Solid-phase microextraction material based on C-UIO66-NH2-coated PAC as well as preparation method and application of solid-phase microextraction material

By preparing solid phase microextracting materials based on C-UIO66-NH2@PAC, the efficient and economic problems of earth odorin and 2-methyl isocyanin detection in water were solved, and high selectivity and stability were achieved, and traditional Cost and complexity issues in the method.

CN118904308APending Publication Date: 2024-11-08SHENYANG WATER QUALITY TESTING TECH DEV CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411157104.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently and economically detect earth odorin and 2-methyl isocyanin in water. Commercial solid phase microextraction materials are costly and have limited recycling times, and traditional methods require organic solvents and complex concentration processes.

Method used

Using solid phase microextraction material based on C-UIO66-NH2@PAC, the powder activated carbon was hydrothermal reaction with ZrCl4 and 2-aminoterephthalic acid in dimethylformamide to form UIO66-NH2@PAC, and then Carbonization, combined with stainless steel wire and binder to prepare a porous fiber material for efficient adsorption and detection of geosinophilin and 2-methyl isocyanin.

Benefits of technology

High selective detection of earth odorin and 2-methyl isocyanin in water is achieved. The material has high stability and reusability, and can remain efficient after 70 cycle tests without the need for organic solvents and concentration processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904308A_ABST
    Figure CN118904308A_ABST
Patent Text Reader

Abstract

The invention discloses a solid-phase microextraction material based on C-UIO66-NH2-coated PAC as well as a preparation method and application of the solid-phase microextraction material. The C-UIO66-NH2-coated PAC-based solid-phase microextraction material is a derived porous carbon material prepared by directly carbonizing UIO66-NH2-coated PAC, and has good stability and a porous structure. The C-UIO66-NH2-coated PAC is used as a solid-phase micro-extraction coating, the stainless steel SSW with the adhesive is rotated in the C-UIO66-NH2-coated PAC, then redundant solids are removed, curing is conducted, operation is repeated till the stable coating with the proper thickness can be formed, and the solid-phase micro-extraction material is obtained. The C-UIO66-NH2-coated PAC-based solid-phase microextraction material disclosed by the invention has excellent high selectivity on detection of geosmin and 2-methylisoborneol in water / domestic drinking water, and has relatively high stability and recoverability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid phase microextraction, and specifically relates to a preparation method and application of a solid phase microextraction material based on C-UIO66-NH2@PAC. Background Art

[0002] Metal-organic frameworks (MOFs) are porous crystalline materials formed by metal ions and organic ligands or clusters through coordination bonds, with hierarchical structures, permanent porosity and high adsorption capacity. MOFs can be used as sacrificial templates to prepare nano-metal oxide porous carbons with large adsorption capacity by direct carbonization, and the structural stability of the carbonized materials can be optimized by doping other elements in the MOFs material. UIO66-NH2 is a classic MOFs material, which is co-doped with Zr-N, so that it changes from hydrophobic to hydrophilic after carbonization, so that polar substances in water can be extracted efficiently and selectively. Carbonized MOFs have been designed and synthesized for various environmental applications.

[0003] The most common oxygen-containing functional groups on the surface of powdered activated carbon (PAC) are hydroxyl, carboxyl, lactone and phenolic hydroxyl. The presence of these functional groups provides conditions for composite with MOFs. In addition, activated carbon is also a porous structure, which can produce additional adsorption sites.

[0004] Geosmin and 2-methylisoborneol are volatile organic compounds secreted by actinomycetes and algae, and are the main factors causing odor problems on the water surface. Solid phase microextraction is one of the most effective ways to enrich trace organic matter, but the use of some commercial coatings is greatly restricted due to their high cost and limited recycling times. Therefore, it is necessary to find more efficient, sensitive and economical SPEM fiber materials to detect geosmin and 2-methylisoborneol in water.

[0005] In recent years, solid phase microextraction has been widely used in research fields such as food and environmental safety because it does not require organic solvents, does not require concentration, and is simple and easy to use. The analytical performance of the SPME fiber based on carbonized MOFs has high extraction efficiency, sufficient reproducibility, high sensitivity, and acceptable reusability. Therefore, it is very meaningful to prepare a SPEM fiber material based on C-UIO66-NH2@PAC. Summary of the invention

[0006] The purpose of the present invention is to provide a solid phase microextraction material based on C-UIO66-NH2@PAC for highly selective detection of geosmin and 2-methylisoborneol in water / drinking water.

