Mercapto-modified metal organic framework magnetic mercury removal material and preparation method thereof

The magnetic mercury removal material of metal organic skeleton modified by thiol group combines iron tetroxide nanoparticles with UiO-66 core-shell material and adheres to lysozyme film, solving the problems of low adsorption capacity and long equilibrium time of traditional materials, achieving high efficiency Mercury ion adsorption and magnetic separation are suitable for mercury pollution control.

CN118904301APending Publication Date: 2024-11-08CHINA CONSTR EIGHT ENG DIV CORP LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410990596.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional inorganic and organic materials have problems such as low adsorption capacity, long adsorption equilibrium time and poor selectivity when removing mercury ions in water and soil.

Method used

The mercury-removing material of metal organic skeleton modified with thiol group is formed to enhance adsorption of mercury ions by combining iron tetraoxide nanoparticles with UiO-66 core-shell material and adhesion of amyloid lysozyme film on the surface. ability. The material preparation method includes ultrasonic treatment, heating reaction and pH adjustment, and the phase transformation of the structure is achieved by using supramolecular assembly, avoiding the high economic and environmental costs brought by chemical reactions.

Benefits of technology

It significantly improves the specific surface area and structural stability of the material. The thiol functional groups form a strong chelation with mercury ions, which has an efficient adsorption effect. It is suitable for the restoration and treatment of mercury-contaminated water and soil. It is easy to separate magnetic properties, which is conducive to recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904301A_ABST
    Figure CN118904301A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfydryl-modified metal organic framework magnetic mercury removal material and a preparation method thereof. The preparation method comprises the following steps: putting ferroferric oxide nanoparticles into a reaction solution to obtain a mixture; performing ultrasonic treatment on the mixture in an ultrasonic bath, performing heating reaction, and cooling to room temperature to obtain a polymer solution; washing the polymer solution to obtain a core-shell material; dissolving tris (2-carboxyethyl) phosphine hydrochloride in the tris (hydroxymethyl) aminomethane buffer solution to obtain a salt solution; lysozyme is dissolved in a tris (hydroxymethyl) aminomethane buffer solution to obtain an enzyme solution, and then the enzyme solution and the salt solution with the adjusted pH are evenly mixed in an equal-volume mode to form a phase transformation solution; the core-shell material is immersed in the phase transition solution to be dispersed, and dispersion liquid is obtained; and carrying out solid-liquid separation on the reacted dispersion liquid to obtain the sulfydryl-modified metal organic framework magnetic mercury removal material. According to the invention, the problems of low adsorption capacity and long adsorption equilibrium time of a traditional mercury ion removal material are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water and soil remediation, and in particular to a thiol-modified metal organic framework magnetic mercury removal material and a preparation method thereof. Background Art

[0002] Environmental pollution is becoming increasingly serious, especially heavy metal pollution. Since heavy metal ions are highly toxic and non-degradable, countries have introduced policies to strengthen management. Mercury pollution sources are widespread and the emissions are large. There are natural activities such as crustal movement and volcanic eruptions, as well as human activities such as mining and metallurgy, which will release a large amount of mercury into water bodies and soil. For example, mercury is one of the top three inorganic pollutants in my country's soil. In water bodies, mercury ions are the main form of existence, which are extremely toxic and can be enriched through the food chain, causing irreversible damage to the human body. Therefore, it is imperative to develop efficient mercury ion removal technology.

[0003] At present, some materials remove and stabilize heavy metals in water and soil through methods such as surface adsorption and co-precipitation. However, traditional inorganic materials such as zeolite and molecular sieve, organic polymer materials such as fiber and resin, and activated carbon have problems such as low adsorption capacity, long adsorption equilibrium time and poor selectivity.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] In order to overcome the defects of the prior art, a thiol-modified metal organic framework magnetic mercury removal material and a preparation method thereof are provided to solve the problems of low adsorption capacity and long adsorption equilibrium time of traditional inorganic or organic materials for removing mercury ions.

