Method for cold pressing machining of pump runner chamber
The pump wheel chamber is formed by applying pressure at room temperature through cold pressing processing, which solves the problems of grain growth and plastic strength reduction caused by hot pressing processing, improves the processing quality and stability of the pump wheel chamber, and realizes energy and cost. save.
Patent Information
- Application Number
- CN202411192730.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional hot pressing processing methods lead to reduced grain growth and specified plastic extension strength in the pump wheel chamber, affecting the performance and stability of the pump.
Using the cold pressing processing method, by applying a pressure of 15MPa to 30MPa at room temperature to perform cold pressing processing, controlling the pressing angle and time, forming a fixed workpiece, and opening a bevel thereon, obtaining a pump wheel chamber. The adverse effects of the high temperature environment of hot pressing on the material are avoided.
It improves the processing quality and stability of the pump wheel chamber, saves energy and costs, while maintaining the original structure and performance of the material, significantly improving the efficiency and performance of the pump.
Smart Images

Figure CN118905029A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pump component processing, and in particular to a method for cold pressing a pump runner chamber. Background Art
[0002] The runner chamber, as a key component connecting the bottom ring and the draft tube, not only forms a hydraulic channel, but also ensures an appropriate gap with the outer edge of the runner blade. This design has a significant impact on the flow of water around the runner, which in turn has a decisive effect on the overall performance of the pump. Therefore, in the design process of the runner chamber, multiple factors must be considered comprehensively to minimize the turbulence and energy loss of the water flow, ensure the smooth passage of the water flow, and thus significantly improve the efficiency and performance of the pump.
[0003] The pump impeller chamber, as a core component in the hydraulic system, needs to meet high-precision standards for its geometry and surface quality, and its internal structure and curved surface design are usually complex and delicate. The traditional processing method for the pump impeller chamber is mainly hot pressing, which can easily lead to grain growth in the pump impeller chamber and affect the specified plastic elongation strength of the pump impeller chamber. Therefore, a more optimized processing method is needed to solve the problem of performance degradation of the pump impeller chamber caused by hot pressing. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a method for cold pressing a pump impeller chamber. The method adopts cold pressing technology to process the pump impeller chamber, avoiding the problems of grain growth and reduction of the specified plastic elongation strength of the pump impeller chamber caused by hot pressing, thereby improving the processing quality and stability of the pump impeller chamber, while saving energy and reducing equipment costs and processing costs.
[0005] In order to achieve the above purpose, the technical solution adopted in this application is:
[0006] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump runner chamber;
[0007] S2, cutting the plate to obtain a workpiece to be processed;
[0008] S3, placing the workpiece to be processed into a cold pressing mold, applying a pressure of 15MPa to 30MPa at a pressing angle of 140° for cold pressing to obtain a shaped workpiece;
[0009] If the applied pressure exceeds 30Mpa, severe friction and deformation will occur between the cold pressing die and the sheet, which will accelerate the wear of the cold pressing die surface and cause fatigue cracks, seriously affecting the service life of the cold pressing die. At the same time, excessive pressure will cause cracks in the shaped workpiece, exacerbating the problem of internal stress concentration.
[0010] S4, perform shape correction processing on the finalized workpiece, and after meeting the tolerance requirement of 140±2° of the external cutting angle of the finalized workpiece, perform cutting allowance and external surface processing to obtain a qualified finalized workpiece;
[0011] S5. Cut a groove on the qualified finalized workpiece to obtain the pump impeller chamber.
[0012] Preferably, in the cold pressing step, the processing rate is 5 mm / s to 8 mm / s.
[0013] Preferably, the cold pressing is performed at room temperature.
[0014] Preferably, the pressing time of cold pressing is 2 minutes; if the cold pressing time is less than 2 minutes, the workpiece to be processed cannot be completely shaped due to the short holding time, which leads to the problem of uneven internal stress; if the cold pressing time exceeds 2 minutes, the holding time is too long, resulting in indentations and damage on the surface of the workpiece to be processed, and even damage to the cold pressing mold, and at the same time, the microstructure and material properties of the shaped workpiece will be changed.
