Method for rapidly preparing AlON ceramic powder, AlON-CeO2 composite photocatalyst and application of AlON-CeO2 composite photocatalyst
By simplifying the production process of AlON photocatalyst, using the combination technology of phenolic resin and nanoγ-Al2O3 powder, an efficient AlON ceramic powder was quickly prepared, and AlON photocatalyst was solved by compounding with CeO2 to form AlON@CeO2 composite photocatalyst. The high production cost and low efficiency of catalysts have achieved efficient degradation of industrial printing and dyeing wastewater pollutants.
Patent Information
- Application Number
- CN202410959387.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The production process of existing AlON photocatalysts is complex and time-consuming, resulting in high production costs and limiting their application.
Thermoset phenolic resin and nano-γ-Al2O3 powder are used to form γ-Al2O3/PF precursor through ultrasonic dispersion and magnetic stirring. AlON ceramic powder is prepared through one-step heating-up carbon-thermal reduction and nitriding reaction, reducing the reaction temperature and time and simplifying the process flow .
The production cost of AlON ceramic powder with high uniformity is achieved quickly and low energy consumption, which reduces production costs and improves the synthesis efficiency of AlON photocatalysts. By compounding with CeO2, the AlON@CeO2 composite photocatalysts are significantly improved. The degradation capacity of pollutants in printing and dyeing wastewater.
Smart Images

Figure CN118904379A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of AlON ceramic powder preparation and photocatalysis, and in particular to a method for rapidly preparing AlON ceramic powder, an AlON@CeO2 composite photocatalyst and applications thereof. Background Art
[0002] The rise and outbreak of the Industrial Revolution has driven rapid economic development, but it has also brought about global environmental pollution and ecological crises, especially the water pollution problem that needs to be solved most urgently. Various toxic pollutants exist, accumulate and spread in water for a long time, seriously endangering human health and ecological balance. Industrial printing and dyeing wastewater contains various toxic organic pollutants, which are difficult to be naturally degraded by organisms, and are easy to cause cancer and deformity of organisms after enrichment in organisms. Among them, Rhodamine B is a dye widely used in textile, printing and dyeing, biology, medicine and papermaking industries. Due to its strong toxicity, carcinogenicity, mutagenicity and difficulty in biodegradability, the degradation of Rhodamine B has become a key task in the treatment of industrial printing and dyeing wastewater.
[0003] Traditional methods to solve industrial printing and dyeing organic wastewater include physical and chemical methods. The physical method is to remove pollutants from wastewater through physical separation and adsorption. The chemical method uses an oxidant to oxidize and decompose organic pollutants into carbon dioxide and water, or uses a reducing agent to reduce oxygen-containing organic pollutants into inorganic substances to reduce the toxicity and difficulty of degradation of organic matter. However, the instruments and equipment required for the physical method are expensive and cannot achieve the expected benefits; the chemical method uses a variety of means for treatment, and the investment of drugs and energy is more, the cost is high, and it cannot achieve a popular effect. The photocatalytic method can use photocatalysts to absorb light energy under ultraviolet light to excite internal electrons and holes, and form active groups with high oxidation ability on the surface (such as ·OH hydroxyl radicals and ·O2-superoxide radicals, etc.), which react with organic matter in wastewater to degrade it into harmless substances. The photocatalytic method has the advantages of energy saving and high efficiency, and has a good effect on treating organic pollutants in wastewater.
[0004] As an emerging photocatalyst, AlON has the advantages of cheap synthetic raw materials, high catalytic efficiency, non-toxicity and no secondary pollution, and has great application potential. However, at present, AlON photocatalysts are basically prepared by carbon powder and alumina powder through carbon thermal reduction nitridation reaction, which usually requires long-term ball milling mixing and long-term carbon thermal reduction nitridation reaction, increasing the production cost of AlON photocatalysts and limiting the development and application of AlON photocatalysts.
