered to be the main cause of the greenhouse effect. Based on the current energy structure dominated by fossil energy, achieving efficient carbon capture plays a vital role in improving the climate.
[0003] Adsorption carbon capture technology is one of the important ways to achieve the separation and removal of CO2 in industrial processes or the atmosphere. The development of high-performance adsorbents is the key to this technology. Solid amine adsorbents have received widespread attention in recent years due to their excellent CO2 adsorption capacity, selectivity and low regeneration energy consumption. In the preparation of solid amine adsorbents, various synthesis methods have been reported in the literature, mainly including impregnation method, grafting method, etc. Among them, the impregnation method is widely used due to its simple operation, low cost and high nitrogen content of the adsorbent. However, the adsorbent prepared by this method often has problems such as uneven distribution of amine groups and easy shedding, which affects its adsorption performance. Grafted aminated adsorbents rely on chemical covalent methods to load amine functional groups on the surface of the carrier, but this method generally has problems such as low grafting rate and low amine content, resulting in low CO2 adsorption. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a bis(ethylene polyamine) functionalized solid amine carbon capture material and a preparation method and application thereof.
[0005] The structure of the bis(ethylene polyamine) functionalized solid amine carbon capture material is shown in the following formula, comprising polystyrene resin carrier particles, on the surface of which two polyethylene polyamine chains are grafted via chemical bonds:
[0006]
[0007] “*” represents resin particles;
[0008] n is an integer of 1-20, and m is an integer of 1-225.
[0009] The preparation method of bis(ethylenepolyamine) functionalized solid amine carbon capture material comprises the following steps:
[0010] (1) Chloroacetylation of polystyrene resin to generate chloroacetylated polystyrene resin; the specific preparation method is: polystyrene (PS) resin particles are swollen in a solvent for a certain period of time, a certain amount of chloroacetyl chloride and a catalyst are added, and the reaction is carried out at a certain temperature for a period of time. After the reaction is completed, the polystyrene resin is washed with a solvent until it is neutral and free of Cl. - , dry to constant weight.
[0011] Wherein, the solvent for swelling and reaction is any one of dichloromethane, chloroform, toluene, trimethylbenzene or a combination of at least two thereof;
[0012] The mass ratio of chloroacetyl chloride to polystyrene resin particles is 1:0.8 to 1:3.
[0013] The catalyst is any one of AlCl3, ZnCl2, FeCl3 and BF3, and its usage is 1 to 2 times of the mass of the polystyrene resin.
[0014] The reaction temperature is 10-60°C, and the reaction time is 4-12h.
[0015] The washing solvent is any one of dichloromethane, chloroform, toluene, trimethylbenzene, tetrahydrofuran and deionized water, or a combination of at least two thereof.
[0016] (2) Chloroacetylated polystyrene resin initiates ring-opening polymerization of 2-methyloxazoline, and then hydrolyzes to prepare a solid amine carbon capture material modified with monopolyethylene polyamine; the specific preparation method is: the chloroacetylated polystyrene resin obtained in step (1) and a certain proportion of 2-methyloxazoline are placed in a solvent, and a ring-opening reaction is carried out at a certain temperature for a period of time, followed by filtration, and washing with a solvent, deionized water, anhydrous ethanol and deionized water in sequence until no organic matter flows out, and then concentrated hydrochloric acid (12 mol / L, equivalent to 2-methyloxazoline) is added, and hydrolysis is carried out at the reaction temperature for a period of time.
[0017] The molar ratio of the chloroacetylated polystyrene resin to 2-methyloxazoline in the ring-opening reaction is 1:1 to 1:20.
[0018] The solvent is any one of acetonitrile, toluene, N,N-dimethylformamide and N,N-dimethylacetamide or a combination of at least two thereof.
[0019] The ring-opening reaction temperature is 80-120°C and the reaction time is 12-72h;
[0020] The hydrolysis reaction temperature is 90-110°C and the time is 24-48 hours.
[0021] (3) The solid amine material modified with monopolyethylene polyamine is further subjected to a condensation reaction with polyethylene polyamine, and then reduced to obtain a solid amine carbon capture material functionalized with dipolyethylene polyamine; the specific method is: the solid amine material modified with monopolyethylene polyamine obtained in step (2) is subjected to a condensation reaction with a certain proportion of polyethylene polyamine in a reaction solvent under the action of a catalyst at a reaction temperature for a period of time, and then washed with deionized water, anhydrous ethanol, deionized water, ~1 mol / L HCl solution to acidity, deionized water to neutrality, ~1 mol / L NaOH solution to alkalinity, and then washed with deionized water until the effluent is neutral, and NaBH4 (the molar ratio of the condensation product to the reducing agent sodium borohydride is 1:2) is added, and a reduction reaction is carried out in an ice bath for 4 hours to obtain a solid amine carbon capture material functionalized with dipolyethylene polyamine.