[0006] To achieve the above object, a method for preparing a thiol-modified metal organic framework magnetic mercury removal material is provided, comprising the following steps:

[0007] placing ferrosoferric oxide nanoparticles as seeds into a reaction solution to obtain a mixture, the reaction solution comprising zirconium tetrachloride, terephthalic acid, dimethylformamide, and glacial acetic acid;

[0008] The mixture was ultrasonically treated in an ultrasonic bath for 30 minutes, and then transferred to a reaction kettle for heating and reaction, and then cooled to room temperature to obtain a polymer solution;

[0009] The polymer solution was washed with dimethylformamide and methanol respectively to obtain Fe3O4@UiO-66 core-shell material;

[0010] dissolving tris(2-carboxyethyl)phosphine hydrochloride in a tris(hydroxymethylaminomethane) buffer solution to obtain a salt solution, and adjusting the pH of the salt solution with a NaOH solution;

[0011] The lysozyme is dissolved in a tris(hydroxymethyl)aminomethane) buffer solution to obtain an enzyme solution, and then the enzyme solution is mixed with an equal volume of a pH-adjusted salt solution to form a phase transition solution;

[0012] The Fe3O4@UiO-66 core-shell material is immersed in the phase transition solution and dispersed to obtain a dispersion, wherein the dispersion is reacted at room temperature to allow an amyloid lysozyme film to adhere to the surface of the Fe3O4@UiO-66 core-shell material;

[0013] The dispersion liquid after the reaction is subjected to solid-liquid separation to obtain a thiol-modified metal organic framework magnetic mercury removal material.

[0014] Furthermore, the ratio of the ferrosoferric oxide nanoparticles, the zirconium tetrachloride, the terephthalic acid, the dimethylformamide and the glacial acetic acid is 0.2-1 g: 0.5-1.5 g: 0.3-1.0 g: 50-100 mL: 4-16 mL.

[0015] Furthermore, the reaction temperature of the heating reaction is 150-200° C., and the reaction time is 10-12 hours.

[0016] Furthermore, before the Fe3O4@UiO-66 core-shell material is immersed in the phase transition solution, the Fe3O4@UiO-66 core-shell material is subjected to ultrasonic treatment for 15 to 20 minutes.

[0017] The invention provides a thiol-modified metal organic framework magnetic mercury removal material. The thiol-modified metal organic framework magnetic mercury removal material is prepared by a preparation method of a thiol-modified metal organic framework magnetic mercury removal material.

[0018] The invention provides an application of a thiol-modified metal organic framework magnetic mercury removal material. The thiol-modified metal organic framework magnetic mercury removal material is added into a mercury-containing aqueous solution to be treated, and oscillated at 150-180 r / min under a constant temperature of 25±0.5°C until adsorption equilibrium is reached.

[0019] The beneficial effect of the present invention is that the thiol-modified metal organic framework magnetic mercury removal material of the present invention has a high specific surface area, a stable structure, and rich functional groups, wherein the thiol functional groups form a strong chelating effect with mercury ions, have a significant adsorption effect, and are suitable for the remediation of mercury-contaminated water and soil.

[0020] The thiol-modified metal organic framework magnetic mercury removal material of the present invention has magnetism, can be easily separated from water, and is conducive to recycling.

[0021] The thiol-modified metal organic framework magnetic mercury removal material of the present invention uses lysozyme in the preparation process, which has the characteristics of wide source, low price, good water solubility and stability; its phase transition process is achieved through supramolecular assembly, does not need to rely on chemical reactions, and can flexibly regulate the structure after phase transition by changing external conditions, thus avoiding the high economic and environmental costs brought by chemical synthesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0023] Figure 1 This is a transmission electron micrograph of the thiol-modified metal organic framework magnetic mercury removal material of Example 1 of the present invention.

[0024] Figure 2 This is the hysteresis curve of the mercury removal material of the thiol-modified metal organic framework magnetic mercury removal material in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It is also necessary to explain that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.

[0026] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0027] The present invention provides a method for preparing a thiol-modified metal organic framework magnetic mercury removal material, comprising the following steps:

[0028] S1. Putting ferrosoferric oxide nanoparticles as seed crystals into a reaction solution to obtain a mixture. The reaction solution includes zirconium tetrachloride, terephthalic acid, dimethylformamide and glacial acetic acid.

