Catalyst for efficiently synthesizing 4-methylcatechol from p-cresol as well as preparation method and application of catalyst

By preparing and applying metal salt catalysts, the synthesis route of 4-methylcatechol is simplified, the problems of long reaction routes and environmental pollution in the existing methods are solved, and efficient and environmentally friendly industrial production is achieved.

CN118904382AActive Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410970993.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing 4-methylcatechol synthesis methods have problems such as long reaction routes, cumbersome operating conditions or serious environmental pollution, and lack simple, efficient, environmentally friendly and suitable for large-scale industrial production.

Method used

The active components are impregnated on the support by equal volume impregnation method, and after calcination, extruded with the binder strips to prepare metal salt catalysts such as iron salt and vanadium salt, and in a fixed bed, they are combined with paracresol, alcohol solvent and hydrogen peroxide. The reaction catalyzes the formation of 4-methylcatechol, the reaction conditions are 40-60°C, normal pressure, and the reaction time is 0.1-1 hour.

Benefits of technology

The synthesis route is simplified, production efficiency is improved, catalyst activity is high, yield is high, by-products are few, and the production of waste salt and wastewater is reduced. It meets the requirements of low-carbon environmental protection and sustainable development, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953202140000081
    Figure BDA0004953202140000081
  • Figure BDA0004953202140000082
    Figure BDA0004953202140000082
Patent Text Reader

Abstract

The invention discloses a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol and a preparation method and application thereof.The preparation method of the catalyst comprises the steps that after active components are dissolved with water, a carrier is impregnated with the active components through an equivalent-volume impregnation method, drying is conducted after sufficient impregnation, roasting is conducted in a muffle furnace, and the catalyst is obtained. The active components comprise one of the following components: 1) ferric salt and vanadium salt, the mass ratio of the ferric salt to the vanadium salt is 1: (0.5-2), and the total mass of the ferric salt and the vanadium salt is 40-70% of the mass of the carrier; the mass ratio of the main metal salt to the doped metal salt is (7.5-50): 1, the total mass of the main metal salt and the doped metal salt is 20-42% of the mass of the carrier, the main metal salt is ferric salt or vanadium salt, and the doped metal salt is cobalt salt, nickel salt, copper salt or palladium salt. The catalyst is used for catalyzing p-cresol to synthesize 4-methylcatechol, the synthesis route is simplified, the production efficiency is improved, the catalyst activity is high, the target product yield is high, and byproducts are few.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic chemical synthesis, and in particular to a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol, and a preparation method and application thereof. Background Art

[0002] 4-Methylcatechol, chemically known as 3,4-dihydroxytoluene or 4-methyl-1,2-benzenediol or homocatechol, is usually a white or off-white crystalline powder. It is an important organic compound and is widely used in many fields such as chemical industry and medicine. In the field of organic synthesis, 4-methylcatechol, as an important raw material or intermediate, can be used to synthesize biologically active compounds or functional materials; in the field of medicine, due to its unique chemical structure, it can be used as a precursor of specific drugs or a key component in the synthesis process, such as in the synthesis of antibacterial agents, dyes and fragrances; in industry, it can be used to prepare developers, rubber antioxidants or antioxidants, inhibitors, stabilizers, etc., to improve product performance or extend service life.

[0003] There are many methods for the synthesis of 4-methylcatechol, including the liquefaction lignin method, the halogenated benzene hydrolysis method, the direct hydroxylation method, the 4-methylguaiacol hydrolysis method and the phenol magnesium-formaldehyde method.

[0004] Chinese patent CN107216238A discloses a method for preparing 4-methylcatechol by magnesium alcohol method. The method uses p-cresol as a raw material, reacts with magnesium alcohol to first generate p-cresol magnesium, synthesizes 3-methyl salicylaldehyde with p-cresol magnesium, and then oxidizes it with hydrogen peroxide to synthesize 4-methylcatechol. The method has mild reaction conditions and high reaction yield, but the operation steps are relatively cumbersome and reagents such as toluene and paraformaldehyde are used, which is not conducive to environmental protection and large-scale industrial production.

[0005] Chinese patent CN103864578A discloses a method for preparing 4-methylcatechol using 2-methoxy-4-methylphenol as a raw material. In this method, the reaction system is protected from light and inert gas, sodium sulfite is added and hydrogen bromide gas is continuously introduced to perform a one-step demethylation reaction, and then 4-methylcatechol can be obtained through neutralization, extraction, centrifugation and other steps. This method uses natural raw materials and has a high product yield, but the operation is complicated, the reaction conditions are relatively harsh, and the amount of hydrogen bromide used is large.