[0015] Preferably, the cold pressing mold is composed of two identical mold units, each mold unit is an arc-shaped plate, and the outer cutting angle of the mold unit is 140°. The two mold units are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate.
[0016] Preferably, a cutting margin is left around the workpiece to be processed, wherein a 50mm cutting margin is ensured around the workpiece to be processed, a contour cutting line is drawn on a qualified shaped workpiece, and the margin is cut according to the contour cutting line; wherein the margin is cut by a plasma cutting machine.
[0017] Preferably, the outer surface of the pump impeller chamber is processed by carbon arc gouging, the thickness of the carbon arc gouging is 1 mm to 2 mm, and the oxide layer and appearance defects on the outer surface of the shaped workpiece are polished to whiten.
[0018] Preferably, in step S1, the plate used is selected from 04Cr 13 Ni5Mo steel plate, carbon steel or 304 stainless steel; the plate must pass the sample inspection, have a plate product quality certificate, and pass the plate ultrasonic test.
[0019] Preferably, in step S2, the surface of the workpiece to be processed does not have defects such as cracks, bubbles, folding, and inclusions, otherwise it will have a negative impact on the quality of the pump impeller chamber, causing the mechanical strength of the pump impeller chamber to decrease, stress concentration, and increased risk of abrasion.
[0020] Preferably, in step S4, a CNC gantry milling machine is used to open the groove.
[0021] Preferably, the oxide layer and appearance defects on the back of the shaped workpiece are polished to remove minor defects, thereby improving surface smoothness and enhancing the quality and market competitiveness of the pump impeller chamber.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention proposes a method for cold pressing a pump impeller chamber. The cold pressing technology is used to process the pump impeller chamber, which can effectively improve the problems of grain growth and reduced specified plastic elongation strength of the plate caused by hot pressing, thereby improving the processing quality and stability of the pump impeller chamber.
[0024] 2. The present invention obtains a cold-pressed pump runner chamber. The preparation method of the pump runner chamber is to cut a plate into workpieces to be processed, and to perform cold pressing by controlling the pressing angle, applying pressure and pressing time to form a shaped workpiece; then, a groove is opened on the shaped workpiece to obtain the pump runner chamber. The present invention not only saves the energy cost and equipment cost required for hot pressing, but also reduces the processing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a product diagram of the pump impeller chamber of Example 2 of the present invention;
[0026] Figure 2 This is a tensile strength test curve of the pump impeller chamber of Example 2 of the present invention;
[0027] Figure 3 This is a product diagram of the pump impeller chamber of Comparative Example 3 of the present invention;
[0028] Figure 4 This is a tensile strength test curve of the pump runner chamber of Comparative Example 3 of the present invention;
[0029] Figure 5 This is a product diagram of the pump runner chamber of Comparative Example 4 of the present invention;
[0030] Figure 6 This is a tensile strength test curve of the pump runner chamber of Comparative Example 4 of the present invention;
[0031] Figure 7 It is a schematic diagram of the pressing angles of Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention;
[0032] Figure 8 Schematic diagram of cold pressing molds of Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention;
[0033] Fig. 9 Schematic diagrams of the processing directions of Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention, wherein (a) is a schematic diagram of the rolling direction, and (b) is a schematic diagram of the annular direction of the plate. DETAILED DESCRIPTION
[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following will be described in detail with reference to the accompanying drawings and table data. The embodiments are only partial, not complete. Other embodiments, as the protection scope of the present disclosure, will be obtained by ordinary technicians in the field without creative work. These descriptions will make the purpose, technical solutions and advantages of the present disclosure easier to understand and provide clear and complete guidance for further understanding.
[0035] Hot pressing is a metal processing technology that achieves plastic deformation of metals by applying pressure under high temperature conditions, thereby manufacturing parts with the desired shape and size. However, the high temperature environment has a multi-faceted effect on the grains of the plate, which involves a complex interaction of thermodynamic and kinetic processes. Specifically, high temperature promotes grain growth and leads to a reduction in the number of grain boundaries. Grain boundaries are an important obstacle to dislocation movement, so the growth of grains means the reduction of such barriers, making it easier for dislocations to move. At the same time, high temperature will also lead to the intensification of atomic vibrations inside the plate, thereby weakening the strength of atomic bonds between the lattices, which manifests as a thermal softening effect. This effect allows the plate to undergo plastic deformation at a lower stress, thereby reducing its specified plastic extension strength. Therefore, from a macroscopic point of view, the impact of the high temperature environment during hot pressing on the pump runner chamber is mainly manifested as a reduction in the specified plastic extension strength.