[0005] Therefore, it is necessary to improve the AlON photocatalyst synthesis process and shorten the preparation time of raw materials. Under the premise of ensuring uniform mixing of raw materials, the carbon thermal reaction temperature can be reduced, the reaction time can be shortened, and AlON powder can be prepared quickly with low energy consumption, so as to provide a feasible method for realizing the application of AlON photocatalysts. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, one of the purposes of the present invention is to provide a method for quickly preparing AlON ceramic powder to solve the problems in traditional technology. It shortens the preparation time of raw materials, reduces the carbon thermal reaction temperature and shortens the reaction time while ensuring uniform mixing of the raw materials, and prepares AlON powder quickly with low energy consumption, thereby providing a feasible method for realizing the application of AlON photocatalysts.
[0007] The second object of the present invention is to provide an AlON@CeO2 composite photocatalyst prepared by combining the AlON ceramic powder obtained above with CeO2, which has a high photocatalytic degradation ability.
[0008] The third object of the present invention is to provide an application of the above-mentioned AlON@CeO2 composite photocatalyst in degrading pollutants such as rhodamine B, methylene orange, and methylene blue in industrial printing and dyeing wastewater, which has the advantages of energy saving and high efficiency, and has a good effect on treating pollutants such as rhodamine B, methylene orange, and methylene blue in wastewater.
[0009] One of the purposes of the present invention is achieved by the following technical solution:
[0010] A method for rapidly preparing AlON ceramic powder comprises the following steps:
[0011] S1: dissolving phenolic resin in anhydrous ethanol to prepare a phenolic resin ethanol solution; adding nano-γ-Al2O3 powder to the phenolic resin ethanol solution, and obtaining a raw material mixture slurry after ultrasonic dispersion and stirring;
[0012] S2: The uniformly stirred raw material mixture slurry is heated, dried and solidified to completely volatilize the ethanol in the slurry and solidify the phenolic resin on the surface of the nano γ-Al2O3 powder to obtain a γ-Al2O3 / PF precursor mixture;
[0013] S3: subjecting the γ-Al2O3 / PF precursor mixture to a one-step carbon thermal reduction nitridation reaction and heat preservation to obtain a single-phase AlON photocatalyst, i.e., AlON ceramic powder.
[0014] In the preparation of the AlON ceramic powder of the present invention, a thermosetting phenolic resin is used as an organic polymer and a carbon source, a nano-γ-Al2O3 powder is used as an aluminum source, and anhydrous ethanol is used as a slurry dispersant. The γ-Al2O3 / PF precursor mixture is prepared by ultrasonic dispersion-magnetic stirring-in-situ curing, and the AlON ceramic powder, i.e., the AlON photocatalyst, is synthesized through a carbon thermal reduction nitridation reaction. The addition of the thermosetting phenolic resin makes it simpler and more efficient to fully mix the carbon source and the aluminum source. After heating, the thermosetting phenolic resin is in-situ cured on the surface of the γ-Al2O3 powder to form a precursor mixture with a "core-shell" structure. The precursor raw material of this structure helps to improve the uniformity of raw material mixing, greatly reduces the mass transfer distance of the carbon thermal reduction nitridation reaction, increases the reaction activity of the raw material, can effectively reduce the reaction temperature of the carbon thermal reduction nitridation reaction, shorten the reaction time, and improve the efficiency of synthesizing the AlON photocatalyst powder.
[0015] Furthermore, in step S1, the phenolic resin is a thermosetting phenol-formaldehyde resin, which is synthesized by reacting phenol with excess formaldehyde under alkaline conditions.
[0016] Furthermore, in step S1, the nano γ-Al2O3 powder is γ-Al2O3 powder with an average particle size of 10-50nm and a purity of 99.99%.
[0017] Furthermore, in step S1, the mass ratio of the anhydrous ethanol, the phenolic resin, and the nano-γ-Al2O3 powder is 30:(0.8-1):5, such as 30:0.8:5, 30:0.85:5, 30:0.9:5, 30:0.95:5, 30:1:5, etc.
