Method and device for decomposing fly ash dioxin and cooperatively solidifying heavy metal

By using Ni/NHPC catalyst and two-stage rotary kiln structure with nitrogen-doped porous carbon material support, the problems of high energy consumption and dioxin regeneration in fly ash dioxin detoxification technology are solved, and high-efficiency decomposition and Heavy metal curing achieves the effect of net zero emissions.

CN118904889APending Publication Date: 2024-11-08UNIV OF SHANGHAI FOR SCI & TECH

Patent Information

Application Number
CN202411037659.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing fly ash dioxin detoxification technology has problems such as high energy consumption, poor heavy metal curing effect, and dioxin regeneration. It is difficult to effectively reduce the fly ash dioxin concentration and achieve stable compliance under low temperature conditions.

Method used

Using nitrogen-doped graded porous carbon material NHPC as a support, stably anchor the metal nickel, construct Ni/NHPC catalyst, dispose of fly ash dioxin by low temperature pyrolysis, and use a two-stage rotary kiln structure to quickly cool it to avoid dioxin Regenerate.

Benefits of technology

The low-temperature and efficient decomposition of fly ash dioxin (decomposition rate >95%) and effective curing of heavy metals are achieved, which reduces energy consumption and avoids the regeneration of dioxin during cooling, achieving net zero emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904889A_ABST
    Figure CN118904889A_ABST
Patent Text Reader

Abstract

The invention provides a method and a device for decomposing fly ash dioxin and synergistically solidifying heavy metals, a nitrogen-doped hierarchical porous carbon material NHPC is used as a carrier, metal nickel Ni is stably anchored, and a Ni / NHPC catalyst is formed, so that while fly ash dioxin is subjected to low-temperature dechlorination, decomposition of a dioxin precursor is enhanced, low-temperature efficient decomposition of fly ash dioxin is promoted, and regeneration of fly ash dioxin is inhibited; wherein the NHPC material has a relatively large specific surface area and a rich micropore-mesopore-macropore structure, and can provide a large number of mass transfer channels which are small in resistance and short in diffusion path, so that heavy metals in fly ash are promoted to diffuse into the NHPC material; in addition, the NHPC material has huge adsorption capacity, so that the heavy metal can be adsorbed and fixed in a fluffy spongy structure of the NHPC material, the leaching of the heavy metal is reduced, and the heavy metal in the fly ash is effectively cured; according to the invention, a two-section rotary kiln device structure is also adopted to carry out low-temperature thermal decomposition treatment on the fly ash dioxin, so that the regeneration of the dioxin is avoided in a whole process, and the low-temperature thermal decomposition energy consumption of the fly ash dioxin is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fly ash treatment, and in particular to a method and a device for decomposing fly ash dioxins and synergistically solidifying heavy metals. Background Art

[0002] Dioxins, including polychlorinated dibenzodioxins and dibenzofurans (PCDD / Fs), have a total of 210 homologues, 17 of which are significantly toxic, with 2,3,7,8-tetrachlorodibenzodioxin being the most toxic. Fly ash is the main carrier of dioxin pollution. About 69.9-91.5% of the total dioxin emissions from the municipal solid waste incineration system are contained in fly ash. The dioxin concentration in fly ash in my country is as high as 5.7-7.5μg-TEQ / kg. In order to improve the technical level of fly ash disposal and reduce the environmental impact of its disposal and utilization process, my country's Ministry of Ecology and Environment issued the "Technical Specifications for Pollution Control of Fly Ash from Municipal Solid Waste Incineration (Trial)" (HJ 1134-2020), which stipulates that the total amount of dioxin residues in fly ash disposal products should not exceed 50ng I-TEQ / kg, while the relevant EU standard is as low as 20ng I-TEQ / kg. In this context, the need for harmless disposal of fly ash is very urgent. The development and improvement of dioxin detoxification technology is an important prerequisite for the safe disposal and resource utilization of incineration fly ash.

[0004] Existing fly ash dioxin detoxification technologies include high-temperature thermal treatment, hydrothermal treatment, mechanochemical treatment and low-temperature thermal decomposition. The high-temperature thermal treatment method is to heat the fly ash to make it sintered (700-1200℃), melted (1200-1600℃), and vitrified (1100-1500℃), decomposing dioxins while effectively solidifying heavy metals. However, this method has the disadvantages of high energy consumption, low-boiling point heavy metals are easy to volatilize, and dioxins are easy to regenerate in low temperature areas. The hydrothermal method uses a reactor to provide a suitable temperature (200-374℃) and high pressure (4-22MPa) environment to promote the dissolution and dechlorination of dioxins in fly ash, but there are also problems such as insufficient technical maturity, high energy consumption, and difficult waste liquid treatment. The mechanochemical treatment method is to apply mechanical force to the fly ash at room temperature to promote the effective decomposition of dioxins in the fly ash, but this method has problems such as high energy consumption, low disposal volume and long treatment cycle.