[0006] Chinese patent CN1298857A discloses a method for preparing 4-methylcatechol by using p-cresol as raw material, adding a certain amount of titanium silicon molecular sieve and reacting with hydrogen peroxide to produce a hydroxylation reaction. The process of this method is relatively simple and clean, but it has disadvantages such as high reaction temperature and low yield.

[0007] Although 4-methylcatechol can be synthesized artificially by chemical synthesis, the existing methods have disadvantages such as long reaction routes, complicated operating conditions, or serious environmental pollution. Therefore, it is of great significance to develop a simple, efficient, environmentally friendly method for preparing 4-methylcatechol that is conducive to large-scale industrial production. Summary of the invention

[0008] In view of the above technical problems existing in the prior art, the object of the present invention is to provide a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol, and a preparation method and application thereof.

[0009] To achieve the above object, the technical solution adopted by the present invention is:

[0010] A preparation method of a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol, comprising the following steps: dissolving an active component in water, impregnating the active component onto a carrier by an equal volume impregnation method, drying the active component after sufficient impregnation, calcining the active component in a muffle furnace at 450-600°C for 1-4h, extruding the calcined product with a binder, drying the product, and calcining the product in a muffle furnace at 450-600°C for 1-4h to obtain the catalyst;

[0011] Wherein, the active component is one of the following:

[0012] 1) Iron salt and vanadium salt, the mass ratio of the two is 1:0.5-2, and the total mass of the two is 40-70% of the mass of the carrier;

[0013] 2) A main metal salt and a doping metal salt, the mass ratio of the two is 7.5-50:1, and the total mass of the two is 20-42% of the mass of the carrier, the main metal salt is an iron salt or a vanadium salt, and the doping metal salt is a cobalt salt, a nickel salt, a copper salt or a palladium salt.

[0014] Furthermore, the iron salt, cobalt salt, nickel salt and copper salt are nitrates, sulfates, chlorides or acetates respectively; the vanadium salt is sodium vanadate or sodium pyrovanadate; and the palladium salt is palladium acetate.

[0015] Furthermore, when the main metal salt is an iron salt and the doped metal salt is a cobalt salt or a copper salt, the mass ratio of the main metal salt to the doped metal salt is 20-40:1.

[0016] Furthermore, when the main metal salt is an iron salt and the doped metal salt is a nickel salt, the mass ratio of the main metal salt to the doped metal salt is 7.5-10:1, and the total mass of the two is 30-35% of the mass of the carrier.

[0017] Furthermore, when the main metal salt is a vanadium salt and the doping metal salt is a palladium salt, the mass ratio of the main metal salt to the doping metal salt is 45-50:1, and the total mass of the two is 20-25% of the mass of the carrier.

[0018] Furthermore, the carrier is TS-1 molecular sieve, MCM-41 molecular sieve or ZSM-5 molecular sieve.

[0019] The present invention also provides an application of the catalyst in catalyzing the synthesis of 4-methylcatechol from p-cresol. The p-cresol, an alcohol solvent and hydrogen peroxide are mixed to obtain a reaction liquid. The reaction liquid is then passed through a fixed bed filled with the catalyst for a catalytic reaction to generate 4-methylcatechol. The temperature of the catalytic reaction is 40-60° C., the pressure is normal pressure, and the mass space velocity of the reaction liquid is 0.1-1h -1 .

[0020] Furthermore, the alcohol solvent is methanol or ethanol, the mass ratio of p-cresol to the alcohol solvent is 1:0.5-2, preferably 1:1; the mass ratio of p-cresol to the H2O2 component in hydrogen peroxide is 1:0.5-3, preferably 1:1-1.5.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are: the preparation method of the catalyst of the present invention is simple, the cost is low, the prepared catalyst has high catalytic activity and stability, and has important industrial application value. The catalyst of the present invention is used to catalyze the synthesis of 4-methylcatechol from p-cresol, simplifies the synthesis route, improves production efficiency, has high catalyst activity, high yield of target products and few by-products, reduces the generation of waste salt and wastewater and environmental pollution in traditional multi-step reactions, meets the requirements of low-carbon environmental protection and sustainable development, and is conducive to large-scale industrial production.