[0018] Further, in step S1, the ultrasonic dispersion time is 20min-40min; the stirring is magnetic stirring, the speed of magnetic stirring is 800rpm-1500rpm, and the time is 20min-40min. Further preferably, the ultrasonic dispersion time is 30min; the stirring is magnetic stirring, the speed of magnetic stirring is 1000rpm, and the time is 30min.
[0019] Further, in step S2, the specific steps of heating, drying and curing treatment include the following:
[0020] (1) Perform the first step of heating, drying and curing treatment at a temperature of 70-90°C for 2h-4h;
[0021] (2) The second step of heating, drying and curing treatment is carried out at a temperature of 180-220°C for 2h-4h.
[0022] Further preferably, the specific steps of heating, drying and curing treatment include the following:
[0023] (1) Performing the first step of heating, drying and curing treatment at a temperature of 80° C. for 3 hours;
[0024] (2) The second step of heating, drying and curing treatment is carried out at a temperature of 180-220°C for 3 hours.
[0025] Further, in step S3, in the one-step temperature-raising carbon thermal reduction nitridation reaction, the heating rate is 6-12°C / min, the reaction temperature is 1700-1800°C, the insulation time is 8-15min, and the reaction atmosphere is a nitrogen environment.
[0026] Further preferably, in the one-step temperature-raising carbon thermal reduction nitridation reaction, the heating rate is 10° C. / min, the reaction temperature is 1700-1800° C., the holding time is 10 min, and the reaction atmosphere is a nitrogen environment.
[0027] The second object of the present invention is achieved by adopting the following technical solution:
[0028] An AlON@CeO2 composite photocatalyst comprises the following steps:
[0029] The AlON ceramic powder obtained above is mixed with the nano CeO2 powder by ball milling to obtain the AlON@CeO2 composite photocatalyst.
[0030] Furthermore, in the AlON@CeO2 composite photocatalyst, the content of nano-CeO2 powder is 25-50wt%, such as 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, etc.
[0031] Furthermore, the grinding balls used in ball milling are high-purity alumina balls, the ball milling method used is wet ball milling, the dispersion medium of wet ball milling is anhydrous ethanol, the ball milling speed is 150-300 rpm, and the ball milling time is 20-30 hours.
[0032] More preferably, the ball milling speed is 200 rpm and the ball milling time is 24 h.
[0033] The third object of the present invention is achieved by adopting the following technical solution:
[0034] An application, characterized in that the AlON@CeO2 composite photocatalyst described above is used to degrade pollutants in industrial printing and dyeing wastewater, and the pollutants include one or more of rhodamine B, methylene orange, and methylene blue.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The method for rapidly preparing AlON ceramic powder of the present invention utilizes thermosetting phenolic resin as a carbon source, nano-γ-Al2O3 powder as an aluminum source, and ethanol as a dispersion medium. The slurry is evenly mixed by ultrasonic dispersion and magnetic stirring, and the phenolic resin is in situ cured on the surface of the nano-γ-Al2O3 powder while the slurry is drying by heating to form a γ-Al2O3 / PF precursor mixture with a "core-shell" structure. After a step of carbon thermal reduction nitridation reaction at a high temperature, a single-phase AlON powder with photocatalytic ability can be synthesized. The method improves the AlON photocatalyst synthesis process and shortens the preparation time of raw materials. On the premise of ensuring uniform mixing of the raw materials, the carbon thermal reaction temperature is reduced, the reaction time is shortened, and AlON powder is prepared quickly with low energy consumption, thereby providing a feasible method for realizing the application of AlON photocatalysts.