[0005] Low-temperature thermal decomposition can decompose 99% of dioxins in fly ash at low temperature (<500℃) in an oxygen-deficient or oxygen-free atmosphere. The reaction conditions are mild and the energy consumption is relatively low. The reaction products can be used as resources and applied to building materials, cement production, etc., to achieve secondary utilization of waste, and have great development potential. However, dioxin generation and decomposition exist simultaneously during low-temperature thermal decomposition. Only when the decomposition rate exceeds the generation rate will the dioxin concentration in fly ash gradually decrease. The decomposition rate and generation rate of fly ash dioxins are greatly affected by the composition of fly ash. CaO and Ca(OH)2 in fly ash can promote the decomposition of highly chlorinated dioxins in fly ash. The carbon source and chlorine source in fly ash will lead to the regeneration of dioxins, and some metals such as Cu, Zn, Mg, etc. will also play a catalytic role in the synthesis of dioxins. The main way of dioxin generation under inert atmosphere is precursor synthesis. Chlorine-containing precursor substances such as chlorobenzene and chlorophenol are generated during the incineration process of garbage. These precursors undergo heterogeneous catalytic reactions on the surfaces of various metal oxides in fly ash to generate dioxins. The composition of fly ash is affected by changes in garbage composition, incineration conditions, flue gas purification system, etc., so it is difficult to ensure that the dioxin concentration in fly ash meets the standard by optimizing the operating conditions alone. How to ensure that the dioxin concentration in fly ash meets the standard while further reducing the energy consumption of fly ash dioxin detoxification is of great environmental significance.

[0006] Patent CN113731420A discloses a catalyst for removing dioxins from fly ash, and its preparation method and application. This method aims at the problem that dioxin compounds are subjected to high-temperature heat treatment and have high energy consumption and high ash disposal costs. The method studies metal nitrate crystalline hydrates and porous carbon materials that affect the efficiency of dioxin degradation, and prepares a catalyst for efficient removal of dioxins under low temperature conditions. The catalyst is prepared by loading metal nitrate crystalline hydrates on the surface of porous carbon materials by impregnation and calcination. The metal nitrate crystalline hydrate is selected from one or more of Fe(NO3)3·9H2O, Co(NO3)2·6H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Pt(NO3)2·2H2O and Pd(NO3)2·6H2O. The porous carbon material is activated carbon, carbon nanotubes or graphene oxide. The method proposed in this patent is to fully mix the catalyst and fly ash in a dosage ratio of 1:5-20, and place the resulting mixture in an inert gas for reaction at a reaction temperature of 200-400°C and a reaction time of 10-80 minutes. However, this method has a poor heavy metal solidification effect.

[0007] Patent CN112675917A discloses a method for preparing a low-temperature degradation catalyst for dioxins based on sludge / garbage fly ash. Proteins in a mixture of sludge and garbage fly ash are extracted by a heat-acid method and hydrolyzed to obtain an amino acid mixed ligand. At the same time, the heavy metals in the garbage fly ash are converted into ions to form the coordination center of the metal organic framework material. During the hydrothermal synthesis of the metal organic framework material, the dioxins in the garbage fly ash are encapsulated in multi-sized pores, and low-temperature catalytic degradation is achieved under visible light / ultraviolet light conditions. However, this method requires additional light for dioxin decomposition, which requires high energy consumption and adds additional costs.

[0008] Patent CN105126606A discloses a method for treating volatile organic matter in incineration fly ash by low-temperature pyrolysis-catalytic degradation. The fly ash is transported to a low-temperature pyrolysis device and pyrolyzed at a temperature of 100 to 350°C in a non-oxidizing atmosphere for 10 to 60 minutes to produce a pyrolysis mixture. The above mixture is then transported to a catalytic degradation device in which the catalyst is a compound containing titanium, tungsten or vanadium, and degraded at a temperature of 100 to 400°C for 300 seconds in an oxidizing atmosphere. However, this method only decomposes dioxins and cannot remove heavy metals, and the catalyst used is expensive and has poor economic benefits. Summary of the invention

[0009] The purpose of the present invention is to overcome the above-mentioned shortcomings and to provide a decomposition method or device which can avoid the regeneration of dioxins, decompose fly ash dioxins at low temperature and high efficiency, and effectively solidify fly ash heavy metals while reducing energy consumption.