[0022] The ratio of the monoethylene polyamine modified solid amine material to the polyethylene polyamine in the condensation reaction is 1:5 to 1:20, and the polyethylene polyamine is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine and pentaethylenehexamine.
[0023] The solvent for the condensation reaction is any one of dioxane, toluene, ethanol, methanol, dimethyl sulfoxide, and N,N-dimethylformamide, or a combination of at least two thereof.
[0024] The catalyst is any one of sulfuric acid, acetic acid, p-toluenesulfonic acid and trifluoroacetic acid or a combination of at least two thereof, and its usage is 0.1 to 1 times of the molar amount of acyl groups in the solid amine material modified by monoethylene polyamine.
[0025] The condensation reaction temperature is 100-130°C, and the reaction time is 6-12h.
[0026] The reduction reaction solvent is either methanol or ethanol.
[0027] Beneficial effects: The bis(ethylenepolyamine) functionalized solid amine carbon capture material prepared by the present invention has a higher amine content and greatly improves the carbon dioxide capture capacity. Compared with most existing solid amine carbon capture materials, the solid amine carbon capture material of the present invention is granular and more conducive to engineering utilization; the carrier and the amine functional component of the material are connected by chemical bonds, and have better cycle stability. The carbon capture capacity remains unchanged after 20 adsorption-desorption cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a bar chart of CO2 cyclic adsorption of the bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-4 prepared in Example 4.
[0029] Figure 2 This is the infrared spectrum of the bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-4 prepared in Example 4. DETAILED DESCRIPTION
[0030] The technical scheme of the present invention is further described below by specific embodiments. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Unless otherwise specified, the raw materials involved in the specific embodiments of the present invention can be obtained by commercial purchase, and the instruments and equipment involved are all conventional instruments and equipment in the art.
[0031] Example 1
[0032] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-1 has the following structure:
[0033] The preparation method comprises the following steps:
[0034] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry dichloromethane, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 4 g of acylating agent chloroacetyl chloride and 14 g of catalyst anhydrous aluminum chloride (added in two batches), and stir at 25 ° C to allow the reaction to proceed evenly for 8 h. After the reaction is completed, wash the resin thoroughly with dichloromethane, tetrahydrofuran, 3% glacial hydrochloric acid, and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0035] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:5 ratio, add 30mL N,N dimethylformamide and 10mL 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 100℃ for 24h, collect the resin by suction filtration after the reaction, wash with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. Take the above product and hydrolyze it with 12mol / L HCl (1mL), hydrolyze at 100℃ for 30h, wash it with deionized water to neutrality after the hydrolysis, add 1mol / L NaOH solution to wash it to alkalinity, and then wash it with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0036] (3) Weigh 0.5g of the solid amine material modified by monopolyethylene polyamine in a 250mL round-bottom flask, add 0.68g of ethylenediamine, 4mL of toluene and 0.2g of p-toluenesulfonic acid respectively, react at 100℃ for 12h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / LNaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol respectively according to the molar ratio of the condensed product to the reducing agent sodium borohydride of 1:2, and react in an ice bath for 4h to obtain the bispolyethylene polyamine functionalized solid amine carbon capture material GSA2-1.
[0037] Example 2
[0038] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-2 has the following structure:
[0039] The preparation method comprises the following steps:
[0040] (1) Obtain chloroacetylated polystyrene resin in the same manner as in Example 1.
[0041] (2) Obtaining a solid amine material modified with monoethylene polyamine is the same as in Example 1.
[0042] (3) Weigh 0.5g of the solid amine material modified by monopolyethylene polyamine in a 250mL round-bottom flask, add 1.17g of diethylene triamine, 4mL of toluene and 0.2g of p-toluene sulfonic acid respectively, react at 100℃ for 12h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol respectively according to the molar ratio of the condensed product to the reducing agent sodium borohydride of 1:2, and react in an ice bath for 4h to obtain the dipolyethylene polyamine functionalized solid amine carbon capture material GSA2-2.
