Fe and Mo loaded waste wind turbine blade catalyst as well as preparation method and application thereof

Through the preparation and application of waste wind power blade catalysts loaded with Fe and Mo, the problem of difficult and high cost of waste wind power blade recycling process is solved, efficient waste water treatment and multi-cyclic organic pollutant degradation are achieved, and the catalyst is demonstrated. Efficient and reusable and environmentally friendly.

CN118904350AActive Publication Date: 2024-11-08GANSU ECO-ENVIRONMENTAL SCI & DESIGN INST +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410951600.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing waste wind power blade recycling technology has problems such as difficult and high cost, especially when dealing with thermoset composite materials, it is difficult to effectively recycle fibers and produce high-value products.

Method used

Using the preparation method of waste wind power blade catalyst loaded with Fe and Mo, by soaking waste wind power blades in solution A containing chitosan, acetic acid and water, then in a solution containing ferrous sulfate heptahydrate and ammonium molybdate tetrahydrate In B, the catalyst is dried and heat treated to form a Fe and Mo supported catalyst, and the catalyst is used for wastewater treatment in Fenton technology.

Benefits of technology

It significantly increases the adsorption amount of metal ions, forms a porous carbon framework, introduces magnetism, improves the reusability and catalytic efficiency of the catalyst, and can efficiently degrade polycyclic organic pollutants, such as tetracycline antibiotics, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904350A_ABST
    Figure CN118904350A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid waste treatment, and discloses a Fe and Mo loaded waste wind turbine blade catalyst as well as a preparation method and application thereof. Comprising the following steps that the waste wind power blade is sequentially soaked in a solution A and a solution B, and the treated waste wind power blade is obtained; the treated waste wind power blade is sequentially subjected to drying and heat treatment, and the waste wind power blade catalyst loaded with Fe and Mo is obtained. The material provided by the invention has excellent reusability, can be used for many times, and has basically unchanged catalytic efficiency. A porous carbon skeleton is formed during high-temperature carbonization of the material, and deposition of Fe and Mo is facilitated. The obtained catalyst is used for catalytically degrading polycyclic organic pollutants such as tetracycline antibiotics in wastewater, and hydrogen peroxide is adopted to generate hydroxyl radicals, so that the method is beneficial to environmental protection. The material provided by the invention has magnetism and can be conveniently separated from a solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid waste treatment, and in particular to a Fe- and Mo-loaded waste wind turbine blade catalyst, and a preparation method and application thereof. Background Art

[0002] With the continuous development of social economy and the continuous increase of energy consumption, the depletion of fossil energy and environmental pollution have become increasingly serious, which has promoted the adjustment of global energy structure, making renewable energy such as wind energy and solar energy gradually change from supplementary energy to alternative energy. Among them, wind energy, as an internationally recognized green renewable energy, has attracted much attention. Wind power generation, as a mature wind energy utilization solution, has been commercialized on a large scale and has strong market competitiveness in renewable energy generation.

[0003] my country has vast resources, especially rich wind power resources. Wind power generation plays an important role in adjusting my country's energy structure and promoting regional economic development. The rapid development of wind power has led to a large-scale increase in the frequency of use of wind turbine blade materials. According to statistics, a total of about 5,700 tons of retired blades were produced in my country in 2018, and it is predicted that 52,000 tons of retired blades will be produced by 2025. Therefore, how to rationally recycle and reuse them is a major problem facing the current wind power field.

[0004] Traditional treatment methods include open-air stacking, landfilling or incineration. However, open-air stacking and landfilling occupy a large area, and the toxic substances released will further pollute the soil and groundwater system while not rotting for a hundred years; direct incineration will produce a large amount of heat, toxic gases and smoke.