[0007] The technical solution adopted by the present invention is: a solid phase microextraction material based on C-UIO66-NH2@PAC, which is a solid phase microextraction material prepared with C-UIO66-NH2@PAC as a coating.

[0008] A method for preparing a solid phase microextraction material based on C-UIO66-NH2@PAC comprises the following steps:

[0009] 1) Preparation of C-UIO66-NH2@PAC: Powdered activated carbon (PAC), ZrCl4 and 2-aminoterephthalic acid were dispersed in dimethylformamide, glacial acetic acid was added to adjust the reaction system to be acidic, and the mixture was stirred at room temperature for 1 to 2 hours. The mixture was placed in a reactor and subjected to a hydrothermal reaction to obtain UIO66-NH2@PAC solid. The obtained UIO66-NH2@PAC solid was placed in a tubular furnace and calcined to obtain C-UIO66-NH2@PAC material.

[0010] 2) dissolving the silicone sealant in cyclohexane to obtain an adhesive; immersing the substrate in the adhesive and immediately taking it out to form a thin adhesive layer; then placing the substrate covered with the thin adhesive layer into the C-UIO66-NH2@PAC material obtained in step 1), rotating it, and then taking it out, removing the excess solids adhering to the surface of the substrate, and then curing it;

[0011] 3) Repeat step 2) 3 to 5 times to obtain a solid phase microextraction material based on C-UIO66-NH2@PAC.

[0012] Furthermore, in step 1), the mass ratio of ZrCl4:2-aminoterephthalic acid is 1:1-1.5; the mass of the powdered activated carbon (PAC) is 1-3% of the total mass of ZrCl4 and 2-aminoterephthalic acid.

[0013] Furthermore, in step 1), the hydrothermal reaction is carried out at 115-125° C. for 20-24 hours.

[0014] Furthermore, in step 1), the calcination is performed by heating the temperature to 800-850° C. at a heating rate of 5-8° C. / min and keeping the temperature for 1-2 hours.

[0015] Furthermore, in step 2), the substrate is stainless steel wire (SSW).

[0016] Furthermore, in step 2), the curing is performed at 75 to 85° C. for 30 to 40 minutes.

[0017] The present invention provides an application of a C-UIO66-NH2@PAC-based solid phase microextraction material in detecting geosmin and 2-methylisoborneol in water or drinking water.

[0018] Furthermore, the method is as follows: the solid phase microextraction material based on C-UIO66-NH2@PAC is placed in the water sample and adsorbed at 70-80 °C for 50-60 min.

[0019] Furthermore, the adsorbed C-UIO66-NH2@PAC solid phase microextraction material was desorbed at 200-250 °C.

[0020] The beneficial effects of the present invention are:

[0021] 1. The present invention uses C-UIO66-NH2@PAC with good stability and porous structure as the solid phase microextraction coating, rotates the stainless steel wire (SSW) needle with adhesive in C-UIO66-NH2@PAC, and then gently blows away the excess solid with a rubber ball and solidifies; the above process is repeated 3 times until a stable coating with appropriate thickness can be formed to obtain the SPEM fiber material. The preparation method is simple.

[0022] 2. In the present invention, the prepared C-UIO66-NH2@PAC has a large specific surface area, high chemical stability and thermal stability.

[0023] 3. The solid phase microextraction material based on C-UIO66-NH2@PAC provided by the present invention has excellent high selectivity for the detection of geosmin and 2-methylisoborneol in water / drinking water. In addition, after 70 cycles of testing, the detection of geosmin and 2-methylisoborneol in water is still highly selective, and has high stability and recyclability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention.

[0025] Figure 2 This is the PXRD diagram of the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention.

[0026] Figure 3 This is a gas chromatogram of the selective adsorption of geosmin and 2-methylisoborneol by the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention.

[0027] Figure 4 This is the mass spectrum of the selective adsorption of geosmin and 2-methylisoborneol by the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention.

[0028] Figure 5 These are the graphs of seventy cycles of adsorption experiments on C-UIO66-NH2 (left) and C-UIO66-NH2@PAC-2% (right).