[0029] The reaction solution consists of zirconium tetrachloride (ZrCl4), terephthalic acid, dimethylformamide (DMF) and glacial acetic acid.

[0030] As a preferred embodiment, the ratio of ferrosoferric oxide nanoparticles, zirconium tetrachloride, terephthalic acid, dimethylformamide and glacial acetic acid is 0.2-1 g: 0.5-1.5 g: 0.3-1.0 g: 50-100 mL: 4-16 mL.

[0031] S2. The mixture was ultrasonically treated in an ultrasonic bath for 30 min, and then transferred to a reactor for heating and reaction, and then cooled to room temperature to obtain a polymer solution.

[0032] The mixture obtained in S1 was sonicated in an ultrasonic bath for 30 min, then transferred to a reactor and heated for reaction and then cooled to room temperature.

[0033] As a preferred embodiment, the reaction temperature of the heating reaction in the reactor is 150-200° C., and the reaction time is 10-12 hours.

[0034] In this embodiment, the reaction kettle is a stainless steel autoclave lined with Teflon.

[0035] S3. The polymer solution was washed with dimethylformamide and methanol respectively to obtain Fe3O4@UiO-66 core-shell material.

[0036] The washed Fe3O4@UiO-66 core-shell material is vacuum dried at 45-60°C for 8-10 h to obtain a dry Fe3O4@UiO-66 core-shell material.

[0037] S4. Dissolve tris(2-carboxyethyl)phosphine hydrochloride in tris(hydroxymethylaminomethane) buffer solution to obtain a salt solution, and adjust the pH of the salt solution with NaOH solution.

[0038] The concentration of tri(2-carboxyethyl)phosphine hydrochloride is 5 to 50 mmol / L.

[0039] The pH of the tris(hydroxymethyl)aminomethane buffer solution is 7 to 7.5, and the concentration is 8 to 20 mmol / L.

[0040] The pH of the salt solution is adjusted to 5-10 using 2 mol / L NaOH.

[0041] S5. Dissolve lysozyme in a tris(hydroxymethylaminomethane) buffer solution to obtain an enzyme solution, and then mix the solution with an equal volume of a pH-adjusted salt solution to form a phase transition solution.

[0042] In this example, the concentration of lysozyme is 1-3 mg / mL.

[0043] S6. Immerse the Fe3O4@UiO-66 core-shell material in a phase transition solution to obtain a dispersion, and react the dispersion at room temperature to allow an amyloid lysozyme film to adhere to the surface of the Fe3O4@UiO-66 core-shell material.

[0044] Before the Fe3O4@UiO-66 core-shell material was immersed in the phase transition solution, the Fe3O4@UiO-66 core-shell material was ultrasonically treated for 15 to 20 min.

[0045] The dosage of Fe3O4@UiO-66 core-shell material is 0.1~1.0g.

[0046] The Fe3O4@UiO-66 core-shell material was immersed in the phase change solution and mechanically stirred at 180-200 r / min.

[0047] S7. The dispersion liquid after the reaction is subjected to solid-liquid separation to obtain a thiol-modified metal organic framework magnetic mercury removal material.

[0048] Specifically, an external magnetic field is used to separate the composite material from the solution in the dispersion after the reaction, and after washing with deionized water for multiple times, it is dried at 45-60° C. for 8-10 hours to obtain a PTL-coated thiol-modified metal organic framework magnetic mercury removal material.

[0049] The invention provides a thiol-modified metal organic framework magnetic mercury removal material. The thiol-modified metal organic framework magnetic mercury removal material is prepared by a preparation method of a thiol-modified metal organic framework magnetic mercury removal material.

[0050] The invention provides an application of a thiol-modified metal organic framework magnetic mercury removal material. The thiol-modified metal organic framework magnetic mercury removal material is added into a mercury-containing aqueous solution to be treated, and oscillated at 150-180 r / min under a constant temperature of 25±0.5°C until adsorption equilibrium is reached.

[0051] The thiol-modified metal organic framework magnetic mercury removal material of the present invention has a high specific surface area, a stable structure, and rich functional groups. The thiol functional groups form a strong chelation with mercury ions, have a significant adsorption effect, and are suitable for the restoration and treatment of mercury-contaminated water and soil.