[0005] At present, the recycling technologies used for discarded blades mainly include mechanical recycling and chemical recycling. The mechanical recycling method is a method of secondary utilization of crushed waste composite materials as raw materials. For large composite materials such as wind turbine blades, their volume is large and they must be pre-cut before crushing. This recycling technology has low cost and simple process, and is widely used in the recycling of fiber-reinforced polymer composites. However, most of the recycled products obtained by this method are of low value, and the fibers are severely damaged during the recycling process, and long fibers cannot be obtained. The chemical recycling method uses chemical reagents to convert the resin matrix of the composite material into small molecules, thereby recovering the fibers. However, this recycling method has problems such as difficulty and high cost for the recycling of thermosetting composite materials.

[0006] Fenton technology is an advanced oxidation technology (AOPs) that has become increasingly important due to its potential effectiveness in treating organic pollutants, especially those that are resistant to biodegradation. The environmentally friendly and low-cost Fenton technology has its unique advantages as an oxidation method, including high degradation efficiency, simple operation and mild reaction conditions, but the technology of using waste wind turbine blades as catalysts in Fenton technology has not been reported.

[0007] Therefore, it is of great significance to study a method for preparing a Fe- and Mo-loaded waste wind turbine blade catalyst with low cost and simple process and to apply the prepared catalyst in Fenton technology. Summary of the invention

[0008] In view of this, the present invention provides a waste wind turbine blade catalyst loaded with Fe and Mo and a preparation method and application thereof, the purpose of which is to solve the technical problems of the existing waste wind turbine blade recycling process being difficult and costly.

[0009] In order to achieve the above object, the present invention adopts the following technical solution:

[0010] The present invention provides a method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo, comprising the following steps:

[0011] (1) soaking the waste wind turbine blades in solution A and solution B in sequence to obtain treated waste wind turbine blades;

[0012] (2) drying and heat treating the treated waste wind turbine blades in sequence to obtain Fe and Mo loaded waste wind turbine blade catalysts;

[0013] Wherein, solution A comprises chitosan, acetic acid and water; solution B comprises ferrous sulfate heptahydrate, ammonium molybdate tetrahydrate and water.

[0014] Preferably, in the solution A, the mass ratio of chitosan, acetic acid and water is 0.5-3:0.5-3:100.

[0015] Preferably, in the solution B, the molar ratio of ferrous sulfate heptahydrate to ammonium molybdate tetrahydrate is 15-20:0.8-1.6, and the concentration of ferrous sulfate heptahydrate is 0.5-2 mol / L.

[0016] Preferably, in step (1), the immersion is carried out under stirring, and the stirring speed is independently 800 to 1000 rpm.

[0017] Preferably, in step (1), the immersion time in solution A is 100 to 150 minutes, and the immersion time in solution B is 100 to 150 minutes.

[0018] Preferably, in step (2), the drying time is 10 to 12 hours and the drying temperature is 50 to 60°C.

[0019] Preferably, in step (2), the heat treatment is carried out under a protective atmosphere, the heat treatment temperature is 800-1000°C, the heat treatment time is 1.5-2.5h, and the heating rate from the drying temperature to the heat treatment temperature is 8.5-12°C / min.

[0020] The present invention also provides a waste wind turbine blade catalyst loaded with Fe and Mo obtained by the method for preparing the waste wind turbine blade catalyst loaded with Fe and Mo.

[0021] The present invention also provides the use of the Fe- and Mo-loaded waste wind turbine blade catalyst in wastewater treatment.

[0022] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention can significantly increase the adsorption amount of metal ions by soaking in chitosan solution.

[0024] (2) The present invention forms a porous carbon skeleton when the material is carbonized at high temperature, which is beneficial to the deposition of Fe and Mo.

[0025] (3) The present invention introduces magnetism into the catalyst, which is beneficial to the Fenton reaction of iron ions and hydrogen peroxide, and at the same time allows the material to be easily separated from the solution.

[0026] (4) The material of the present invention has excellent reusability and can be used multiple times with substantially unchanged catalytic efficiency.