[0036] In view of the fact that the traditional hot pressing method for processing a pump runner chamber is prone to cause grain growth of the plate, thereby affecting the specified plastic elongation strength of the pump runner chamber, the present invention provides a method for cold pressing a pump runner chamber, comprising the following steps: preparing a cold pressing mold according to the shape, size and processing accuracy requirements of the pump runner chamber; taking the plate as a workpiece to be processed, placing the workpiece to be processed into the cold pressing mold, applying a pressure of 15MPa to 30MPa at a pressing angle of 140° for cold pressing to obtain a shaped workpiece; performing shape correction processing on the shaped workpiece, and after meeting the tolerance requirement of 140±2° of the external cutting angle of the shaped workpiece, cutting the allowance and external surface processing to obtain a qualified shaped workpiece; opening a groove on the qualified shaped workpiece to obtain a pump runner chamber.
[0037] The cold-pressing method of the present invention realizes direct and efficient deformation processing of the plate at room temperature by controlling the applied pressure and the pressing angle. This method completely abandons the heating process in the traditional hot pressing process, significantly reduces energy consumption, and effectively reduces production costs; more importantly, the cold-pressing method of the present invention can realize high-quality processing of the pump runner chamber without changing the original structure and performance of the plate, demonstrating excellent processing efficiency and material protection capabilities. Among them, the control angle is as follows: Figure 7 shown.
[0038] The technical solution of the present invention is further explained by using embodiments below, which are specifically as follows:
[0039] Example 1
[0040] A method for cold pressing a pump runner chamber, the specific steps are as follows:
[0041] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8 As shown, the cold pressing mold consists of two mold units, which are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate. The length of each mold unit is 4800mm and the width is 5100mm. The width of the gap between the two mold units is 2450mm.
[0042] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0043] S3, placing the workpiece to be processed into a cold pressing mold, applying a pressure of 30 MPa at a pressing angle of 140°, performing cold pressing at a processing rate of 5 mm / s, and maintaining for 2 min to obtain a finalized workpiece;
[0044] S4. After measuring the finalized workpiece, the shape is calibrated and the contour cutting line is drawn; wherein the external cutting angle of the finalized workpiece after the shape calibration is 138°;
[0045] S5. According to the cutting line, use a plasma cutting machine to cut the excess, and use carbon arc gouging to process the outer surface of the shaped workpiece. The thickness of the carbon arc gouging is 2mm;
[0046] S6. Use CNC gantry milling to cut out the groove to obtain the pump impeller chamber, which is recorded as cold pressing 138°.
[0047] Example 2
[0048] A method for cold pressing a pump runner chamber, which is the same as the steps in Example 1, except that the pressure is 25 MPa. The specific steps are as follows:
[0049] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8 As shown, the cold pressing mold consists of two mold units, which are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate. The length of each mold unit is 4800mm and the width is 5100mm. The width of the gap between the two mold units is 2450mm.
[0050] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0051] S3, placing the workpiece to be processed into a cold pressing mold, applying a pressure of 25 MPa at a pressing angle of 140°, performing cold pressing at a processing rate of 7 mm / s, and maintaining for 2 min to obtain a finalized workpiece;
[0052] S4, after measuring the finalized workpiece, perform shape calibration and draw the contour cutting line; wherein, the external cutting angle of the finalized workpiece after shape calibration is 140°;
[0053] S5. According to the cutting line, use a plasma cutting machine to cut the excess, and use carbon arc gouging to process the outer surface of the shaped workpiece. The thickness of the carbon arc gouging is 2mm;
[0054] S6. Use CNC gantry milling to cut out the groove to obtain the pump impeller chamber, which is recorded as cold pressing 140°.