[0022] The implementation of the present invention will provide a stable and reliable source of 4-methylcatechol for the fields of medicine, chemical industry, etc., and promote the development of related industries. DETAILED DESCRIPTION

[0023] The content and purity of the product in the present invention are detected by gas chromatography. The present invention is described in detail below in conjunction with some specific embodiments, but the present invention is not subject to any limitation of these embodiments. Any modification, equivalent replacement and improvement made on the thought and principle of the present invention, etc., should all be included in the protection scope of the present invention.

[0024] In the embodiments of the present invention, TS-1 molecular sieve, MCM-41 molecular sieve and ZSM-5 molecular sieve were purchased from Zhuoran Environmental Protection Technology (Dalian) Co., Ltd. The average pore size of TS-1 molecular sieve is greater than 0.56 nanometers, and the specific surface area is about 370 m 2 / g; the average pore size of MCM-41 molecular sieve is 2.5 to 3.5 nanometers, and the specific surface area is about 425m 2 / g; the average pore size of ZSM-5 molecular sieve is 0.55-0.6 nanometers, and the specific surface area is greater than 350m 2 / g. Ti-MWW molecular sieve was purchased from Angxing New Materials Changzhou Co., Ltd., with an average pore size greater than 0.4 nanometers and a specific surface area greater than 450m 2 / g.

[0025] Embodiment 1:

[0026] Using water as solvent, 15g of sodium vanadate and 15g of ferric nitrate were loaded onto 50g of TS-1 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst A.

[0027] Embodiment 2:

[0028] Using water as solvent, 0.5g of cobalt nitrate and 20g of ferric nitrate were loaded onto 50g of TS-1 molecular sieve by equal volume impregnation method, baked at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst B.

[0029] Embodiment 3:

[0030] Using water as solvent, 0.5g of copper nitrate and 10g of ferric chloride were loaded onto 50g of TS-1 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst C.

[0031] Embodiment 4:

[0032] Using water as solvent, 2g of nickel nitrate and 15g of ferric sulfate were loaded onto 50g of MCM-41 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst D.

[0033] Embodiment 5:

[0034] Using water as solvent, 0.2g of palladium acetate and 10g of sodium vanadate were loaded onto 50g of ZSM-5 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst E.

[0035] Embodiment 6:

[0036] Using water as solvent, 20g of ferric nitrate was loaded onto 50g of TS-1 molecular sieve by equal volume impregnation method, baked at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst F.

[0037] Embodiment 7:

[0038] Using water as solvent, 10g of copper nitrate and 0.5g of ferric chloride were loaded onto 50g of TS-1 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst G.

[0039] Embodiment 8:

[0040] Using water as solvent, 0.2 g of palladium acetate and 15 g of copper nitrate were loaded onto 50 g of ZSM-5 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst H.

[0041] Embodiment 9:

[0042] Using water as solvent, 0.5g zinc nitrate and 20g ferric nitrate were loaded onto 50g TS-1 molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst I.

[0043] Embodiment 10:

[0044] Using water as solvent and TS-1 molecular sieve without metal loading, the mixture was dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use. Then, a sesbania powder adhesive was added (the mass of the adhesive was 5% of the mass of the calcined product) and dispersed with an appropriate amount of water. The mixture was extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, which was recorded as catalyst J.

[0045] Embodiment 11:

[0046] Using water as solvent, 0.5g of copper nitrate and 10g of ferric chloride were loaded onto 50g of Ti-MWW molecular sieve by equal volume impregnation method, dried at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst K.

[0047] Embodiment 12:

[0048] Using water as solvent, 0.5g of copper nitrate and 10g of ferric chloride were loaded onto 50g of alumina by equal volume impregnation method, baked at 120°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours for use, and then added with field sesbania powder adhesive (the mass of the adhesive is 5% of the mass of the calcined product) and dispersed with appropriate amount of water, extruded into strips, dried at 120°C for 3 hours, and then calcined again at 550°C in a muffle furnace for 3 hours to obtain the final catalyst, recorded as catalyst L.