[0027] (5) The catalyst obtained by the present invention is used to catalyze the degradation of polycyclic organic pollutants such as tetracycline antibiotics in wastewater, and hydrogen peroxide is used to generate hydroxyl radicals, which is beneficial to green environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0029] Figure 1 It is a schematic diagram of the process of the present invention;

[0030] Figure 2The XRD spectra of the Fe- and Mo-loaded waste wind turbine blade catalysts obtained in Examples 1 to 3 and the waste wind turbine blade catalyst obtained in Comparative Example 1;

[0031] Figure 3 This is a SEM image of the Fe- and Mo-loaded waste wind turbine blade catalyst obtained in Example 1, wherein the magnification of a is 1 μm, the magnification of b is 5 μm, and the magnification of c is 10 μm;

[0032] Figure 4 This is a SEM image of the Fe-loaded waste wind turbine blade catalyst obtained in Comparative Example 2, wherein the magnification of a is 1 μm, the magnification of b is 5 μm, and the magnification of c is 10 μm;

[0033] Figure 5 The UV-vis spectra at different time intervals when the Fe and Mo loaded waste wind turbine blade catalyst obtained in Example 1 catalyzes the degradation of tetracycline solution;

[0034] Figure 6 This is a graph showing the degradation efficiency of tetracycline by the Fe and Mo loaded waste wind turbine blade catalyst obtained in Examples 1 to 3 in a H2O2-based system;

[0035] Figure 7 This is a graph showing the reuse performance of the Fe- and Mo-loaded waste wind turbine blade catalyst obtained in Example 1;

[0036] Figure 8 This is a graph of the leaching amount of Fe and Mo from the waste wind turbine blade catalyst loaded with Fe and Mo obtained in Example 1 during use;

[0037] Fig. 9 This is a graph showing the removal efficiency of various antibiotics by the Fe- and Mo-loaded waste wind turbine blade catalyst obtained in Example 1 under the action of H2O2. DETAILED DESCRIPTION

[0038] The present invention provides a method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo, comprising the following steps:

[0039] (1) soaking the waste wind turbine blades in solution A and solution B in sequence to obtain treated waste wind turbine blades;

[0040] (2) drying and heat treating the treated waste wind turbine blades in sequence to obtain Fe and Mo loaded waste wind turbine blade catalysts;

[0041] Wherein, solution A comprises chitosan, acetic acid and water; solution B comprises ferrous sulfate heptahydrate, ammonium molybdate tetrahydrate and water.

[0042] In the present invention, the specification of the discarded wind turbine blades is preferably 1 cm×1 cm×1 cm.

[0043] In the solution A of the present invention, the mass ratio of chitosan, acetic acid and water is preferably 0.5-3:0.5-3:100, more preferably 1-2.5:1-2.5:100, and more preferably 1.5-2:1.5-2:100.

[0044] In the present invention, the acetic acid is used to help dissolve chitosan.

[0045] In the solution B of the present invention, the molar ratio of ferrous sulfate heptahydrate to ammonium molybdate tetrahydrate is preferably 15-20:0.8-1.6, more preferably 16-19:1-1.4, more preferably 17-18:1.2-1.3, and the concentration of ferrous sulfate heptahydrate is preferably 0.5-2 mol / L, more preferably 1-1.8 mol / L, more preferably 1.2-1.5 mol / L.

[0046] In step (1) of the present invention, the immersion is preferably carried out under stirring, and the stirring speed is independently preferably 800 to 1000 rpm, more preferably 850 to 950 rpm, and even more preferably 880 to 900 rpm.

[0047] In step (1) of the present invention, the immersion time in solution A is preferably 100 to 150 min, more preferably 110 to 140 min, and more preferably 120 to 130 min, and the immersion time in solution B is preferably 100 to 150 min, more preferably 110 to 140 min, and more preferably 120 to 130 min.