[0029] Figure 6 It is the test results of geosmin (GSM) and 2-methylisoborneol (2-MIB) by different extraction materials;

[0030] Among them, 1-UIO66-NH2, 2-UIO66-NH2@PAC-2%, 3-C-UIO66-NH2, 4-C-UIO66-NH2@PAC-2%, and 5-DVB / CAR / PDMS. DETAILED DESCRIPTION

[0031] Example 1 A solid phase microextraction material based on C-UIO66-NH2@PAC (I) Preparation method is as follows:

[0032] 1. Preparation of C-UIO66-NH2@PAC materials

[0033] 10.3 mg of powdered activated carbon (PAC) was co-dispersed with 0.250 g of ZrCl4 and 0.268 g of 2-aminoterephthalic acid (H2BDC-NH2) in 50 mL of dimethylformamide (DMF) to dissolve, and then 4 mL of glacial acetic acid was added to adjust the reaction system to be acidic. The mixture was stirred at room temperature for 1 hour, placed in a reactor, and subjected to a hydrothermal reaction in a vacuum oven at 120°C for 24 hours to obtain UIO66-NH2@PAC solid, which was marked as UIO66-NH2@PAC-2%. The obtained UIO66-NH2@PAC was placed in a tubular furnace, heated to 800°C at a heating rate of 5°C / min, and kept at 800°C for 1 hour, and finally the derived porous carbon material C-UIO66-NH2@PAC was obtained, which was marked as C-UIO66-NH2@PAC-2% and set aside.

[0034] 2. Pretreatment of stainless steel wire (SSW)

[0035] The stainless steel wire (SSW) was cut into 8 cm lengths, and ultrasonically treated in deionized water, methanol, and acetone for 15 min each to clean the surface substrate, and then dried in an oven at 60° C. for 1 h.

[0036] 3. Preparation of solid phase microextraction materials

[0037] 0.5 g of silicone sealant was dissolved in 1.9 mL of cyclohexane to obtain an adhesive; the cleaned SSW was immersed in the adhesive and immediately taken out to form a thin adhesive layer; the SSW with a thin adhesive layer was then rotated in the derived porous carbon material C-UIO66-NH2@PAC obtained in step 1 to make the C-UIO66-NH2@PAC material adhere to the SSW, and then the excess solid was gently blown off with a rubber ball, and then cured at 80°C for 30 minutes. This operation process was repeated 3 times until a stable coating with appropriate thickness was formed, and a C-UIO66-NH2@PAC-based solid phase microextraction material with a coating thickness of 60 μm was obtained.

[0038] (II) Testing

[0039] Figure 1 This is a scanning electron microscope (SEM) image of the solid phase microextraction material based on C-UIO66-NH2@PAC. The surface morphology and thickness of the solid phase microextraction material based on C-UIO66-NH2@PAC can be seen. The material distribution on the fiber surface is uniform and dense, and the coating thickness is about 60μm.

[0040] Figure 2 This is the X-ray diffraction pattern (PXRD) of the solid phase microextraction material based on C-UIO66-NH2@PAC, which shows that during the preparation process of the solid phase microextraction material based on C-UIO66-NH2@PAC, the structure of C-UIO-66-NH2 is not destroyed and the structure remains intact.

[0041] Example 2 Highly Selective Detection of Geosmin and 2-Methylisoborneol in Water / Drinking Water Using C-UIO66-NH2@PAC-Based Solid Phase Microextraction Material (I) Highly Selective Detection of Geosmin (GSM) and 2-Methylisoborneol (2-MIB) in Water / Drinking Water Using C-UIO66-NH2@PAC-Based Solid Phase Microextraction Material Prepared in Example 1

[0042] Here’s how:

[0043] The solid phase microextraction material based on C-UIO66-NH2@PAC was activated at 160 °C for 30 min under helium conditions before use.

[0044] Take 10mL of water sample containing geosmin and 2-methylisoborneol (geosmin concentration is 2ng / mL, 2-methylisoborneol concentration is 2ng / mL), insert it into the solid phase microextraction material based on C-UIO66-NH2@PAC, adsorb it at 70℃ for 50min, enrich it by solid phase microextraction, and then detect it by GC-MS. Finally, desorb it at 230℃ and reuse it.

[0045] Figure 3 The gas chromatogram of the selective adsorption of geosmin and 2-methylisoborneol by the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention. Figure 3 Comparing the left and right figures, it can be found that the solid phase microextraction material of C-UIO66-NH2@PAC can efficiently detect geosmin and 2-methylisoborneol.

[0046] Figure 4 This is the mass spectrum of the selective adsorption of geosmin and 2-methylisoborneol by the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention.

[0047] Depend on Figure 3 and Figure 4 It can be seen that the solid phase microextraction material of C-UIO66-NH2@PAC prepared in the present invention can efficiently detect geosmin and 2-methylisoborneol.

[0048] (II) Recycling of solid phase microextraction materials based on C-UIO66-NH2@PAC

[0049] The adsorbed C-UIO66-NH2@PAC solid phase microextraction material was desorbed at 230°C. Then, after activation at 160°C for 30 min under helium conditions, it could be used again to explore the reusability of the material.