[0055] Example 3
[0056] A method for cold pressing a pump runner chamber, which is the same as the steps in Example 1, except that the pressure is 15 MPa. The specific steps are as follows:
[0057] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8 As shown, the cold pressing mold consists of two mold units, which are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate. The length of each mold unit is 4800mm and the width is 5100mm. The width of the gap between the two mold units is 2450mm.
[0058] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0059] S3, placing the workpiece to be processed into a cold pressing mold, applying a pressure of 15 MPa at a pressing angle of 140°, performing cold pressing at a processing rate of 8 mm / s, and maintaining for 2 min to obtain a finalized workpiece;
[0060] S4. After measuring the finalized workpiece, the shape is calibrated and the contour cutting line is drawn; wherein the external cutting angle of the finalized workpiece after the shape calibration is 142°;
[0061] S5. According to the cutting line, use a plasma cutting machine to cut the excess, and use carbon arc gouging to process the outer surface of the shaped workpiece. The thickness of the carbon arc gouging is 1mm.
[0062] S6. Use CNC gantry milling to cut out the groove and obtain the pump impeller chamber, which is recorded as cold pressing 142°.
[0063] Comparative Example 1
[0064] A method for cold pressing a pump runner chamber, which is the same as the steps in Example 1, except that the pressure is 45 MPa. The specific steps are as follows:
[0065] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8 As shown, the cold pressing mold consists of two mold units, which are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate. The length of each mold unit is 4800mm and the width is 5100mm. The width of the gap between the two mold units is 2450mm.
[0066] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0067] S3, placing the workpiece to be processed into a cold pressing mold, applying a pressure of 45 MPa at a pressing angle of 140°, performing cold pressing at a processing rate of 5 mm / s, and maintaining for 2 min to obtain a finalized workpiece;
[0068] S4, after measuring the finalized workpiece, perform shape calibration and draw the contour cutting line; wherein, the external cutting angle of the finalized workpiece after shape calibration is 120°;
[0069] S5. According to the cutting line, use a plasma cutting machine to cut the excess, and use carbon arc gouging to process the outer surface of the shaped workpiece. The thickness of the carbon arc gouging is 2mm;
[0070] S6. Use CNC gantry milling to cut out the groove to obtain the pump impeller chamber, which is recorded as cold pressing 120°.
[0071] Comparative Example 2
[0072] A method for cold pressing a pump runner chamber, which is the same as the steps in Example 1, except that the pressure is 35 MPa. The specific steps are as follows:
[0073] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8As shown, the cold pressing mold consists of two mold units, which are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate. The length of each mold unit is 4800mm and the width is 5100mm. The width of the gap between the two mold units is 2450mm.
[0074] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0075] S3, placing the workpiece to be processed into a cold pressing mold, applying a pressure of 35 MPa at a pressing angle of 140°, performing cold pressing at a processing rate of 5 mm / s, and maintaining for 2 min to obtain a finalized workpiece;
[0076] S4, after measuring the finalized workpiece, perform shape calibration and draw the contour cutting line; wherein, the external cutting angle of the finalized workpiece after shape calibration is 130°;
[0077] S5. According to the cutting line, use a plasma cutting machine to cut the excess, and use carbon arc gouging to process the outer surface of the shaped workpiece. The thickness of the carbon arc gouging is 2mm;
[0078] S6. Use CNC gantry milling to cut out the groove to obtain the pump impeller chamber, which is recorded as cold pressing 130°.