[0010] To achieve the above object, the present invention proposes a method for decomposing fly ash dioxins and synergistically solidifying heavy metals, using nitrogen-doped hierarchical porous carbon material NHPC as a carrier to firmly anchor metal nickel Ni to form a Ni / NHPC catalyst, so that the fly ash dioxins are dechlorinated at low temperature while strengthening the decomposition of dioxin precursors;

[0011] The method for decomposing fly ash dioxins and co-solidifying heavy metals comprises the following steps:

[0012] Step 1: Weigh a carbon source, a nitrogen source and a foaming agent, and prepare a nitrogen-doped hierarchical porous carbon material NHPC by a foaming method;

[0013] Step 2: Using the nitrogen-doped hierarchical porous carbon material NHPC as a carrier, mixing a nickel source with the NHPC, and loading nickel Ni on the NHPC carrier by an ultrasound-assisted reduction method to obtain a Ni / NHPC catalyst;

[0014] Step 3: Mix the Ni / NHPC catalyst and the fly ash, perform low-temperature pyrolysis treatment in pure N2 gas, and perform rapid cooling after treatment to achieve low-temperature thermal decomposition of dioxins in the fly ash.

[0015] The main principle of low-temperature thermal decomposition of fly ash dioxins is hydrodechlorination: active H atoms react with Cl atoms on aromatic rings, chlorine is removed and combined with H atoms to form HCl. The hydrogen source of fly ash dioxins comes from the dissociation and activation of hydrogen-containing substances in fly ash; metal Ni is low in price, high in mechanical strength, high in catalytic activity and selectivity for hydrodechlorination, and is often used to prepare alloys and batteries. It also has important applications in the field of catalysts. Ni-based catalysts are often used in hydrogenation reactions, dehydrogenation reactions, etc.; metal Ni can promote the dissociation and activation of H atoms in the reaction system, reduce the activation energy of dechlorination of target molecules, and thus increase the dechlorination rate of dioxins.

[0016] Furthermore, in step 1, the mass ratio of the carbon source, the nitrogen source and the foaming agent is 1:3:1; the carbon source is corn cob, the nitrogen source is ammonium oxalate monohydrate, and the foaming agent is potassium bicarbonate; step 1 is specifically:

[0017] 1.1: Weigh corn cobs, ammonium oxalate monohydrate and a foaming agent according to the mass ratio, grind them into mixed powder, place the mixed powder in a tube furnace, and introduce nitrogen N2 to exhaust the air in the reaction environment;

[0018] 1.2: operating the tube furnace, heating the room temperature to 900° C. at a rate of 10° C. / min in nitrogen, maintaining the temperature for 1 h, and then cooling to room temperature to obtain a black solid powder;

[0019] 1.3: The solid powder is dissolved in 500 ml of deionized water, and 5-10 ml of concentrated hydrochloric acid is added at the same time. The mixture is stirred at room temperature for 12 h at a stirring speed of 400 r / min. The mixture is then filtered and washed with deionized water until the filtrate is close to neutral. The filter residue is collected and dried and ground to obtain nitrogen-doped hierarchical porous carbon material NHPC.

[0020] Hierarchical porous carbon material HPC has a developed three-dimensional interconnected framework structure of micropores, mesopores and macropores, which can provide a large number of mass transfer channels with low resistance and short diffusion paths and are widely used as catalyst carriers, electrode materials and high-efficiency adsorbents. Further use of nitrogen-doped hierarchical porous carbon material NHPC can further modify the electronic structure of HPC, strengthen the interaction between active metals and HPC, form an M-N4 coordination structure to firmly anchor active metal atoms and promote their high dispersion. The present invention uses NHPC as a new catalyst carrier to firmly anchor and highly disperse metal Ni, thereby constructing a Ni / NHPC catalyst, inducing the dechlorination of dioxins in fly ash at low temperature (<350°C) while strengthening the decomposition of dioxin precursors, so as to achieve the purpose of achieving efficient detoxification of fly ash dioxins at low temperature (<350°C) (decomposition rate>95%).

[0021] Furthermore, the substrate NHPC material of the Ni / NHPC catalyst has a large specific surface area (1909.3m2 / g) and rich micropore-mesopore-macroporous structure, which can provide a large number of mass transfer channels with small resistance and short diffusion path, promoting the diffusion of heavy metals in fly ash into the interior of NHPC materials; in addition, the huge adsorption capacity of NHPC materials can adsorb and fix heavy metals in the fluffy sponge-like structure of NHPC materials, reduce heavy metal leaching, and thus achieve effective solidification of heavy metals in fly ash.

[0022] Furthermore, in step 2, the nickel source is nickel nitrate hexahydrate Ni(NO3)2·6H2O; and the mass ratio of the nickel source to NHPC is 1:1.8.