[0043] Example 3
[0044] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-3 has the following structure:
[0045] The preparation method comprises the following steps:
[0046] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry chloroform, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 8 g of acylating agent chloroacetyl chloride and 12 g of catalyst zinc chloride (added in two batches), and stir at 20°C to allow the reaction to proceed evenly for 6 h. After the reaction is completed, wash the resin thoroughly with chloroform, tetrahydrofuran, 3% glacial hydrochloric acid, and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0047] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:5 ratio, add 30mL toluene and 10mL 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 120°C for 24h, collect the resin by suction filtration after the reaction, wash with toluene, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. Take the above product and hydrolyze it with 12mol / L HCl (1.5mL), hydrolyze it at 100°C for 30h, wash it with deionized water to neutrality after the hydrolysis, add 1mol / L NaOH solution to wash it to alkalinity, and then wash it with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0048] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 1.17g of diethylene triamine, 4mL of N,N-methylene formamide and 0.1g of acetic acid, respectively, and react at 120°C for 24h. After the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, and vacuum dry to constant weight to obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol in a molar ratio of 1:2 between the condensed product and the reducing agent sodium borohydride, and react in an ice bath for 4h to obtain the dipolyethylene polyamine functionalized solid amine carbon capture material GSA2-3.
[0049] Example 4
[0050] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-4 has the following structure:
[0051] The preparation method comprises the following steps:
[0052] (1) Obtain chloroacetylated polystyrene resin in the same manner as in Example 1.
[0053] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:10, add 30mL toluene and 20mL 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 120°C for 24h, collect the resin by suction filtration after the reaction, wash with toluene, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. Take the above product and hydrolyze it with 12mol / L HCl (2mL), hydrolyze it at 100°C for 30h, wash it with deionized water to neutrality after the hydrolysis, add 1mol / L NaOH solution to wash it to alkalinity, and then wash it with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0054] (3) Weigh 0.5g of the solid amine material modified by monopolyethylene polyamine in a 250mL round-bottom flask, add 2.34g of diethylenetriamine, 4mL of toluene and 0.2g of p-toluenesulfonic acid respectively, react at 120°C for 24h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol respectively according to the molar ratio of the condensed product to the reducing agent sodium borohydride of 1:2, and react in an ice bath for 4h to obtain the dipolyethylene polyamine functionalized solid amine carbon capture material GSA2-4.
[0055] Example 5
[0056] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-5 has the following structure:
[0057] The preparation method comprises the following steps:
[0058] (1) Obtain chloroacetylated polystyrene resin in the same manner as in Example 1.
[0059] (2) Obtaining a solid amine material modified with monoethylene polyamine is the same as in Example 1.
[0060] (3) Weigh 0.5g of the solid amine material modified by monopolyethylene polyamine in a 250mL round-bottom flask, add 1.66g of triethylenetetramine, 4mL of toluene and 0.2g of p-toluenesulfonic acid respectively, react at 100℃ for 12h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol respectively according to the molar ratio of the condensed product to the reducing agent sodium borohydride of 1:2, and react in an ice bath for 4h to obtain the dipolyethylene polyamine functionalized solid amine carbon capture material GSA2-5.
[0061] Example 6
[0062] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-6 has the following structure:
[0063] The preparation method comprises the following steps:
[0064] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry toluene, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 10 g of acylating agent chloroacetyl chloride and 12 g of catalyst anhydrous ferric chloride (added in two batches), and stir at 30 ° C to allow the reaction to proceed evenly for 8 h. After the reaction is completed, the resin is washed thoroughly with toluene, tetrahydrofuran, 3% glacial hydrochloric acid, and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0065] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:10, 30mL N,N dimethylformamide and 20mL 2-methyl-2-oxazoline were added under nitrogen atmosphere, and the reaction was carried out at 100°C for 36h. After the reaction, the resin was collected by suction filtration, and washed with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic matter flowed out. The above product was hydrolyzed with 12mol / L HCl (4mL) at 110°C for 36h. After the hydrolysis, it was washed with deionized water to neutrality, 1mol / L NaOH solution was added to wash it to alkalinity, and then washed with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0066] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 3.32g of triethylenetetramine, 4mL of ethanol and 0.2g of p-toluenesulfonic acid respectively, react at 120°C for 10h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol respectively according to the molar ratio of the condensed product to the reducing agent sodium borohydride of 1:2, and react in an ice bath for 4h to obtain the bispolyethylene polyamine functionalized solid amine carbon capture material GSA2-6.
[0067] Example 7
[0068] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-7 has the following structure:
[0069]
[0070] Wherein n=14; the preparation method comprises the following steps:
[0071] (1) Obtain chloroacetylated polystyrene resin in the same manner as in Example 1.
[0072] (2) Obtaining a solid amine material modified with monoethylene polyamine is the same as in Example 1.