[0052] The thiol-modified metal organic framework magnetic mercury removal material of the present invention has magnetism, can be easily separated from water, and is conducive to recycling.

[0053] The thiol-modified metal organic framework magnetic mercury removal material of the present invention uses lysozyme in the preparation process, which has the characteristics of wide source, low price, good water solubility and stability; its phase transition process is achieved through supramolecular assembly, does not need to rely on chemical reactions, and can flexibly regulate the structure after phase transition by changing external conditions, thus avoiding the high economic and environmental costs brought by chemical synthesis.

[0054] The present invention is further described in detail below in conjunction with the embodiments and comparative examples. It should be noted that the specific embodiments described herein are only used to explain the present invention and do not limit the scope and application of the present invention.

[0055] Embodiment 1:

[0056] This embodiment provides a method for preparing a thiol-modified metal organic framework magnetic mercury removal material, comprising the following steps:

[0057] 0.8 g of Fe 3 O 4 was added to a reaction solution containing 1.0 g of ZrCl 4 , 0.8 g of terephthalic acid, 100 mL of dimethylformamide and 4 mL of glacial acetic acid to obtain a mixture.

[0058] After being treated in an ultrasonic bath for 30 min, the mixture was transferred to a reactor, heated at 120 °C for 24 h, and cooled to room temperature to obtain a polymer solution. The polymer solution was washed with dimethylformamide and methanol, respectively, and dried in vacuo at 50 °C to obtain Fe3O4@UiO-66 core-shell material.

[0059] Prepare 10 mmol / L Tris(hydroxymethyl)aminomethane buffer solution and adjust the pH to 7 with 2 mol / L NaOH.

[0060] A 10 mmol / L tris(2-carboxyethyl)phosphine solution in tris(hydroxymethylaminomethane) buffer (100 ml) was adjusted to pH 8 with 2 mol / L NaOH, and then mixed with an equal volume of a 1.25 mg / mL lysozyme solution in tris(hydroxymethylaminomethane) buffer (100 ml) to form a phase transition solution.

[0061] 0.5 g of Fe3O4@UiO-66 core-shell material treated with ultrasound for 10 min was evenly dispersed in the phase transition mixture and mechanically stirred at room temperature for 3 h to form a phase transition lysozyme film on the surface of the Fe3O4@UiO-66 core-shell material.

[0062] Subsequently, solid-liquid separation was achieved by applying an external magnetic field, and after multiple washings with deionized water, the material was dried at 50°C for 12 hours to obtain a magnetic mercury removal material coated with a phase transition lysozyme film (thiol-modified metal-organic framework magnetic mercury removal material).

[0063] The prepared thiol-modified metal organic framework magnetic mercury removal material is used to adsorb mercury ions in water:

[0064] 0.05 g of thiol-modified metal organic framework magnetic mercury removal material was added to 50 mL of 100 mg / L mercury-containing solution, and the solution was shaken at 150 r / min for 24 h in a constant temperature air bath shaker at 25±0.5°C to reach adsorption equilibrium.

[0065] Subsequently, the composite material was separated by a magnet, and the supernatant was taken to determine the Hg2+ concentration. The adsorption capacity of the magnetic adsorption material was calculated to be 277.6 mg / g.

[0066] Figure 1This is the TEM image of the thiol-modified metal-organic framework magnetic mercury removal material prepared in this embodiment. It can be seen from the figure that the thiol-modified metal-organic framework magnetic mercury removal material prepared in this embodiment has an obvious core-shell structure, forming a thiol-modified metal-organic framework magnetic mercury removal material with Fe3O4 nanoparticles as the core, UiO-66 as the shell, and a phase-transition lysozyme film coated on the outer layer.

[0067] Figure 2 The hysteresis curve of the thiol-modified metal organic framework magnetic mercury removal material prepared in this example has a saturation magnetization (Ms) of 51.3emu / g, which has good superparamagnetic properties and is conducive to recovery from the solution in practical applications.