[0023] Furthermore, the step 2 is specifically as follows:

[0024] 2.1: Weigh 100 mg of nickel nitrate hexahydrate Ni(NO3)2·6H2O into a beaker, add 10 ml of deionized water, stir evenly to obtain a Ni(NO3)2·6H2O solution with a concentration of 10 mg / ml;

[0025] 2.2: Weigh 180 mg of the nitrogen-doped hierarchical porous carbon material NHPC into a beaker, add 20 ml of deionized water, and perform ultrasonic treatment for 30 min to uniformly disperse the NHPC in the water to obtain an NHPC aqueous solution;

[0026] 2.3: Slowly drip the Ni(NO3)2·6H2O solution into the NHPC aqueous solution, and assist with ultrasonic vibration to ensure that Ni 2+ After the addition was completed, ultrasonication was performed for 30 min to make the Ni 2+ Uniformly adsorbed to the surface of carbon materials;

[0027] 2.4: Prepare 1mg / ml NaBH4 solution, take 10ml and slowly drip it into the mixed solution, while assisting with ultrasonic vibration to absorb Ni adsorbed on the surface of the carbon material. 2+ Reduction, continued ultrasonication for 40 min;

[0028] 2.5: After the ultrasound is finished, the mixture is washed and filtered with deionized water, and the filter residue is collected and placed in an oven for drying to obtain a Ni / NHPC catalyst. In the Ni / NHPC catalyst, the theoretical loading amount of nickel Ni is 5%.

[0029] Furthermore, the specific surface area of ​​the Ni / NHPC catalyst is 1766 m 2 / g, and the total pore volume is 0.810cm 3 / g, micropore volume is 0.561cm 3 / g, and the mesopore volume is 0.243cm 3 / g, and the macropore volume is 0.006cm 3 / g, N doping amount is 0.95%, and Ni loading amount is 5%.

[0030] Furthermore, in step 3, a two-stage rotary kiln structure is used to carry out low-temperature thermal decomposition treatment of dioxins in the fly ash. The two-stage rotary kiln structure includes a first kiln body and a second kiln body. The first kiln body is used for low-temperature thermal decomposition treatment of the fly ash under an inert atmosphere; the second kiln body is used for rapid cooling of the treated fly ash in an inert atmosphere and waste heat recovery.

[0031] Furthermore, in step 3, the amount of the Ni / NHPC catalyst is 0.5-1wt% of the fly ash, and the specific steps of step 3 are: the Ni / NHPC catalyst and the fly ash are mixed and placed in the first kiln body of a two-stage rotary kiln, and subjected to low-temperature pyrolysis treatment in pure N2 gas for 30 minutes, with the pyrolysis temperature being 300°C; after treatment, the fly ash is placed in the second kiln body of the two-stage rotary kiln for rapid cooling to prevent the fly ash dioxins from being regenerated through the precursor synthesis path during the cooling process, thereby achieving low-temperature thermal decomposition of the fly ash dioxins.

[0032] The present invention also provides a device for decomposing fly ash dioxins and co-solidifying heavy metals, which is used to implement the above-mentioned method for decomposing fly ash dioxins and co-solidifying heavy metals. The device adopts a two-stage rotary kiln structure, and the device includes a reaction kiln, a cold zone kiln and a feeder. The reaction kiln is the first stage kiln body, and the cold zone kiln is the second stage kiln body.

[0033] The reaction kiln is connected to the cold zone kiln through a retaining wall; a sprinkler is provided above the cold zone kiln;

[0034] The reaction kiln is provided with a feed port, and the feeder is arranged on the top of the reaction kiln through the feed port; a feed valve is installed on the connection end between the feeder and the reaction kiln;

[0035] The side of the reaction kiln away from the cold zone kiln is connected to an air intake pipe, and an air intake valve and a heater are installed on the air intake pipe;

[0036] The side of the cold zone kiln away from the reaction kiln is connected with an exhaust pipe, and an exhaust valve is installed on the exhaust pipe.

[0037] The rotary kiln has the advantages of uniform heating, uniform material mixing, and continuous feeding. Under the interactive influence of the complex components of fly ash, dioxins are very easy to regenerate through the precursor synthesis path within the temperature range of 200-400°C. The device of the present invention uses a two-stage rotary kiln to treat fly ash dioxins at low temperature. The first section is used as a reaction kiln to treat the fly ash at low temperature under an inert atmosphere. The second section is used as a cold zone kiln to quickly cool the treated fly ash in an inert atmosphere and recover the waste heat. The device allows the treated fly ash to quickly reduce the thermal decomposition temperature to below 200°C, thereby shortening the residence time of the fly ash in the temperature range of 200-400°C, avoiding the regeneration of dioxins throughout the entire process, and reducing the energy consumption of low-temperature thermal decomposition of fly ash dioxins.