[0073] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 6.80g of PEI-600, 4mL of toluene and 0.2g of p-toluenesulfonic acid, react at 100°C for 12h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol in a molar ratio of 1:2 between the condensed product and the reducing agent sodium borohydride, and react in an ice bath for 4h to obtain the bispolyethylene polyamine functionalized solid amine carbon capture material GSA2-7.
[0074] Example 8
[0075] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-8 has the following structure:
[0076]
[0077] Wherein n=14; the preparation method comprises the following steps:
[0078] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry dichloromethane, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 4 g of acylating agent chloroacetyl chloride and 14 g of catalyst anhydrous aluminum chloride (added in two batches), and stir at 50 ° C to allow the reaction to proceed evenly for 12 h. After the reaction is completed, wash the resin thoroughly with dichloromethane, tetrahydrofuran, 3% glacial hydrochloric acid, and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0079] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:5 ratio, add 30mL acetonitrile and 10mL 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 120℃ for 60h, collect the resin by suction filtration after the reaction, wash with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. Take the above product and hydrolyze it with 12mol / L HCl (1mL), hydrolyze at 100℃ for 48h, wash it with deionized water to neutrality after the hydrolysis, add 1mol / L NaOH solution to wash it to alkalinity, and then wash it with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0080] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 6.80g of PEI-600, 4mL of dimethyl sulfoxide and 0.2g of sulfuric acid respectively, react at 100℃ for 6h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / LNaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of ethanol respectively according to the molar ratio of the condensed product to the reducing agent sodium borohydride of 1:2, and react in an ice bath for 4h to obtain the bis-polyethylene polyamine functionalized solid amine carbon capture material GSA2-8.
[0081] Example 9
[0082] The bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-9 has the following structure:
[0083]
[0084] Wherein n=14; the preparation method comprises the following steps:
[0085] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry trimethylbenzene, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 15 g of acylating agent chloroacetyl chloride and 6 g of catalyst boron trifluoride (added in two batches), and stir at 40 ° C to allow the reaction to proceed evenly for 10 h. After the reaction is completed, the resin is washed thoroughly with trimethylbenzene, tetrahydrofuran, 3% glacial hydrochloric acid and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0086] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:10, 30mL N,N-dimethylacetamide and 20mL 2-methyl-2-oxazoline were added under nitrogen atmosphere, and the reaction was carried out at 110°C for 48h. After the reaction, the resin was collected by suction filtration, and washed with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic matter flowed out. The above product was hydrolyzed with 12mol / L HCl (5mL) at 90°C for 42h. After the hydrolysis, it was washed with deionized water to neutrality, 1mol / L NaOH solution was added to wash it to alkalinity, and then washed with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0087] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 13.60g of PEI-600, 4mL of methanol and 0.26g of trifluoroacetic acid, react at 130°C for 12h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of methanol in a molar ratio of 1:2 between the condensed product and the reducing agent sodium borohydride, and react in an ice bath for 4h to obtain the bispolyethylene polyamine functionalized solid amine carbon capture material GSA2-9.
[0088] Example 10
[0089] The structure of the bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-10 is shown below:
[0090]
[0091] Wherein, n=27; the preparation method comprises the following steps:
[0092] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry chloroform, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 8 g of acylating agent chloroacetyl chloride and 12 g of catalyst zinc chloride (added in two batches), and stir at 60 ° C to allow the reaction to proceed evenly for 12 h. After the reaction is completed, wash the resin thoroughly with chloroform, tetrahydrofuran, 3% glacial hydrochloric acid and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0093] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:10, add 30mL N,N dimethylformamide and 20mL 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 100℃ for 24h, collect the resin by suction filtration after the reaction, wash with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. Take the above product and hydrolyze it with 12mol / L HCl (3mL), hydrolyze at 110℃ for 48h, wash it with deionized water to neutrality after the hydrolysis, add 1mol / L NaOH solution to wash it to alkalinity, and then wash it with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0094] (3) Weigh 0.5g of the mono-polyethylene polyamine modified solid amine material into a 250mL round-bottom flask, add 27.18g of PEI-1200, 4mL of N,N-dimethylformamide and 0.5g of p-toluenesulfonic acid, respectively, and react at 120°C for 12h. After the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, and vacuum dry to constant weight to obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of ethanol in a molar ratio of 1:2 between the condensed product and the reducing agent sodium borohydride, and react in an ice bath for 4h to obtain the di-polyethylene polyamine functionalized solid amine carbon capture material GSA2-10.