[0037] 2. The raw material cost of the present invention is low. The precursor is prepared only by ultrasonic dispersion, magnetic stirring and heating curing. It is not only simple to operate, but also can prepare a precursor mixture with uniform raw material mixing and high reaction activity. At the same time, the precursor mixture only needs a one-step heating process to synthesize a single-phase AlON photocatalyst powder. It has the advantages of low raw material cost, simple preparation process, low reaction energy consumption, etc. It can realize low-cost, simple and efficient large-scale engineering preparation of AlON photocatalyst powder, and can promote the application of AlON photocatalyst. The AlON photocatalyst powder and nano-CeO2 powder can be mixed by ball milling to obtain an AlON@CeO2 composite photocatalyst, which can greatly improve the catalytic degradation ability of the AlON photocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The XRD phase results of the powder products A2, B2, C2 and F2 prepared in Examples 1-3 and Comparative Example 1;
[0039] Figure 2 TEM photos and electron diffraction patterns of the γ-Al2O3 / PF precursor mixture C1 prepared in Example 3, wherein (a) and (b) are TEM photos, and (c) is an electron diffraction pattern;
[0040] Figure 3 The degradation efficiency curve of the photocatalysts C3, D, E and G prepared in Examples 3-5 and Comparative Example 2 under ultraviolet light irradiation for photocatalytic degradation of Rhodamine B solution;
[0041] Figure 4 These are photos of the AlON@CeO2 composite photocatalyst powder D prepared in Example 4 catalyzing the degradation of Rhodamine B solution under ultraviolet light for different times and a graph showing the change in concentration of the Rhodamine B solution. DETAILED DESCRIPTION
[0042] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0044] In the following examples, the nano-γ-Al2O3 powder is a γ-Al2O3 powder with an average particle size of 10-50 nm and a purity of 99.99%.
[0045] Example 1: Powder A2
[0046] (1) Preparation of raw material mixture slurry: 50 g of nano-γ-Al2O3 powder and 8 g of thermosetting phenolic resin were added to 300 g of ethanol, and then ultrasonicated for 30 min and stirred at 1000 rpm for 30 min to obtain a mixture slurry A0 in which the powder was evenly dispersed;
[0047] (2) Preparation of precursor mixture: The uniformly dispersed raw material mixture slurry A0 was placed in an oven at 80°C and kept for 3 hours, and then placed on a heating plate at 180°C for curing. After being kept for 3 hours, the γ-Al2O3 / PF precursor mixture A1 was obtained.
[0048] (3) Preparation of AlON powder: The γ-Al2O3 / PF precursor mixture A1 was placed in a vertical graphite high-temperature atmosphere furnace. Under a flowing nitrogen environment and a pressure of 0.2-0.4 KPa, the temperature was raised to 1800°C at a rate of 10°C / min and kept at that temperature for 10 min to obtain powder A2.
[0049] Depend on Figure 1 It can be seen that the powder is a single-phase AlON powder.
[0050] Example 2: Powder B2
[0051] (1) Preparation of raw material mixture slurry: 50 g of nano-γ-Al2O3 powder and 9 g of thermosetting phenolic resin were added to 300 g of ethanol, and then ultrasonicated for 30 min and stirred at 1000 rpm for 30 min to obtain a mixture slurry B0 in which the powder was evenly dispersed;
[0052] (2) Preparation of precursor mixture: The uniformly dispersed raw material mixture slurry B0 was placed in an oven at 80°C and kept for 3 hours, and then placed on a hot plate at 200°C for curing. After being kept for 3 hours, a γ-Al2O3 / PF precursor mixture B1 was obtained.
[0053] (3) Preparation of AlON powder: The γ-Al2O3 / PF precursor mixture B1 was placed in a vertical graphite high-temperature atmosphere furnace. Under a flowing nitrogen environment and a pressure of 0.2-0.4 KPa, the temperature was raised to 1750°C at a rate of 10°C / min and kept at that temperature for 10 min to obtain powder B2.
[0054] Depend on Figure 1 It can be seen that the powder is a single-phase AlON powder.
[0055] Example 3: Powder C2 and AlON photocatalyst powder C3
[0056] (1) Preparation of raw material mixture slurry: 50 g of nano-γ-Al2O3 powder and 10 g of thermosetting phenolic resin were added to 300 g of ethanol, and then ultrasonicated for 30 min and stirred at 1000 rpm for 30 min to obtain a mixture slurry C0 in which the powder was evenly dispersed;
[0057] (2) Preparation of precursor mixture: The uniformly dispersed raw material mixture slurry C0 was placed in an oven at 80°C for 3 h, and then placed on a hot plate at 220°C for curing. After being kept for 3 h, a γ-Al2O3 / PF precursor mixture C1 (from Figure 2 From the TEM photo and electron diffraction pattern of the precursor mixture C1, it can be seen that the precursor presents a "core-shell" structure in which phenolic resin is coated on the surface of γ-Al2O3 powder).