[0038] Furthermore, the operation method of the device is:

[0039] 1) Open the air inlet valve, the exhaust valve and the baffle, and close the feed valve; introduce nitrogen N2 into the reaction kiln through the air inlet pipe, thereby exhausting the air in the device and maintaining a pure nitrogen atmosphere during the reaction process;

[0040] 2) closing the exhaust valve and the baffle, starting the heater, and heating to 300° C.;

[0041] 3) After the temperature is stabilized, the reaction kiln is started, the feed valve is opened, and the mixed material is added into the reaction kiln for reaction;

[0042] 4) After the reaction is completed, the baffle is opened to allow the mixed material to enter the cooler for cooling, and the sprayer is opened to rapidly cool the treated fly ash by spraying water;

[0043] 5) After the fly ash treatment is completed, the exhaust valve is opened to discharge the reaction tail gas.

[0044] Compared with the prior art, the advantages of the present invention are:

[0045] 1. In the method of the present invention, NHPC is used as a carrier to firmly anchor metal Ni to construct a Ni / NHPC catalyst. The Ni / NHPC catalyst not only dechlorinates dioxins in fly ash at low temperature, but also enhances the decomposition of dioxin precursors, promotes the low-temperature and efficient decomposition of fly ash dioxins, and inhibits their regeneration.

[0046] 2. The metal Ni used in the method of the present invention is low in price, high in mechanical strength, high in catalytic activity and selectivity for hydrogenation dechlorination, and can promote the dissociation and activation of H atoms in the reaction system, reduce the dechlorination activation energy of the target molecule, and thus increase the dechlorination rate of dioxins.

[0047] 3. The NHPC material as the base of the Ni / NHPC catalyst in the present invention has a large specific surface area and a rich micropore-mesopore-macroporous structure, which can provide a large number of mass transfer channels with small resistance and short diffusion paths, thereby promoting the diffusion of heavy metals in fly ash into the interior of the NHPC material; in addition, the huge adsorption capacity of the NHPC material can adsorb and fix the heavy metals in the fluffy sponge-like structure of the NHPC material, reduce the leaching of heavy metals, and thus achieve effective solidification of heavy metals in fly ash.

[0048] 4. Under the interactive influence of the complex components of fly ash, dioxins are very easy to regenerate through the precursor synthesis path within the temperature range of 200-400°C. The present invention adopts a two-stage rotary kiln structure. The rotary kiln has the advantages of uniform heating, uniform material mixing, and continuous feeding. The two-stage rotary kiln is used to carry out low-temperature thermal decomposition of fly ash dioxins, so that the thermal decomposition temperature of the treated fly ash is quickly reduced to below 200°C, shortening the residence time of the fly ash in the temperature range of 200-400°C, avoiding the regeneration of dioxins in the whole process, and reducing the energy consumption of low-temperature thermal decomposition of fly ash dioxins.

[0049] 5. Through the method and device of the present invention, the gaseous pollutants released from the fly ash after treatment are very few, and most of the pollutants are fixed in the solid phase, which can achieve net zero emissions without the need to set up a flue gas purification system. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 The figure is a schematic diagram of the structure of a device for decomposing dioxins in fly ash and co-solidifying heavy metals according to an embodiment of the present invention.

[0051] Figure 2 This is a flow chart of a method for decomposing fly ash dioxins and synergistically solidifying heavy metals according to an embodiment of the present invention. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further described below.

[0053] This embodiment provides a method and device for decomposing fly ash dioxins and co-solidifying heavy metals. Figure 1 As shown, a two-stage rotary kiln structure is adopted, including a reaction kiln 6, a cold zone kiln 10 and a feeder 3, wherein the reaction kiln 6 is the first stage kiln body, and the cold zone kiln 10 is the second stage kiln body;

[0054] The left side of the reaction kiln 6 is connected to an air intake pipe, on which a heater 1 and an air intake valve 2 are sequentially arranged to control the entry of gas; the right side of the reaction kiln 6 is connected to a cold zone kiln 10 through a baffle 7, and the baffle 7 is used to control the material in the reaction kiln 6 to enter the cold zone kiln 10. A sprayer 8 is arranged above the cold zone kiln 10, and the sprayer 8 sprays cooling water 9 to quickly cool the material in the cold zone kiln 10; the right side of the cold zone kiln 10 is connected to an exhaust pipe through an exhaust port, and an exhaust valve 11 is installed on the exhaust pipe to control the discharge of gas; in addition, a feed port is opened at the top of the reaction kiln 6, and is connected to a conical feeder 3 through the feed port. A feed valve is installed on the connecting end between the conical feeder 3 and the reaction kiln 6 to control the input amount of material.