[0095] Embodiment 11
[0096] The structure of the bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-11 is shown below:
[0097]
[0098] Wherein, n=40; the preparation method comprises the following steps:
[0099] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry toluene, stir magnetically at room temperature to uniformly swell the resin for 3 h, add 10 g of acylating agent chloroacetyl chloride, 12 g of catalyst anhydrous ferric chloride (added in two batches), and stir at 40°C to uniformly react for 10 h. After the reaction is completed, wash the resin thoroughly with toluene, tetrahydrofuran, 3% glacial hydrochloric acid and cold deionized water in sequence until the eluate is neutral and free of Cl-, and finally wash it with anhydrous methanol for 6 times until the effluent is clear and transparent, and dry it in vacuum at 60°C to constant weight to obtain chloroacetylated polystyrene resin.
[0100] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉 =1:10, 30mL N,N-dimethylacetamide and 20mL 2-methyl-2-oxazoline were added under nitrogen atmosphere, and the reaction was carried out at 110°C for 36h. After the reaction, the resin was collected by suction filtration, and washed with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. The above product was hydrolyzed with 12mol / L HCl (4mL) at 90°C for 36h. After the hydrolysis, it was washed with deionized water to neutrality, 1mol / L NaOH solution was added to wash it to alkalinity, and then washed with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0101] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 40.77g of PEI-1800, 4mL of dioxane and 0.1g of acetic acid, react at 130°C for 10h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of ethanol in a molar ratio of 1:2 between the condensed product and the reducing agent sodium borohydride, and react in an ice bath for 4h to obtain the dipolyethylene polyamine functionalized solid amine carbon capture material GSA2-11.
[0102] Example 12
[0103] The structure of the bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-12 is shown below:
[0104]
[0105] Wherein, n=225; the preparation method comprises the following steps:
[0106] (1) Weigh 10 g of polystyrene (PS) resin into a 250 mL three-necked round-bottom flask, add 100 mL of dry trimethylbenzene, stir magnetically at room temperature to allow the resin to swell evenly for 3 h, then add 15 g of acylating agent chloroacetyl chloride and 6 g of catalyst boron trifluoride (added in two batches), and stir at 50 ° C to allow the reaction to proceed evenly for 12 h. After the reaction is completed, the resin is washed thoroughly with trimethylbenzene, tetrahydrofuran, 3% glacial hydrochloric acid and cold deionized water in sequence until the eluate is neutral and free of Cl - Finally, the product was washed with anhydrous methanol for 6 times until the effluent was clear and transparent, and then dried under vacuum at 60°C to a constant weight to obtain chloroacetylated polystyrene resin.
[0107] (2) Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and PS-COCH2-Cl :n 2-甲基噁唑啉=1:10, add 30mL toluene and 20mL 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 120°C for 48h, collect the resin by suction filtration after the reaction, wash with DMF, deionized water, anhydrous ethanol and deionized water in sequence until no organic flow out. Take the above product and hydrolyze it with 12mol / L HCl (5mL), hydrolyze at 110°C for 48h, wash it with deionized water to neutrality after the hydrolysis, add 1mol / L NaOH solution to wash it to alkalinity, and then wash it with deionized water to neutrality to obtain a solid amine material modified with monopolyethylene polyamine.
[0108] (3) Weigh 0.5g of the solid amine material modified with monopolyethylene polyamine in a 250mL round-bottom flask, add 226.6g of PEI-10000, 4mL of ethanol and 0.26g of trifluoroacetic acid, react at 120°C for 12h, and after the reaction, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral, vacuum dry to constant weight, and obtain the condensed product. Take 0.3g of the condensed product in a small reaction bottle, add sodium borohydride and 10mL of ethanol in a molar ratio of 1:2 between the condensed product and the reducing agent sodium borohydride, and react in an ice bath for 4h to obtain the bispolyethylene polyamine functionalized solid amine carbon capture material GSA2-12.
[0109] Comparative Example 1
[0110] The solid amine carbon capture material GSA2-13 has the following structure:
[0111] The preparation method comprises the following steps:
[0112] The chloroacetylated polystyrene resin obtained is the same as that in Example 1.
[0113] Weigh 0.5 g of chloroacetylated polystyrene resin (PS-COCH2-Cl), add 5 mL of tetrahydrofuran (THF) and swell for 3 h. Cl :n EDA =1:9 ratio, add 1.23g ethylenediamine, and react at 30°C for 3h. After the reaction, filter the resin, wash with anhydrous ethanol, shake in 0.2mol / L NaOH solution for 12h, and then wash with deionized water until neutral and free of Cl - , and dried under vacuum at 50° C. to constant weight to obtain the solid amine carbon capture material GSA2-13.