[0048] In step (2) of the present invention, the drying time is preferably 10 to 12 hours, more preferably 10.5 to 11.5 hours, more preferably 11 hours, and the drying temperature is preferably 50 to 60°C, more preferably 52 to 58°C, more preferably 55 to 56°C.

[0049] In step (2) of the present invention, the heat treatment is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen or helium. The heat treatment temperature is preferably 800-1000°C, more preferably 850-950°C, and more preferably 880-900°C. The heat treatment time is preferably 1.5-2.5h, and more preferably 2h. The heating rate from the drying temperature to the heat treatment temperature is preferably 8.5-12°C / min, more preferably 9-11.5°C / min, and more preferably 9.5-10°C / min.

[0050] The present invention also provides a waste wind turbine blade catalyst loaded with Fe and Mo obtained by the method for preparing the waste wind turbine blade catalyst loaded with Fe and Mo.

[0051] The present invention also provides the use of the Fe- and Mo-loaded waste wind turbine blade catalyst in wastewater treatment.

[0052] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0053] Example 1

[0054] Cut the discarded wind turbine blades into small cubes with a length, width and height of 1cm×1cm×1cm;

[0055] Chitosan, acetic acid and water in a mass ratio of 1:1:100 were mixed to obtain solution A; FeSO4·7H2O and (NH4)6Mo7O in an atomic ratio of Fe:Mo=2.5:1 were taken. 24 ·4H2O is mixed with water to form a solution, in which the concentration of FeSO4·7H2O is 1 mol / L, to obtain solution B;

[0056] Put an appropriate amount of small cubes into a three-necked flask, pour in solution A, and stir at a speed of 1000 rpm for 2 hours; after pouring out the solution, pour solution B into the three-necked flask, stir at a speed of 1000 rpm for 2 hours, and then take out the small cubes to obtain the treated waste wind turbine blades;

[0057] The treated waste wind turbine blades were dried at 60°C for 12 minutes, and then placed in a tubular furnace. In a N2 atmosphere, the temperature was raised to 900°C at a rate of 10°C / min, and burned for 2 hours. After that, the temperature was naturally cooled to obtain a waste wind turbine blade catalyst loaded with Fe and Mo, which was recorded as "Fe-Mo / PVC-900".

[0058] Example 2

[0059] Cut the discarded wind turbine blades into small cubes with a length, width and height of 1cm×1cm×1cm;

[0060] Chitosan, acetic acid and water in a mass ratio of 1:1:100 were mixed to obtain solution A; FeSO4·7H2O and (NH4)6Mo7O in an atomic ratio of Fe:Mo=2.5:1 were taken. 24 ·4H2O is mixed with water to form a solution, in which the concentration of FeSO4·7H2O is 1 mol / L, to obtain solution B;

[0061] Put an appropriate amount of small cubes into a three-necked flask, pour in solution A, and stir at a speed of 1000 rpm for 2 hours; after pouring out the solution, pour solution B into the three-necked flask, stir at a speed of 1000 rpm for 2 hours, and then take out the small cubes to obtain the treated waste wind turbine blades;

[0062] The treated waste wind turbine blades were dried at 60°C for 12 hours, and then placed in a tubular furnace. In a N2 atmosphere, the temperature was raised to 700°C at a rate of 10°C / min, and burned for 2 hours. After that, the temperature was naturally cooled to obtain a waste wind turbine blade catalyst loaded with Fe and Mo, which was recorded as "Fe-Mo / PVC-700".