[0058] (3) Preparation of AlON powder: The γ-Al2O3 / PF precursor mixture C1 was placed in a vertical graphite high-temperature atmosphere furnace, and heated to 1700°C at a rate of 10°C / min under a flowing nitrogen environment and a pressure of 0.2-0.4 KPa. The mixture was kept at this temperature for 10 min to obtain powder C2. Figure 1 It can be seen that the powder is a single-phase AlON powder.
[0059] (4) Preparation of photocatalyst: Weigh 10 g of AlON powder C2 in a ball mill, use high-purity alumina balls as grinding balls, anhydrous ethanol as dispersion medium, and ball mill at a ball mill speed of 200 rpm for 24 h. After drying at 200°C for 24 h, AlON photocatalyst powder C3 is obtained.
[0060] (5) Photocatalytic degradation of Rhodamine B: 50 mg of AlON photocatalyst powder C3 was added to 40 ml of contaminated water (Rhodamine B concentration in contaminated water was 10 mg / L). After adsorption in a dark room for 30 min, a 500 W xenon lamp (λ>420 nm) was used as the light source, which was placed 15 cm away from the reactor. The reaction was carried out at room temperature of 25 °C for photocatalytic degradation of Rhodamine B.
[0061] The photocatalytic degradation efficiency curve of this embodiment is as follows: Figure 3 The degradation rates are shown in Table 1.
[0062] Example 4: AlON / CeO2 composite photocatalyst powder D
[0063] (1) Weigh 7.5 g of the AlON powder C2 prepared in Example 3 and 2.5 g of nano-CeO2 powder in a ball mill, use high-purity alumina balls as grinding balls, and anhydrous ethanol as a dispersion medium. After ball milling at a ball mill speed of 200 rpm for 24 h, the AlON@CeO2 composite photocatalyst powder D is obtained after drying at 200°C for 24 h.
[0064] (2) Photocatalytic degradation of Rhodamine B: 50 mg of AlON@CeO2 composite photocatalyst powder D was added to 40 ml of contaminated water (Rhodamine B concentration in contaminated water was 10 mg / L). After adsorption in a dark room for 30 min, a 500 W xenon lamp (λ>420 nm) was used as the light source, placed 15 cm away from the reactor, and the photocatalytic degradation of Rhodamine B was carried out at room temperature of 25 °C.
[0065] The photocatalytic degradation efficiency curve of this embodiment is as follows: Figure 3 The degradation rates are shown in Table 1.
[0066] Example 5: AlON / CeO2 composite photocatalyst powder E
[0067] (1) Weigh 5 g of the AlON powder C2 prepared in Example 3 and 5 g of nano-CeO2 powder in a ball mill, use high-purity alumina balls as grinding balls, anhydrous ethanol as dispersion medium, and ball mill at a ball mill speed of 200 rpm for 24 h. After drying at 200°C × 24 h, AlON@CeO2 composite photocatalyst powder E was obtained.
[0068] (2) Photocatalytic degradation of Rhodamine B: 50 mg of AlON@CeO2 composite photocatalyst powder E was added to 40 ml of contaminated water (Rhodamine B concentration in contaminated water was 10 mg / L). After adsorption in a dark room for 30 min, a 500 W xenon lamp (λ>420 nm) was used as the light source, which was placed 15 cm away from the reactor, and the photocatalytic degradation of Rhodamine B was carried out at room temperature of 25 °C.
[0069] The photocatalytic degradation efficiency curve of Rhodamine B in this example is as follows: Figure 3 The degradation rates are shown in Table 1.