[0114] Comparative Example 2
[0115] The solid amine carbon capture material GSA2-14 has the following structure:
[0116] The preparation method comprises the following steps:
[0117] The chloroacetylated polystyrene resin obtained is the same as that in Example 1.
[0118] Weigh 0.5 g of chloroacetylated polystyrene resin (PS-COCH2-Cl), add 5 mL of tetrahydrofuran (THF) and swell for 3 h. Cl :n DETA =1:9 ratio, add 2.10g diethylenetriamine, and react at 30°C for 3h. After the reaction, filter the resin, wash with anhydrous ethanol, shake in 0.2mol / L NaOH solution for 12h, and then wash with deionized water until neutral and free of Cl - , and dried under vacuum at 50° C. to constant weight to obtain the solid amine carbon capture material GSA2-14.
[0119] Comparative Example 3
[0120] The solid amine carbon capture material GSA2-15 has a polyamine chain with the following structure:
[0121] The preparation method comprises the following steps:
[0122] The chloroacetylated polystyrene resin obtained is the same as that in Example 1.
[0123] Weigh 0.5 g of chloroacetylated polystyrene resin (PS-COCH2-Cl), add 5 mL of tetrahydrofuran (THF) and swell for 3 h. Cl :n TETA =1:9 ratio, add 2.98g triethylenetetramine, and react at 30°C for 3h. After the reaction, filter the resin, wash with anhydrous ethanol, shake in 0.2mol / L NaOH solution for 12h, and then wash with deionized water until neutral and free of Cl - , and dried under vacuum at 50° C. to constant weight to obtain the solid amine carbon capture material GSA2-15.
[0124] Comparative Example 4
[0125] The solid amine carbon capture material GSA2-16 has a polyamine chain with the following structure:
[0126]
[0127] Wherein, n=14; the preparation method comprises the following steps:
[0128] The chloroacetylated polystyrene resin obtained is the same as that in Example 1.
[0129] Weigh 0.5 g of chloroacetylated polystyrene resin (PS-COCH2-Cl) and Cl :n PEI-600 =1:3 ratio, add 4.08g PEI-600, react at 90℃ for 5h. After the reaction, filter the resin, wash with deionized water, anhydrous ethanol, deionized water, ~1mol / L HCl solution to acidity, deionized water to neutrality, ~1mol / L NaOH solution to alkalinity, and then wash with deionized water until the effluent is neutral and free of Cl - The solid amine carbon capture material GSA2-16 was obtained by vacuum drying at 60°C to a constant weight.
[0130] Comparative Example 5
[0131] The solid amine carbon capture material GSA2-17 has the following structure:
[0132] The preparation method comprises the following steps:
[0133] The chloroacetylated polystyrene resin obtained is the same as that in Example 1.
[0134] Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and add 100 mL of chloroacetylated polystyrene resin to the mixture. PS-COCH2-Cl :n 2-甲基噁唑啉 =1:5 ratio, add 30mL of anhydrous and oxygen-free N,N dimethylformamide (DMF) and 9.50mL of 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 100°C for 24h, collect the resin by suction filtration after the reaction, wash with DMF, deionized water, anhydrous ethanol and deionized water in turn. Take the above product and hydrolyze it with 12mol / L HCl, and hydrolyze it at 100°C for 48h. After the hydrolysis is completed, wash it with deionized water to neutrality, add 1mol / L NaOH solution to wash it to alkalinity, and finally wash it with deionized water to neutrality. Obtain the solid amine material GSA2-17 modified with monopolyethylene polyamine.
[0135] Comparative Example 6
[0136] The solid amine carbon capture material GSA2-18 has a polyamine chain with the following structure:
[0137] The preparation method comprises the following steps:
[0138] The chloroacetylated polystyrene resin obtained is the same as that in Example 1.
[0139] Weigh 0.5 g of chloroacetylated polystyrene resin into a dry 100 mL Shrek tube and add 100 mL of chloroacetylated polystyrene resin to the mixture. PS-COCH2-Cl :n 2-甲基噁唑啉=1:10 ratio, add 30mL of anhydrous and oxygen-free N,N dimethylformamide (DMF) and 19.00mL of 2-methyl-2-oxazoline respectively under nitrogen atmosphere, react at 100°C for 24h, collect the resin by suction filtration after the reaction, wash with DMF, deionized water, anhydrous ethanol and deionized water in sequence. Take the above product and hydrolyze it with 12mol / L HCl at 100°C for 48h. After the hydrolysis is completed, wash it with deionized water to neutrality, add 1mol / L NaOH solution to wash it to alkalinity, and finally wash it with deionized water to neutrality. Obtain the solid amine material GSA2-18 modified with monopolyethylene polyamine.