[0055] Based on the above device, the method of this embodiment is as follows Figure 2 As shown, the specific steps are:

[0056] S1: Preparation of NHPC carrier

[0057] 1.1: Before the experiment, weigh 12g corn cob, 36g ammonium oxalate monohydrate and 12g potassium bicarbonate respectively, put the above materials in a ceramic mortar and grind them into mixed powder;

[0058] 1.2: The mixed powder was placed in a quartz boat and then placed in a tube furnace, and N2 was introduced at a rate of 300 ml / min for 10 minutes to exhaust the air in the reaction device;

[0059] 1.3: Then run the tube furnace, under 200 ml / min N2 atmosphere, raise the temperature from room temperature to 900 °C at a rate of 10 °C / min, and maintain for 1 h;

[0060] 1.4: Then cool to room temperature to obtain a black solid powder; dissolve the obtained powder in 500 ml of deionized water, add 5-10 ml of concentrated hydrochloric acid, and stir at room temperature at a speed of 400 r / min for 12 hours;

[0061] 1.5: Then filter and wash with deionized water until the filtrate pH is ≈ 7, collect the filter residue, dry and grind it to obtain NHPC.

[0062] S2: Preparation of Ni / NHPC catalyst by ultrasound-assisted reduction

[0063] 2.1: Weigh 100 mg of Ni(NO3)2·6H2O into a beaker, add 10 ml of deionized water, stir evenly to obtain a Ni(NO3)2·6H2O solution with a concentration of 10 mg / ml;

[0064] 2.1: Weigh 180 mg of NHPC

[0065] In a 100ml beaker, add 20ml of deionized water and ultrasonicate for 30min to evenly disperse it in the water;

[0066] 2.3: Slowly drip the prepared Ni(NO3)2·6H2O solution into the NHPC aqueous solution, and assist with ultrasonic vibration during the process to ensure that Ni 2+ After the addition was completed, the mixed solution was ultrasonicated for 30 min to make Ni 2+ Uniformly adsorbed to the surface of carbon materials;

[0067] 2.4: Take 10 ml of 1 mg / ml NaBH4 solution and slowly drip it into the above solution while assisting with ultrasonic vibration. This process will remove Ni adsorbed on the surface of the carbon material. 2+ Reduction, continued ultrasonication for 40 min;

[0068] 2.5: After the ultrasonic treatment, the mixture was washed and filtered with deionized water, the filter residue was collected and dried in an oven to obtain a Ni / NHPC catalyst with a Ni theoretical loading of 5%.

[0069] S3: Ni / NHPC catalyst for low temperature thermal decomposition of fly ash dioxins

[0070] Use the above Figure 1 The device for decomposing fly ash dioxins and synergistically solidifying heavy metals shown in the figure, after mixing the Ni / NHPC catalyst and fly ash obtained in step S2 to form a mixture 5, the mixture 5 is placed in a reaction kiln 6 of the device and treated at 300°C in a pure N2 atmosphere for 30 minutes; the baffle 7 is opened, and the treated mixture 5 enters the cooling kiln 10, and spray water 9 is ejected through the sprayer 8 for rapid cooling to prevent the fly ash dioxins from being regenerated through the precursor synthesis path during the cooling process. The specific operation method is: first, open the air intake valve 2, the exhaust valve 11 and the baffle 7, close the feed valve 4, and introduce nitrogen N2 to exhaust the air in the device to maintain a pure nitrogen atmosphere during the reaction process; then close the exhaust valve 11 and the baffle 7, start the heater 1 to heat to 300°C, and after the temperature stabilizes, start the reaction kiln 6, open the feed valve 4, and introduce N The mixture 5 of i / NHPC catalyst and fly ash is fed into the reaction kiln 6 through the feeder 3 for reaction; after the reaction is completed, the baffle 7 is opened to allow the mixture 5 after the reaction to enter the cooling kiln 10 for cooling, and the sprayer 8 is opened to spray out the spray water 9 to rapidly cool the fly ash after the treatment. After the fly ash treatment is completed, the exhaust valve 11 is opened to discharge the reaction tail gas.

[0071] In order to verify the technical effect and practical application performance of this embodiment, the embodiment is used as an experimental group, and a comparison group 1 and a comparison group 2 are set up.

[0072] Comparative group 1: The difference from the experimental group is that no catalyst is added, and fly ash dioxins are directly decomposed by low-temperature thermal decomposition;

[0073] Comparative group 2: The difference from the experimental group is that NHPC catalyst is used to thermally decompose fly ash dioxins at low temperature.

[0074] The changes in toxic equivalent concentration and chlorine generation of fly ash dioxins before and after low-temperature thermal decomposition were detected under these three conditions. The experimental results are shown in Tables 1 and 2, where Table 1 is a comparison of the toxic equivalent concentration of fly ash dioxins before and after low-temperature thermal decomposition; Table 2 is a comparison of the chlorine generation of fly ash dioxins before and after low-temperature thermal decomposition.