[0070] (3) Photocatalytic degradation of methylene orange: 50 mg of AlON@CeO2 composite photocatalyst powder E was added to 40 ml of contaminated water (methylene orange concentration in contaminated water was 10 mg / L), and after adsorption in a dark room for 30 min, a 500 W xenon lamp (λ>420 nm) was used as a light source, placed 15 cm away from the reactor, and photocatalytic degradation of methylene orange was performed at room temperature of 25°C. The degradation rate of this example is shown in Table 2.
[0071] (4) Photocatalytic degradation of methylene blue: 50 mg of AlON@CeO2 composite photocatalyst powder E was added to 40 ml of contaminated water (methylene blue concentration in contaminated water was 10 mg / L), and after adsorption in a dark room for 30 min, a 500 W xenon lamp (λ>420 nm) was used as a light source, placed 15 cm away from the reactor, and photocatalytic degradation of methylene blue was performed at room temperature of 25°C. The degradation rate of this example is shown in Table 2.
[0072] Comparative Example 1: Powder F2
[0073] (1) Preparation of raw material mixture slurry: 50 g of nano-γ-Al2O3 powder and 10 g of thermosetting phenolic resin were added to 300 g of ethanol, and then ultrasonicated for 30 min and stirred at 1000 rpm for 30 min to obtain a mixture slurry F0 in which the powder was evenly dispersed;
[0074] (2) Preparation of precursor mixture: The uniformly dispersed raw material mixture slurry F0 was placed in an oven at 80°C and kept for 3 hours, and then placed on a hot plate at 220°C for curing. After being kept for 3 hours, a γ-Al2O3 / PF precursor mixture F1 was obtained.
[0075] (3) Preparation of AlON powder: The γ-Al2O3 / PF precursor mixture F1 was placed in a vertical graphite high-temperature atmosphere furnace. Under a flowing nitrogen environment and a pressure of 0.2-0.4 KPa, the temperature was raised to 1700°C at a rate of 10°C / min and kept at that temperature for 0 min to obtain powder F2.
[0076] Depend on Figure 2 It can be seen that the phases of the powder are AlON and AlN.
[0077] Comparative Example 2: AlON / CeO2 composite photocatalyst powder G
[0078] (1) Weigh 2.5 g of the AlON powder C2 prepared in Example 3 and 7.5 g of nano-CeO2 powder in a ball mill, use high-purity alumina balls as grinding balls, and anhydrous ethanol as a dispersion medium. After ball milling at a ball mill speed of 200 rpm for 24 h, the AlON@CeO2 composite photocatalyst powder G is obtained after drying at 200°C for 24 h.
[0079] (2) Photocatalytic degradation of Rhodamine B: 50 mg of AlON@CeO2 composite photocatalyst powder G was added to 40 ml of contaminated water (Rhodamine B concentration in contaminated water was 10 mg / L). After adsorption in a dark room for 30 min, a 500 W xenon lamp (λ>420 nm) was used as the light source, which was placed 15 cm away from the reactor, and the photocatalytic degradation of Rhodamine B was carried out at room temperature of 25 °C.
[0080] The photocatalytic degradation efficiency curve of this embodiment is as follows: Figure 3 The degradation rates are shown in Table 1.
[0081] Table 1 Degradation rate of Rhodamine B
[0082] project Degradation rate (%) Example 3 40.2 Example 4 77.3 Example 5 75.2 Comparative Example 2 56.2
[0083] It can be seen from Table 1 above that the AlON photocatalyst powder C3 of Example 3 has a degradation effect on Rhodamine B. Compared with the AlON@CeO2 composite photocatalyst powder of Comparative Example 2, the AlON@CeO2 composite photocatalyst powders of Examples 4 and 5 have higher degradation rates.
[0084] Table 2 Degradation rate of methylene orange and methylene blue by photocatalyst powder E of Example 5
[0085]
[0086] It can be seen from Table 1 above that the AlON@CeO2 composite photocatalyst powder E of Example 5 also has a good degradation effect on methylene orange and methylene blue.