[0063] Example 3

[0064] Cut the discarded wind turbine blades into small cubes with a length, width and height of 1cm×1cm×1cm;

[0065] Chitosan, acetic acid and water in a mass ratio of 1:1:100 were mixed to obtain solution A; FeSO4·7H2O and (NH4)6Mo7O in an atomic ratio of Fe:Mo=2.5:1 were taken. 24 ·4H2O is mixed with water to form a solution, in which the concentration of FeSO4·7H2O is 1 mol / L, to obtain solution B;

[0066] Put an appropriate amount of small cubes into a three-necked flask, pour in solution A, and stir at a speed of 1000 rpm for 2 hours. After pouring out the solution, pour solution B into the three-necked flask, stir at a speed of 1000 rpm for 2 hours, and then remove the small cubes to obtain the treated waste wind turbine blades;

[0067] The treated waste wind turbine blades were dried at 60°C for 12 hours, and then placed in a tubular furnace. In a N2 atmosphere, the temperature was raised to 500°C at a rate of 10°C / min, and burned for 2 hours. After that, the temperature was naturally cooled to obtain a waste wind turbine blade catalyst loaded with Fe and Mo, which was recorded as "Fe-Mo / PVC-500".

[0068] Comparative Example 1

[0069] Cut the discarded wind turbine blades into small cubes with a length, width and height of 1cm×1cm×1cm;

[0070] Chitosan, acetic acid and water were mixed in a mass ratio of 1:1:100 to obtain solution A;

[0071] Put an appropriate amount of small cubes into a three-necked flask, pour in solution A, and stir at a speed of 1000 rpm for 2 hours, remove the small cubes, and obtain the treated waste wind turbine blades;

[0072] The treated waste wind turbine blades were dried at 60°C for 12 hours, and then placed in a tubular furnace. In a N2 atmosphere, the temperature was raised to 900°C at a rate of 10°C / min, and burned for 2 hours. After that, the temperature was naturally cooled to obtain a waste wind turbine blade catalyst, which was recorded as "PVC-900".

[0073] Comparative Example 2

[0074] Cut the discarded wind turbine blades into small cubes with a length, width and height of 1cm×1cm×1cm;

[0075] Chitosan, acetic acid and water in a mass ratio of 1:1:100 were mixed to obtain solution A; FeSO4·7H2O was mixed with water to obtain solution B with a concentration of FeSO4·7H2O of 1 mol / L;

[0076] Put an appropriate amount of small cubes into a three-necked flask, pour in solution A, and stir at a speed of 1000 rpm for 2 hours. After pouring out the solution, pour solution B into the three-necked flask, stir at a speed of 1000 rpm for 2 hours, and then remove the small cubes to obtain the treated waste wind turbine blades;

[0077] The treated waste wind turbine blades were dried at 60°C for 12 hours, and then placed in a tubular furnace. In a N2 atmosphere, the temperature was raised to 900°C at a rate of 10°C / min, and burned for 2 hours. After that, the temperature was naturally cooled to obtain an Fe-loaded waste wind turbine blade catalyst, which was recorded as "Fe / PVC-900".

[0078] Performance Testing

[0079] 1. Degradation time

[0080] 0.18 g of Fe-Mo / PVC-900 obtained in Example 1 was added to 60 mL of wastewater containing tetracycline at a concentration of 20 mg / L, and 6.7 mL of H2O2 at a concentration of 10 mmol / L was added. After the addition of H2O2 was completed, the concentration of residual tetracycline in the solution was measured by an ultraviolet spectrophotometer at reaction times of 0 min, 3 min, 5 min, 10 min, 15 min, 25 min, 40 min, 60 min, 90 min and 120 min, respectively. The test results are as follows: Figure 5 shown.

[0081] The UV-vis spectra of the Fe and Mo-loaded waste wind turbine blade catalyst obtained in Example 1 at different time intervals when catalyzing the degradation of tetracycline solution are as follows: Figure 5 As shown. Figure 5 It can be seen that the two main absorption characteristic peaks at 358nm and 275nm gradually disappeared with the extension of reaction time, indicating that tetracycline in the wastewater has been fully degraded.