[0079] Comparative Example 3
[0080] A method for hot pressing a pump runner chamber, the specific steps are as follows:
[0081] S1. Prepare the hot pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8 As shown, the hot pressing mold has a length of 4800 mm, a width of 5100 mm, and an opening height of 2450 mm;
[0082] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0083] S3. Place the workpieces to be processed into the heating furnace, with a spacing of 100 mm between the workpieces to ensure uniform heating during heating, facilitate lifting and ensure safety, and obtain preheated workpieces;
[0084] S4, placing the preheated workpiece into a hot pressing mold, performing hot pressing at a pressing angle of 140° and a pressure of 55 MPa, holding for 2 minutes, and then performing secondary heating, heating to 1050°C and keeping the temperature for 2 minutes, then quickly taking it out and extremely cooling it to 180°C to obtain a shaped workpiece;
[0085] S5. After measuring the finalized workpiece, the workpiece is calibrated and the contour cutting line is drawn; wherein the external cutting angle of the finalized workpiece after the calibration is 90°;
[0086] S6. According to the cutting line, use a plasma cutting machine to cut the excess, and use carbon arc gouging to process the outer surface of the shaped workpiece. The thickness of the carbon arc gouging is 2mm;
[0087] S7. Use CNC gantry milling to cut out the groove to obtain the pump impeller chamber, which is recorded as hot pressing 90°.
[0088] Comparative Example 4
[0089] A method for hot pressing a pump runner chamber, which has the same steps as those in Comparative Example 3, except that the pressure is 45 MPa. The specific steps are as follows:
[0090] S1. Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber, such as Figure 8 As shown, the cold pressing mold consists of two mold units, which are arranged in parallel up and down, and a gap is reserved in the middle for inserting the plate. The length of each mold unit is 4800mm and the width is 5100mm. The width of the gap between the two mold units is 2450mm.
[0091] S2, using 04Cr 13 Ni5Mo steel plate, cutting and blanking, its annular direction is consistent with the rolling direction of the steel plate, such as Fig. 9 As shown, a 50mm cutting margin is left around each side to remove burrs and obtain the workpiece to be processed;
[0092] S3. Place the workpieces to be processed into the heating furnace, with a gap of 100 mm between the workpieces to ensure uniform heating during heating, facilitate lifting and ensure safety, and obtain preheated workpieces;
[0093] S4, placing the preheated workpiece into a hot pressing mold, applying a pressure of 45 MPa at a pressing angle of 140°, performing hot pressing, holding for 2 minutes, and then performing secondary heating, heating to 1050°C and keeping the temperature for 2 minutes, then quickly taking it out and extremely cooling it to 180°C to obtain a shaped workpiece;
[0094] S5. After measuring the finalized workpiece, perform shape calibration, and draw the contour cutting line after the tolerance requirements are met; wherein, the external cutting angle of the finalized workpiece after shape calibration is 120°;
[0095] S6. According to the cutting line, use a plasma cutting machine to cut the excess, and directly use carbon arc gouging to process the shell surface of the shaped workpiece, and the size is controlled within 2mm;
[0096] S7. Use CNC gantry milling to cut out the groove to obtain the pump impeller chamber, which is recorded as hot pressing 120°.
[0097] During the cold pressing test, cracks appeared in the samples pressed at 120° and 130°, while the samples pressed at 138°, 140° and 142° were intact.
[0098] In order to further compare the effects of cold pressing and hot pressing on the mechanical properties of the pump impeller chamber, the pump impeller chambers obtained in Example 2 and Comparative Examples 3 to 4 were subjected to tensile tests and Charpy pendulum tests, respectively. The results are shown in Tables 1 and 2:
[0099] Table 1 is a comparison table of the tensile strength, specified plastic elongation strength, and post-fracture growth rate of the pump runner chamber obtained in Example 2 and Comparative Examples 3 to 4
[0100] product Tensile strength / MPa Specified plastic elongation strength / MPa Growth rate after breaking / % Comparative Example 3 Hot pressing 90° 1060 839 9.0 Comparative Example 4 Hot pressing 120° 1051 829 8.5 Example 2 Cold Pressed 140° 1037 944 13.5
[0101] Note: Test equipment: microcomputer-controlled electronic universal testing machine model TSE225D;
[0102] Environmental conditions: temperature 20°C, humidity 50% RH; test standard: GB / T228.1-2021.
[0103] Table 2 is a comparison table of Charpy pendulum impact tests of the pump impeller chambers prepared in Example 2 and Comparative Examples 3 to 4.
[0104]
[0105] Note: Testing equipment: PIT452D metal pendulum impact tester;
[0106] Environmental conditions: temperature 20℃, humidity 60%RH; test standard: GB / T229-2020.