[0050] Figure 5 The following is a graph showing seventy cycles of adsorption experiments on C-UIO66-NH2 (left) and C-UIO66-NH2@PAC-2% (right). Figure 5 It can be seen that after 70 cycles of the experiment, the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention still has a good extraction efficiency.

[0051] (III) Detection results of geosmin (GSM) and 2-methylisoborneol (2-MIB) using different extraction materials

[0052] Take 10mL of water sample containing geosmin and 2-methylisoborneol (geosmin concentration is 2ng / mL and 2-methylisoborneol concentration is 2ng / mL), insert different solid phase microextraction materials (UIO66-NH2, UIO66-NH2@PAC-2%, C-UIO66-NH2, C-UIO66-NH2@PAC-2% and DVB / CAR / PDMS), adsorb at 70℃ for 50min, enrich by solid phase microextraction, and then detect the solution by GC-MS. Finally, desorb at 230℃ and reuse.

[0053] Figure 6The following are the test results of geosmin (GSM) and 2-methylisoborneol (2-MIB) using different extraction materials. Figure 6 It can be seen that the solid phase microextraction material based on C-UIO66-NH2@PAC of the present invention has high selectivity for both geosmin (GSM) and 2-methylisoborneol (2-MIB).

Claims

1. A solid phase microextraction material based on C-UIO66-NH2@PAC, characterized in that: The solid phase microextraction material based on C-UIO66-NH2@PAC is a solid phase microextraction material prepared with C-UIO66-NH2@PAC as a coating.

2. The method for preparing a solid phase microextraction material based on C-UIO66-NH2@PAC according to claim 1, characterized in that: The preparation method comprises the following steps: 1) Preparation of C-UIO66-NH2@PAC: Powdered activated carbon PAC, ZrCl4 and 2-aminoterephthalic acid were dispersed in dimethylformamide, glacial acetic acid was added to adjust the reaction system to be acidic, and the mixture was stirred at room temperature for 1 to 2 hours. The mixture was placed in a reactor and subjected to a hydrothermal reaction to obtain UIO66-NH2@PAC solid. The obtained UIO66-NH2@PAC solid was placed in a tubular furnace and calcined to obtain C-UIO66-NH2@PAC material. 2) dissolving the silicone sealant in cyclohexane to obtain an adhesive; immersing the substrate in the adhesive and immediately taking it out to form a thin adhesive layer; then placing the substrate covered with the thin adhesive layer into the C-UIO66-NH2@PAC material obtained in step 1), rotating it, and then taking it out, removing the excess solids adhering to the surface of the substrate, and then curing it; 3) Repeat step 2) 3 to 5 times to obtain a solid phase microextraction material based on C-UIO66-NH2@PAC.

3. The preparation method according to claim 2, characterized in that: In step 1), the mass ratio of ZrCl4:2-aminoterephthalic acid is 1:1-1.5; the mass of the powdered activated carbon PAC is 1-3% of the total mass of ZrCl4 and 2-aminoterephthalic acid.

4. The preparation method according to claim 2, characterized in that: In step 1), the hydrothermal reaction is carried out at 115-125° C. for 20-24 hours.

5. The preparation method according to claim 2, characterized in that: In step 1), the calcination is performed by heating the temperature to 800-850° C. at a heating rate of 5-8° C. / min and keeping the temperature for 1-2 hours.

6. The preparation method according to claim 2, characterized in that: In step 2), the substrate is stainless steel wire SSW.

7. The preparation method according to claim 2, characterized in that: In step 2), the curing is performed at 75 to 85° C. for 30 to 40 minutes.

8. Use of a solid phase microextraction material based on C-UIO66-NH2@PAC as described in claim 1 in detecting geosmin and 2-methylisoborneol in water or drinking water.

9. The use according to claim 8, characterized in that: The method is as follows: the solid phase microextraction material based on C-UIO66-NH2@PAC is placed in the water sample and adsorbed at 70-80°C for 50-60 minutes.

10. The use according to claim 9, characterized in that: The adsorbed C-UIO66-NH2@PAC solid phase microextraction material was desorbed at 200-250 °C.

Citation Information

Patent Citations

  • Preparation method of carbon nanotube / UiO-66-NH2 nano-composite material

    CN109589932A

  • Solid-phase microextraction material based on UiO-66-NH2 as well as preparation method and application of solid-phase microextraction material

    CN116116395A

  • Preparation method of solid-phase microextraction coating and application of coating

    CN116413352A