[0082] 2. Degradation efficiency

[0083] Take four groups of 60ml wastewater with a tetracycline concentration of 20mg / L, add 6.7mL of 10mmol / L H2O2, 6.7mL of 10mmol / L H2O2 and 0.18g Fe-Mo / PVC-900, 6.7mL of 10mmol / L H2O2 and 0.18g Fe-Mo / PVC-700, 6.7mL of 10mmol / L H2O2 and 0.18g Fe-Mo / PVC-500 to the four groups of wastewater for reaction, and use an ultraviolet spectrophotometer to determine the residual tetracycline concentration in the solution at reaction times of 0min, 3min, 5min, 10min, 15min, 25min, 40min, 60min, 90min and 120min, respectively. The test results are as follows: Figure 6 shown.

[0084] The degradation efficiency of the Fe and Mo-loaded waste wind turbine blade catalyst obtained in Examples 1 to 3 for tetracycline in a H2O2-based system is shown in the figure below: Figure 6 As shown. Figure 6 It can be seen that when only H2O2 exists in the wastewater, the degradation efficiency of tetracycline within 30 minutes is less than 5%. After adding Fe-Mo / PVC-500 and Fe-Mo / PVC-700 to the catalytic system, the degradation efficiency of tetracycline within 30 minutes reaches 23% and 42%, respectively. After adding Fe-Mo / PVC-900 to the catalytic system, the degradation efficiency of tetracycline within 30 minutes can reach more than 85%.

[0085] 3. Reusability

[0086] 0.18 g of Fe-Mo / PVC-900 obtained in Example 1 was added to 60 mL of wastewater containing tetracycline at a concentration of 20 mg / L, and 6.7 mL of H2O2 at a concentration of 10 mmol / L was added. After the addition of H2O2 was completed, the residual tetracycline concentration in the solution was measured by an ultraviolet spectrophotometer after reacting for 2 hours, and then an ordinary magnet was added to the degraded wastewater to separate Fe-Mo / PVC-900 from the wastewater;

[0087] Repeat the above operation for the separated Fe-Mo / PVC-900 to obtain Figure 7 The reuse performance of the Fe and Mo loaded waste wind turbine blade catalyst obtained in Example 1 is shown in the figure below: Figure 7 As shown. Figure 7 It can be seen that after the Fe-Mo / PVC-900 catalyst was used for ten consecutive cycles, the removal rate of tetracycline could still reach more than 87%.

[0088] 4. Leaching amount of Fe and Mo

[0089] (1) Fe leaching amount

[0090] 15 mL of the wastewater after 1-10 cycles of degradation in the reuse performance test was taken to obtain ten groups of samples. 5 mL of buffer solution (164 g of sodium acetate was dissolved in water, and 84 mL of acetic acid was added to dilute the solution to 1000 mL), 1 mL of 20 g / L ascorbic acid solution, and 1 mL of 2 g / L 1,10-phenanthroline solution were added to the ten groups of samples respectively, and a drop of 10-fold diluted hydrochloric acid solution was added to adjust the pH value. After reacting for 20 minutes, the Fe content in the ten groups of samples was determined by a UV spectrophotometer.

[0091] (2) Mo leaching amount

[0092] Take 20 mL of each wastewater after 1-10 cycles of degradation in the reuse performance test to obtain ten groups of samples. Add 3 mL of 1+1H2SO4 solution diluted with water to 30 mL, 1 mL of 1.2570 g / L copper sulfate solution, 3 mL of 100 g / L ascorbic acid solution, 8 mL of 250 g / L potassium thiocyanate solution, and then add water to 50 mL to the ten groups of samples. After reacting for 20 minutes, use an ultraviolet spectrophotometer to determine the Mo content in the ten groups of samples.

[0093] The leaching amount of Fe and Mo from the waste wind turbine blade catalyst loaded with Fe and Mo obtained in Example 1 during use is shown in the following figure: Figure 8 As shown. Figure 8 It can be seen that after Fe-Mo / PVC-900 was reused ten times, the leaching amount of Fe and Mo ions gradually decreased. After being reused five times, the leaching amount of Mo ions was less than 0.03 mg / L. After being reused ten times, the leaching amount of Fe ions was less than 0.025 mg / L.