[0068] Embodiment 2:

[0069] 0.8 g of Fe3O4 was added to a reaction solution containing 1.2 g of ZrCl4, 1.0 g of terephthalic acid, 100 mL of dimethylformamide and 4 mL of glacial acetic acid; after being treated in an ultrasonic bath for 30 min, the mixture was transferred to a reactor, heated at 120°C for 24 h, cooled to room temperature, washed with dimethylformamide and methanol respectively, and dried in vacuum at 50°C to obtain Fe3O4@UiO-66 core-shell material.

[0070] Prepare 15mmol / L tris(2-carboxyethyl)phosphine buffer solution, adjust pH to 7 with 2mol / L NaOH; adjust pH to 8 with 2mol / L NaOH in 10mmol / L tris(2-carboxyethyl)phosphine buffer solution (100ml), and then mix with 1.5mg / mL lysozyme buffer solution (100ml) in equal volumes to form a phase transition solution. 0.5g Fe3O4@UiO-66 core-shell material treated with ultrasound for 10min was evenly dispersed in the phase transition mixture, and mechanically stirred at room temperature for 3h to form a phase transition lysozyme film on the surface of the Fe3O4@UiO-66 core-shell material. Subsequently, solid-liquid separation was achieved by applying an external magnetic field, and after multiple washings with deionized water, it was dried at 50℃ for 12h to obtain a magnetic mercury removal material coated with a phase transition lysozyme film.

[0071] The prepared thiol-modified metal organic framework magnetic mercury removal material was used to adsorb mercury ions in water: 0.05g of thiol-modified metal organic framework magnetic mercury removal material was added to 50mL of mercury-containing solution with a concentration of 100mg / L, and the mixture was shaken at 150r / min for 24h in a constant temperature air bath shaker at 25±0.5℃ to reach adsorption equilibrium. Subsequently, the thiol-modified metal organic framework magnetic mercury removal material was separated by a magnet, and the supernatant was taken to determine the Hg2+ concentration. By calculation, the adsorption capacity of the magnetic adsorption material was 308.5mg / g.

[0072] Embodiment 3:

[0073] 0.5 g of Fe3O4 was added to a reaction solution containing 1.0 g of ZrCl4, 1.0 g of terephthalic acid, 100 mL of dimethylformamide and 4 mL of glacial acetic acid; after being treated in an ultrasonic bath for 30 min, the mixture was transferred to a reactor, heated at 120°C for 24 h, cooled to room temperature, washed with dimethylformamide and methanol respectively, and dried in vacuum at 50°C to obtain Fe3O4@UiO-66 core-shell material.

[0074] Prepare 20mmol / L tris(2-carboxyethyl)phosphine buffer solution, adjust pH to 7 with 2mol / L NaOH; adjust pH to 8 with 2mol / L NaOH in 100ml tris(2-carboxyethyl)phosphine buffer solution (100ml), and then mix with 1.5mg / mL lysozyme buffer solution (100ml) in equal volumes to form a phase transition solution. 0.5g Fe3O4@UiO-66 core-shell material treated with ultrasound for 10min was evenly dispersed in the phase transition mixture, and mechanically stirred at room temperature for 3h to form a phase transition lysozyme film on the surface of the Fe3O4@UiO-66 core-shell material. Subsequently, solid-liquid separation was achieved by applying an external magnetic field, and after multiple washings with deionized water, it was dried at 50℃ for 12h to obtain a magnetic mercury removal material coated with a phase transition lysozyme film.

[0075] The prepared thiol-modified metal organic framework magnetic mercury removal material is used to adsorb mercury ions in water:

[0076] 0.05 g of thiol-modified metal organic framework magnetic mercury removal material was added to 50 mL of a mercury solution with a concentration of 100 mg / L, and the mixture was shaken at 150 r / min for 24 hours in a constant temperature air bath shaker at 25±0.5°C to reach adsorption equilibrium. Subsequently, the composite material was separated by a magnet, and the supernatant was taken to determine the Hg2+ concentration. By calculation, the adsorption capacity of the magnetic adsorption material was 286.8 mg / g.

[0077] Comparative Example 1:

[0078] The material preparation method of Comparative Example 1 differs from the composite material preparation method in Example 1 only in that:

[0079] In Comparative Example 1, the process of putting the Fe3O4@UiO-66 core-shell material into the phase transition solution for coating was omitted, and a phase transition lysozyme film was not formed. Then, the mercury ions in the water were removed according to the steps of Example 1.