[0140] Performance Test:
[0141] Test of the bis(ethylene polyamine) functionalized solid amine carbon capture material GSA2-4 provided in Example 4
[0142] (1) CO2 cyclic adsorption performance: 30 mg of the bis(ethylene polyamine) functionalized solid amine carbon capture material GSA2-4 provided in Example 4 was weighed into an adsorption instrument, and 1 atm CO2 gas (400 sccm) was introduced at 25°C, the weight gain was recorded, and the adsorption amount was calculated; the inlet gas was changed to N2, the temperature was raised to 100°C for CO2 desorption for 45 min, the temperature was lowered to 25°C, the inlet gas was changed to CO2, and adsorption was performed again, and this was repeated 20 times to obtain a CO2 cyclic adsorption bar graph of the bis(ethylene polyamine) functionalized solid amine carbon capture material GSA2-4 provided in Example 4 as shown in FIG. Figure 1 As shown;
[0143] (2) Infrared spectrum analysis: The polyethylene polyamine functionalized solid amine carbon capture material before and after condensation and after reduction was ground into powder and mixed with potassium bromide. After tableting, it was placed in a combined window plate and tested using IS50 Fourier transform infrared. The structure of the resin was inferred based on the position of the absorption peak in the infrared spectrum. The results are as follows Figure 2 shown.
[0144] from Figure 1 It can be seen that the bis(ethylenepolyamine) functionalized solid amine carbon capture material GSA2-4 provided in Example 4 has excellent cycle stability. After 20 adsorption / desorption cycles, the CO2 adsorption capacity of the material only decreased by about 0.4%.
[0145] from Figure 2 It can be seen that after the polystyrene resin is chloroacetylated to generate chloroacetylated polystyrene resin, the -1 The C=O stretching vibration absorption peak appeared at 1286 cm -1 The peak at 638 cm is attributed to the in-plane bending vibration peak of the chloroacetyl -CH2-C1 group of the phenyl ring. -1The C-C1 stretching vibration peak appeared at 1683 cm-1. The appearance of the above three characteristic peaks proves that the chloroacetylated polystyrene resin was successfully prepared. The chloroacetylated polystyrene resin initiated the ring-opening polymerization of 2-methyloxazoline, and then hydrolyzed to prepare the solid amine carbon capture material modified by monoethylene polyamine. Through infrared spectroscopy, it can be seen that due to the condensation of carbonyl and amino groups, the 1683 cm-1 peak in the original chloroacetylated polystyrene resin -1 The C=O stretching vibration absorption peak at 3430cm -1 A strong NH stretching vibration peak appeared at 1380cm. The above data results fully prove that the solid amine carbon capture material modified by monoethylene polyamine was successfully prepared through ring-opening polymerization and hydrolysis reaction. After reduction, the stretching vibration characteristic peak of C=N weakened, and the peak at 1380cm -1 The CN stretching vibration peak appears at , indicating successful reduction.
[0146] Tests on the bis(ethylenepolyamine) functionalized solid amine carbon capture materials GSA2-1-12 provided in Examples 1-12 and the solid amine carbon capture materials GSA2-13-18 provided in Comparative Examples 1-6:
[0147] (1) Amine loading (E): Weigh m (about 0.1 g) of solid amine carbon capture material into a 100 mL conical flask, add 50 mL of HCl solution with a concentration of C2 (~0.10 mol / L), shake at 25°C for 12 h, take 10 mL of the shaking solution and titrate with NaOH solution with a concentration of C1 (~0.05 mol / L), and the volume of NaOH consumed is V (mL). Titrate three times in parallel according to Calculate and obtain the amine loading;
[0148] (2) CO2 adsorption capacity: Weigh about 30 mg of solid amine carbon capture material into the adsorption instrument, introduce 1 atm CO2 gas at 25°C, record the weight gain, and calculate the CO2 adsorption capacity.
[0149] The test was carried out according to the above test method, and the test results are shown in Table 1:
[0150] Table 1
[0151]
[0152]
[0153] According to the data in Table 1, it can be seen that compared with the solid amine carbon capture materials GSA2-13-16 prepared by direct grafting method provided by Comparative Examples 1 to 4 and the solid amine carbon capture materials prepared by ring-opening polymerization method provided by Comparative Examples 5 to 6, the diethylene polyamine functionalized solid amine carbon capture materials GSA2-1 to GSA2-12 provided by Examples 1 to 12 have significantly higher amine loading, and thus higher CO2 adsorption capacity.