[0049] Examples 13-24

[0050] The reaction of synthesizing 4-methylcatechol from p-cresol was carried out on a fixed bed, using the catalysts of Examples 1-12 respectively. The reaction conditions were as follows: the loading amount of the catalyst on the fixed bed was 80 g, the raw materials with a mass ratio of p-cresol: methanol: 30% hydrogen peroxide = 1:1:5 were mixed to obtain a reaction liquid, the reaction liquid was introduced into the fixed bed, and reacted under the action of the catalyst, the reaction temperature was 50°C, the pressure was normal pressure, and the mass space velocity of the reaction liquid was 0.2 h -1 The reaction results are shown in Table 1 and Table 2:

[0051] Table 1

[0052]

[0053] Table 2

[0054]

[0055] It can be seen from the experimental results in Table 1-2 that the selection of metal salt active components and catalyst carriers has a great influence on the catalytic activity of the catalyst.

Claims

1. A method for preparing a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol, characterized in that The method comprises the following steps: dissolving the active component in water, impregnating the active component onto the carrier by an equal volume impregnation method, drying the active component after sufficient impregnation, calcining the active component in a muffle furnace at 450-600° C. for 1-4 hours, extruding the calcined product with a binder, drying the product, and calcining the product in a muffle furnace at 450-600° C. for 1-4 hours to obtain the catalyst; Wherein, the active component is one of the following: 1) Iron salt and vanadium salt, the mass ratio of the two is 1:0.5-2, and the total mass of the two is 40-70% of the carrier mass; 2) The mass ratio of the main metal salt and the doping metal salt is 7.5-50:1, and the total mass of the two is 20-42% of the mass of the carrier. The main metal salt is an iron salt or a vanadium salt, and the doping metal salt is a cobalt salt, a nickel salt, a copper salt or a palladium salt.

2. The method for preparing a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol as claimed in claim 1, characterized in that The iron salt, cobalt salt, nickel salt and copper salt are nitrate, sulfate, chloride or acetate respectively; the vanadium salt is sodium vanadate or sodium pyrovanadate; and the palladium salt is palladium acetate.

3. The method for preparing a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol as claimed in claim 1, characterized in that When the main metal salt is an iron salt and the doped metal salt is a cobalt salt or a copper salt, the mass ratio of the main metal salt to the doped metal salt is 20-40:

1.

4. The method for preparing a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol as claimed in claim 1, characterized in that When the main metal salt is an iron salt and the doped metal salt is a nickel salt, the mass ratio of the main metal salt to the doped metal salt is 7.5-10:1, and the total mass of the two is 30-35% of the mass of the carrier.

5. The method for preparing a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol as claimed in claim 1, characterized in that When the main metal salt is a vanadium salt and the doping metal salt is a palladium salt, the mass ratio of the main metal salt to the doping metal salt is 45-50:1, and the total mass of the two is 20-25% of the mass of the carrier.

6. The method for preparing a catalyst for efficiently synthesizing 4-methylcatechol from p-cresol as claimed in claim 1, characterized in that The carrier is TS-1 molecular sieve, MCM-41 molecular sieve or ZSM-5 molecular sieve.

7. A catalyst for efficiently synthesizing 4-methylcatechol from p-cresol prepared by the method according to any one of claims 1 to 6.

8. Use of the catalyst as claimed in claim 7 in catalyzing the synthesis of 4-methylcatechol from p-cresol.

9. The use according to claim 8, characterized in that The p-cresol, alcohol solvent and hydrogen peroxide are mixed to obtain a reaction liquid, and the reaction liquid is then catalytically reacted by passing through a fixed bed filled with a catalyst to generate 4-methylcatechol. The temperature of the catalytic reaction is 40-60° C., the pressure is normal pressure, and the mass space velocity of the reaction liquid is 0.1-1h -1 .

10. The use according to claim 9, characterized in that The alcohol solvent is methanol or ethanol, and the mass ratio of p-cresol to the alcohol solvent is 1:0.5-2, preferably 1:1; the mass ratio of p-cresol to the H2O2 component in hydrogen peroxide is 1:0.5-3, preferably 1:1-1.5.

Citation Information

Patent Citations

  • Synthesis method of 4-methylcatechol

    CN103864578A

  • Method for preparing 4-methylcatechol by using methanol and magnesium

    CN107216238A

  • Process for preparing 4-methyl catechol

    CN1298857A

  • Method for preparing methyl phenol from methylbenzene through catalytic oxidation in one step

    CN101092332A

  • Preparation method of double-metal-loaded molecular sieve catalyst for decomposing nitrous oxide

    CN103055934A