[0087] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. For example, the AlON powder prepared by the present invention is not limited to the composite with CeO2 powder, but can also be composited with other powders to prepare photocatalysts; similarly, the composite catalyst prepared by the present invention is not limited to catalytic degradation of Rhodamine B, but can also catalytically degrade pollution sources such as methylene orange, methylene blue or other pollution sources. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be based on the attached claims.
Claims
1. A method for rapidly preparing AlON ceramic powder, characterized in that: The steps include: S1: dissolving phenolic resin in anhydrous ethanol to prepare a phenolic resin ethanol solution; adding nano-γ-Al2O3 powder to the phenolic resin ethanol solution, and obtaining a raw material mixture slurry after ultrasonic dispersion and stirring; S2: The uniformly stirred raw material mixture slurry is heated, dried and solidified to completely volatilize the ethanol in the slurry and solidify the phenolic resin on the surface of the nano γ-Al2O3 powder to obtain a γ-Al2O3 / PF precursor mixture; S3: subjecting the γ-Al2O3 / PF precursor mixture to a one-step carbon thermal reduction nitridation reaction at elevated temperature, and then heat preservation to obtain AlON ceramic powder.
2. The method for rapidly preparing AlON ceramic powder according to claim 1, characterized in that: In step S1, the phenolic resin is a thermosetting phenol formaldehyde resin.
3. The method for rapidly preparing AlON ceramic powder according to claim 1, characterized in that: In step S1, the nano γ-Al2O3 powder is a γ-Al2O3 powder with an average particle size of 10-50nm and a purity of 99.99%.
4. The method for rapidly preparing AlON ceramic powder according to claim 1, characterized in that: In step S1, the mass ratio of anhydrous ethanol, phenolic resin and nano-γ-Al2O3 powder is 30:(0.8-1):
5.
5. The method for rapidly preparing AlON ceramic powder according to claim 1, characterized in that: In step S1, the ultrasonic dispersion time is 20 min-40 min; the stirring is magnetic stirring, the speed of the magnetic stirring is 800 rpm-1500 rpm, and the time is 20 min-40 min.
6. The method for rapidly preparing AlON ceramic powder according to claim 1, characterized in that: In step S2, the specific steps of heating, drying and curing treatment include the following: (1) Perform the first step of heating, drying and curing treatment at a temperature of 70-90°C for 2h-4h; (2) The second step of heating, drying and curing treatment is carried out at a temperature of 180-220°C for 2h-4h.
7. The method for rapidly preparing AlON ceramic powder according to claim 1, characterized in that: In step S3, in the one-step temperature-raising carbon thermal reduction nitridation reaction, the heating rate is 6-12°C / min, the reaction temperature is 1700-1800°C, the holding time is 8-15min, and the reaction atmosphere is a nitrogen environment.
8. An AlON@CeO2 composite photocatalyst, characterized in that: The steps include: The AlON ceramic powder obtained by the method according to any one of claims 1 to 7 is mixed with nano CeO2 powder by ball milling to obtain the AlON@CeO2 composite photocatalyst.
9. The AlON@CeO2 composite photocatalyst according to claim 8, characterized in that: In the AlON@CeO2 composite photocatalyst, the content of nano-CeO2 powder is 25-50wt%; the grinding balls used in ball milling are high-purity alumina balls, the ball milling method used is wet ball milling, the dispersion medium of wet ball milling is anhydrous ethanol, the ball milling speed is 150-300rpm, and the ball milling time is 20-30h.
10. An application, characterized in that: The AlON@CeO2 composite photocatalyst as described in any one of claims 8 or 9 is used to degrade pollutants in industrial printing and dyeing wastewater, and the pollutants include one or more of rhodamine B, methylene orange, and methylene blue.
Citation Information
Patent Citations
Preparation method of Al5O6N-combined corundum composite refractory material
CN105294081A
Application of AlON powder as photocatalyst
CN106111178A
Cerium dioxide-based composite catalyst, and preparation method and application thereof
CN108906067A
Preparation method of AlON transparent ceramic powder
CN112374895A
Method for rapidly preparing pure-phase AlON fine powder through one-step heating carbon thermal reduction nitridation
CN113105246A