[0075] Table 1

[0076]

[0077] As can be seen from Table 1, the addition of NHPC and Ni / NHPC can significantly reduce the toxic equivalent concentration of dioxins in fly ash and improve the degradation rate. Among them, when using Ni / NHPC catalyst with a Ni loading of 5%, the degradation rate is the highest, which is 82.40%.

[0078] Table 2

[0079]

[0080] As can be seen from Table 2, the addition of NHPC and Ni / NHPC can effectively remove low-chlorinated dioxins (4-6C l) and high-chlorinated dioxins (7-8C l); when using Ni / NHPC catalyst with a Ni loading of 5%, the removal rates of chlorinated dioxins (4-6C l) and high-chlorinated dioxins (7-8C l) are the highest, which are 81.75% and 90.80%, respectively.

[0081] In summary, through the method and device proposed in the present invention, NHPC is used as a carrier to firmly anchor metal Ni to construct a Ni / NHPC catalyst. The Ni / NHPC catalyst can not only achieve low-temperature dechlorination of dioxins in fly ash, but also promote low-temperature and efficient decomposition of dioxins in fly ash.

[0082] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.

Claims

1. A method for decomposing fly ash dioxins and synergistically solidifying heavy metals, characterized in that: Using nitrogen-doped hierarchical porous carbon material NHPC as a carrier, metal nickel Ni is firmly anchored to form a Ni / NHPC catalyst, so that the fly ash dioxins can be dechlorinated at low temperature while enhancing the decomposition of dioxin precursors; The method for decomposing fly ash dioxins and synergistically solidifying heavy metals comprises the following steps: Step 1: Weigh a carbon source, a nitrogen source and a foaming agent, and prepare a nitrogen-doped hierarchical porous carbon material NHPC by a foaming method; Step 2: Using the nitrogen-doped hierarchical porous carbon material NHPC as a carrier, mixing a nickel source with the NHPC, and loading nickel Ni on the NHPC carrier by an ultrasound-assisted reduction method to obtain a Ni / NHPC catalyst; Step 3: Mix the Ni / NHPC catalyst and the fly ash, perform low-temperature pyrolysis treatment in pure N2 gas, and rapidly cool after treatment to achieve low-temperature thermal decomposition of dioxins in the fly ash.

2. The method for decomposing fly ash dioxins and synergistically solidifying heavy metals according to claim 1, characterized in that: In step 1, the mass ratio of the carbon source, the nitrogen source and the foaming agent is 1:3:1; the carbon source is corn cob, the nitrogen source is ammonium oxalate monohydrate, and the foaming agent is potassium bicarbonate; step 1 is specifically: 1.1: Weigh corn cobs, ammonium oxalate monohydrate and a foaming agent according to the mass ratio, grind them into mixed powder, place the mixed powder in a tube furnace, and introduce nitrogen N2 to exhaust the air in the reaction environment; 1.2: operating the tube furnace, heating the room temperature to 900° C. at a rate of 10° C. / min in nitrogen, maintaining the temperature for 1 h, and then cooling to room temperature to obtain a black solid powder; 1.3: The solid powder is dissolved in 500 ml of deionized water, and 5-10 ml of concentrated hydrochloric acid is added at the same time. The mixture is stirred at room temperature for 12 h at a stirring speed of 400 r / min. The mixture is then filtered and washed with deionized water until the filtrate is close to neutral. The filter residue is collected and dried and ground to obtain nitrogen-doped hierarchical porous carbon material NHPC.

3. The method for decomposing fly ash dioxins and synergistically solidifying heavy metals according to claim 1, characterized in that: In step 2, the nickel source is nickel nitrate hexahydrate Ni(NO3)2·6H2O; step 2 is specifically as follows: 2.1: Weigh 100 mg of nickel nitrate hexahydrate Ni(NO3)2·6H2O into a beaker, add 10 ml of deionized water, stir evenly to obtain a Ni(NO3)2·6H2O solution with a concentration of 10 mg / ml; 2.2: Weigh 180 mg of the nitrogen-doped hierarchical porous carbon material NHPC into a beaker, add 20 ml of deionized water, and perform ultrasonic treatment for 30 min to uniformly disperse the NHPC in the water to obtain an NHPC aqueous solution; 2.3: Slowly drip the Ni(NO3)2·6H2O solution into the NHPC aqueous solution, and assist with ultrasonic vibration to ensure that Ni 2 + After the addition is completed, the mixed solution is ultrasonicated for 30 minutes to make Ni 2+ Uniformly adsorbed to the surface of carbon materials; 2.4: Prepare 1mg / ml NaBH4 solution, take 10ml and slowly drip it into the mixed solution, while assisting with ultrasonic vibration to absorb Ni adsorbed on the surface of the carbon material. 2+ Reduction, continued ultrasonication for 40 min; 2.5: After the ultrasound is finished, the mixture is washed and filtered with deionized water, and the filter residue is collected and placed in an oven for drying to obtain a Ni / NHPC catalyst. In the Ni / NHPC catalyst, the theoretical loading amount of nickel Ni is 5%.