[0094] 5. Removal efficiency of various antibiotics

[0095] 0.18 g of Fe-Mo / PVC-900 obtained in Example 1 was added to 60 mL of wastewater containing tetracycline (TC) at a concentration of 20 mg / L, 60 mL of wastewater containing oxytetracycline (OTC) at a concentration of 20 mg / L, 60 mL of wastewater containing ciprofloxacin (CIP) at a concentration of 20 mg / L, and 60 mL of wastewater containing norfloxacin (FPA) at a concentration of 20 mg / L, and 6.7 mL of H2O2 at a concentration of 10 mmol / L was added respectively. After the addition of H2O2 was completed, the concentrations of tetracycline, oxytetracycline, ciprofloxacin, and norfloxacin residual in the solution were determined by an ultraviolet spectrophotometer during the reaction for 120 min. The test results are as follows: Fig. 9 shown.

[0096] The removal efficiency of various antibiotics by the Fe and Mo loaded waste wind turbine blade catalyst obtained in Example 1 under the action of H2O2 is shown in the figure below: Fig. 9 As shown. Fig. 9 It can be seen that the removal rates of tetracycline, oxytetracycline, ciprofloxacin and norfloxacin by Fe-Mo / PVC-900 catalyst under the action of H2O2 can reach 94.00%, 90.00%, 84.71% and 91.00% respectively.

[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo, characterized in that: The following steps are involved: (1) soaking the waste wind turbine blades in solution A and solution B in sequence to obtain treated waste wind turbine blades; (2) drying and heat treating the treated waste wind turbine blades in sequence to obtain Fe and Mo loaded waste wind turbine blade catalysts; Wherein, solution A comprises chitosan, acetic acid and water; solution B comprises ferrous sulfate heptahydrate, ammonium molybdate tetrahydrate and water.

2. The method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo according to claim 1, characterized in that: In the solution A, the mass ratio of chitosan, acetic acid and water is 0.5-3:0.5-3:

100.

3. The method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo according to claim 2, characterized in that: In the solution B, the molar ratio of ferrous sulfate heptahydrate to ammonium molybdate tetrahydrate is 15-20:0.8-1.6, and the concentration of ferrous sulfate heptahydrate is 0.5-2 mol / L.

4. The method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo according to claim 2 or 3, characterized in that: In the step (1), the immersion is carried out under stirring, and the stirring speed is independently 800 to 1000 rpm.

5. The method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo according to claim 4, characterized in that: In the step (1), the immersion time in solution A is 100 to 150 minutes, and the immersion time in solution B is 100 to 150 minutes.

6. The method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo according to claim 5, characterized in that: In the step (2), the drying time is 10 to 12 hours and the drying temperature is 50 to 60°C.

7. The method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo according to claim 6, characterized in that: In the step (2), the heat treatment is carried out under a protective atmosphere, the heat treatment temperature is 800-1000° C., the heat treatment time is 1.5-2.5 hours, and the heating rate from the drying temperature to the heat treatment temperature is 8.5-12° C. / min.

8. A waste wind turbine blade catalyst loaded with Fe and Mo obtained by the method for preparing a waste wind turbine blade catalyst loaded with Fe and Mo as described in any one of claims 1 to 7.

9. Use of the Fe and Mo loaded waste wind turbine blade catalyst according to claim 8 in wastewater treatment.

Citation Information

Patent Citations

  • Visible-light-induced photocatalyst for degrading dye in wastewater as well as preparation method and application thereof

    CN112642463A

  • Method for preparing denitration catalyst by utilizing waste wind turbine blade and application of denitration catalyst

    CN115624968A

  • Water treatment catalyst based on monatomic configuration and preparation method and application thereof

    CN117718072A

  • Catalysts for fenton system containing metal oxide containing functional group on surface and fenton system using the same

    EP3885035A1