[0154] The applicant declares that the present invention illustrates a solid amine carbon capture material and its preparation method and application through the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A bis(ethylenepolyamine) functionalized solid amine carbon capture material, characterized in that: The solid amine carbon capture material uses polystyrene resin as carrier particles, and two polyethylene polyamines are grafted onto the surface of the carrier particles through chemical bonds: its structural formula is shown below: "*" represents resin particles; n is an integer of 1-20, and m is an integer of 1-225.
2. A method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material as claimed in claim 1, characterized in that: The preparation method steps are as follows: (1) chloroacetylation of polystyrene resin particles to generate chloroacetylated polystyrene resin; (2) 2-methyloxazoline ring-opening polymerization is initiated by chloroacetylated polystyrene resin, followed by hydrolysis to prepare a solid amine carbon capture material modified with monoethylene polyamine; (3) The solid amine carbon capture material modified with monopolyethylene polyamine is subjected to a condensation reaction with polyethylene polyamine, and then reduced to obtain a solid amine carbon capture material functionalized with bispolyethylene polyamine.
3. The method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material according to claim 2, characterized in that: The specific method of chloroacetylation of the polystyrene resin in step (1) is: swelling the polystyrene resin particles in a solvent, then adding chloroacetyl chloride and a catalyst to react, and after the reaction is completed, washing with a solvent until it is neutral and free of Cl - , dry to constant weight.
4. The method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material according to claim 3, characterized in that: The solvent for swelling the resin particles is: any one of dichloromethane, chloroform, toluene, and trimethylbenzene, or a combination of at least two of them; the mass ratio of chloroacetyl chloride to polystyrene resin particles is 1:0.8-1:3; the catalyst is any one of AlCl3, ZnCl2, FeCl3, and BF3, and its dosage is 1-2 times the mass of the polystyrene resin; the reaction temperature is 10-60°C, and the reaction time is 4-12 hours; the washing solvent is: any one of dichloromethane, chloroform, toluene, trimethylbenzene, tetrahydrofuran, and deionized water, or a combination of at least two of them.
5. The method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material according to claim 2, characterized in that: The specific preparation method of the monoethylene polyamine modified solid amine carbon capture material in step (2) is: subjecting the chloroacetylated polystyrene resin obtained in step (1) to a ring-opening reaction with 2-methyloxazoline in a solvent, followed by filtration, washing, and then adding concentrated hydrochloric acid for hydrolysis reaction.
6. The method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material according to claim 5, characterized in that: The molar ratio of chloroacetylated polystyrene resin to 2-methyloxazoline in the ring-opening reaction is 1:1 to 1:20; the solvent is any one of acetonitrile, toluene, N,N-dimethylformamide, and N,N-dimethylacetamide or a combination of at least two thereof; the ring-opening reaction temperature is 80 to 120°C, the reaction time is 12 to 72 hours, and the hydrolysis reaction temperature is 90 to 110°C, and the reaction time is 24 to 48 hours.
7. The method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material according to claim 2, characterized in that: The specific preparation method of the bis-polyethylene polyamine functionalized solid amine carbon capture material is as follows: the mono-polyethylene polyamine modified solid amine carbon capture material obtained in step (2) is subjected to a condensation reaction with polyethylene polyamine in a reaction solvent under the action of a catalyst, and then washed and NaBH4 is added to carry out a reduction reaction in an ice bath for 12 hours to obtain the bis-polyethylene polyamine functionalized solid amine carbon capture material.
8. The method for preparing a bis(ethylenepolyamine) functionalized solid amine carbon capture material according to claim 7, characterized in that: The molar ratio of acyl group to polyethylene polyamine in the solid amine carbon capture material modified by monopolyethylene polyamine is 1:5-1:20; the polyethylene polyamine is any one of ethylenediamine, diethylenetriamine, triethylenetetramine and PEI-600; the reaction solvent is any one of toluene, ethanol, methanol, dimethyl sulfoxide and N,N-dimethylformamide or a combination of at least two of them; the catalyst is any one of sulfuric acid, acetic acid, p-toluenesulfonic acid and trifluoroacetic acid or a combination of at least two of them, and the amount thereof is 0.1-1 times of the molar amount of acyl group in the solid amine material modified by monopolyethylene polyamine; the condensation reaction temperature is 100-130°C, and the reaction time is 6-12h; the reduction reaction solvent is methanol or ethanol.
9. An application of the bis(ethylenepolyamine) functionalized solid amine carbon capture material as claimed in claim 1, characterized in that: The solid amine carbon capture material is used for adsorption of carbon dioxide.
Citation Information
Cited By
Solid amine resin adsorbent as well as preparation method and application thereof
CN119608122A