4. The method for decomposing fly ash dioxins and synergistically solidifying heavy metals according to claim 3, characterized in that: The specific surface area of ​​the Ni / NHPC catalyst is 1766 m 2 / g, and the total pore volume is 0.810cm 3 / g, micropore volume is 0.561cm 3 / g, and the mesopore volume is 0.243cm 3 / g, and the macropore volume is 0.006cm 3 / g, N doping amount is 0.95%, and Ni loading amount is 5%.

5. The method for decomposing fly ash dioxins and synergistically solidifying heavy metals according to claim 1, characterized in that: In step 3, a two-stage rotary kiln structure is used to carry out low-temperature thermal decomposition treatment of dioxins in the fly ash; the two-stage rotary kiln includes a first kiln body and a second kiln body, the first kiln body is used for low-temperature thermal decomposition treatment of the fly ash under an inert atmosphere; the second kiln body is used to achieve rapid cooling of the treated fly ash in an inert atmosphere and to recover waste heat.

6. The method for decomposing fly ash dioxins and synergistically solidifying heavy metals according to claim 5, characterized in that: In step 3, the amount of the Ni / NHPC catalyst is 0.5-1wt% of the fly ash. Specifically, step 3 comprises: mixing the Ni / NHPC catalyst and the fly ash and placing them in the first kiln body, subjecting them to low-temperature pyrolysis treatment in pure N2 gas for 30 minutes at a pyrolysis temperature of 300°C; and rapidly cooling them in the second kiln body after treatment to avoid the fly ash dioxins from being regenerated through the precursor synthesis pathway during the cooling process, thereby achieving low-temperature thermal decomposition of the fly ash dioxins.

7. A device for decomposing fly ash dioxins and synergistically solidifying heavy metals, used to implement the method for decomposing fly ash dioxins and synergistically solidifying heavy metals as claimed in any one of claims 1 to 6, characterized in that: Including reaction kiln, cold zone kiln and feeder: The reaction kiln is the first kiln body, and the cold zone kiln is the second kiln body; The reaction kiln is connected to the cold zone kiln through a retaining wall; a sprinkler is provided above the cold zone kiln; The reaction kiln is provided with a feed port, and the feeder is arranged on the top of the reaction kiln through the feed port; a feed valve is installed on the connection end between the feeder and the reaction kiln; The side of the reaction kiln away from the cold zone kiln is connected to an air intake pipe, and an air intake valve and a heater are installed on the air intake pipe; The side of the cold zone kiln away from the reaction kiln is connected with an exhaust pipe, and an exhaust valve is installed on the exhaust pipe.

8. The device for decomposing fly ash dioxins and co-solidifying heavy metals according to claim 7, characterized in that: The operation method of the device is: 1) Open the air inlet valve, the exhaust valve and the baffle, and close the feed valve; introduce nitrogen N2 into the reaction kiln through the air inlet pipe, thereby exhausting the air in the device and maintaining a pure nitrogen atmosphere during the reaction process; 2) closing the exhaust valve and the baffle, starting the heater, and heating to 300° C.; 3) After the temperature is stabilized, the reaction kiln is started, the feed valve is opened, and the mixed material is added into the reaction kiln for reaction; 4) After the reaction is completed, the baffle is opened to allow the mixed material to enter the cooler for cooling, and the sprayer is opened to rapidly cool the treated fly ash by spraying water; 5) After the fly ash treatment is completed, the exhaust valve is opened to discharge the reaction tail gas.

Citation Information

Patent Citations

  • Nitrogen-doped hierarchical pore carbon and preparation method and application thereof

    CN106179440A

  • Composite catalyst, and preparation method and application thereof

    CN109277109A

  • Vortex self-heating type low-temperature dioxin detoxification device and detoxification system

    CN112856432A

  • Catalyst for removing dioxin in fly ash as well as preparation method and application of catalyst

    CN113731420A

  • Preparation method of ruthenium-loaded nitrogen-doped porous carbon hydrogen evolution electrocatalyst

    CN114540863A

Cited By

  • Fly ash dioxin rapid catalytic decomposition method and device based on in-situ Joule heat

    CN120054999A

  • Fly ash segmented desorption dioxin flue gas cooperative treatment method and system

    CN121607400A

  • A heating device for purifying beryllium oxide

    CN122835117A

  • A heating device for purifying beryllium oxide

    CN122835117B