[0080] The adsorption capacities of mercury ions of the thiol-modified metal organic framework magnetic mercury removal materials prepared in Examples 1, 2 and 3 and the product obtained in Comparative Example 1 are summarized as follows, as shown in Table 1:

[0081] Table 1. Comparison of the effects of different magnetic materials in removing mercury ions in the present invention

[0082]

[0083] It can be seen from the adsorption capacity of mercury ions of Example 1 and Comparative Example 1 in Table 1 that, on the basis of Comparative Example 1, the embodiment further has a PTL film layer rich in thiol functional groups, which can significantly improve the adsorption capacity of the composite material for mercury ions.

[0084] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.

Claims

1. A method for preparing a thiol-modified metal organic framework magnetic mercury removal material, characterized in that: The following steps are involved: placing ferrosoferric oxide nanoparticles as seeds into a reaction solution to obtain a mixture, the reaction solution comprising zirconium tetrachloride, terephthalic acid, dimethylformamide, and glacial acetic acid; The mixture was ultrasonically treated in an ultrasonic bath for 30 minutes, and then transferred to a reaction kettle for heating and reaction, and then cooled to room temperature to obtain a polymer solution; The polymer solution was washed with dimethylformamide and methanol respectively to obtain Fe3O4@UiO-66 core-shell material; dissolving tris(2-carboxyethyl)phosphine hydrochloride in a tris(hydroxymethylaminomethane) buffer solution to obtain a salt solution, and adjusting the pH of the salt solution with a NaOH solution; The lysozyme is dissolved in a tris(hydroxymethyl)aminomethane) buffer solution to obtain an enzyme solution, and then the enzyme solution is mixed with an equal volume of a pH-adjusted salt solution to form a phase transition solution; The Fe3O4@UiO-66 core-shell material is immersed in the phase transition solution and dispersed to obtain a dispersion, wherein the dispersion is reacted at room temperature to allow an amyloid lysozyme film to adhere to the surface of the Fe3O4@UiO-66 core-shell material; The dispersion liquid after the reaction is subjected to solid-liquid separation to obtain a thiol-modified metal organic framework magnetic mercury removal material.

2. The method for preparing the thiol-modified metal organic framework magnetic mercury removal material according to claim 1, characterized in that: The ratio of the ferrosoferric oxide nanoparticles, the zirconium tetrachloride, the terephthalic acid, the dimethylformamide and the glacial acetic acid is 0.2-1 g: 0.5-1.5 g: 0.3-1.0 g: 50-100 mL: 4-16 mL.

3. The method for preparing the thiol-modified metal organic framework magnetic mercury removal material according to claim 1, characterized in that: The reaction temperature of the heating reaction is 150-200° C., and the reaction time is 10-12 hours.

4. The method for preparing the thiol-modified metal organic framework magnetic mercury removal material according to claim 1, characterized in that: Before the Fe3O4@UiO-66 core-shell material is immersed in the phase transition solution, the Fe3O4@UiO-66 core-shell material is subjected to ultrasonic treatment for 15 to 20 minutes.

5. A thiol-modified metal organic framework magnetic mercury removal material, characterized in that: The thiol-modified metal organic framework magnetic mercury removal material is prepared by the preparation method of the thiol-modified metal organic framework magnetic mercury removal material according to any one of claims 1 to 4.

6. Application of a thiol-modified metal organic framework magnetic mercury removal material, characterized in that: The thiol-modified metal organic framework magnetic mercury removal material of claim 5 is added to the mercury-containing aqueous solution to be treated, and oscillated at 150-180 r / min at a constant temperature of 25±0.5° C. until adsorption equilibrium is reached.

Citation Information

Patent Citations

  • Phenylboronic acid functionalized magnetic metal organic skeleton microsphere and its synthesis method and use

    CN108636359A

  • Magnetic nano adsorbent for adsorbing mercury ions and preparation and application thereof

    CN110142031A

  • Acid-resistant magnetic nano-material of phase-transition lysozyme coating as well as preparation method and application of acid-resistant magnetic nano-material

    CN116586041A

  • Carbon-doped membranes, methods of making same, and uses thereof

    WO2023224973A1