[0107] By comparing and analyzing the test results in Table 1 and Table 2, we found that:
[0108] For the pump impeller chambers hot-pressed at 90° and 120°, the average absorbed energy was 219J and 213J, respectively, showing relatively low impact toughness. This is because the hot pressing process affects the grain structure of the pump impeller chamber, resulting in a decrease in its mechanical properties. This is not ideal for components such as the pump impeller chamber that need to withstand high pressure and impact loads; although it is within an acceptable range, the fracture behavior of the pump impeller chamber in the stress concentration area will be affected due to the reduction in mechanical properties, thereby increasing the risk of fracture.
[0109] For the pump impeller chamber cold pressed at 140°, the average absorbed energy is 232J, which is relatively high, showing better impact toughness. This is because the cold pressing process can maintain the grain structure of the pump impeller chamber and will not have a negative impact on its mechanical properties. Therefore, the cold pressed pump impeller chamber has a relatively stable tensile strength and a higher specified plastic elongation strength. At the same time, its post-fracture growth rate is also relatively high, which means that the pump impeller chamber has better deformation ability when impacted, which helps to reduce the impact of the impact load on the pump impeller chamber.
[0110] Figure 1 This is a product picture of the pump runner chamber of Example 2 of the present invention. Figure 1 It was concluded that the cold pressed 140° sample had no defects and met the processing requirements.
[0111] Figure 2 This is a tensile strength test curve of the pump runner chamber of Example 2 of the present invention. Figure 2 It was found that the cold pressed 140° sample yielded at 81 kN and broke at an elongation of about 73 mm.
[0112] Figure 3 This is the product picture of the pump runner chamber of comparative example 3 of the present invention. Figure 3 It was concluded that the hot pressed 90° sample had no defects and met the processing requirements.
[0113] Figure 4 This is a tensile strength test curve of the pump runner chamber of Comparative Example 3 of the present invention. Figure 4 It was found that the hot pressed 90° sample yielded at 81 kN and broke at an elongation of about 58 mm.
[0114] Figure 5 This is the product picture of the pump runner chamber of Comparative Example 4 of the present invention. Figure 5 It was concluded that the sample hot-pressed at 120° had no defects and met the processing requirements;
[0115] Figure 6 This is a tensile strength test curve of the pump runner chamber of Comparative Example 4 of the present invention. Figure 6 It was found that the hot pressed 120° sample yielded at 81 kN and broke at an elongation of about 61 mm.
[0116] After comprehensive consideration, cold pressing is a better choice for components such as pump impeller chambers that need to withstand high pressure and impact loads. Cold pressing can maintain the grain structure and mechanical properties of the pump impeller chamber, making the tensile strength and specified plastic elongation strength more stable and reliable; at the same time, cold pressing can provide higher impact resistance, which helps the pump impeller chamber maintain stable performance in actual use.
[0117] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0118] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for cold pressing a pump runner chamber, characterized in that: The steps include: Prepare the cold pressing mold according to the shape, size and processing accuracy requirements of the pump impeller chamber; The plate is used as the workpiece to be processed, the workpiece to be processed is placed in a cold pressing mold, and a pressure of 15MPa to 30MPa is applied at a pressing angle of 140° to perform cold pressing to obtain a shaped workpiece; The workpiece is calibrated to meet the tolerance requirement of 140±2° for the external cutting angle of the workpiece, and then the cutting allowance and external surface treatment are performed to obtain a qualified workpiece. A groove is cut on the qualified finalized workpiece to obtain a pump impeller chamber.
2. A method for cold pressing a pump runner chamber according to claim 1, characterized in that: During the cold pressing process, the pressing rate is 5 mm / s to 8 mm / s.
3. The method for cold pressing a pump runner chamber according to claim 1, characterized in that: Cold pressing is carried out at room temperature.
4. A method for cold pressing a pump runner chamber according to claim 1, characterized in that: The pressing time of the cold pressing process is 2 minutes.
5. The method for cold pressing a pump runner chamber according to claim 1, characterized in that: The cold pressing mold consists of two identical mold units, each of which is an arc-shaped plate, and the outer cutting angle of the mold unit is 140°. The two mold units are arranged parallel to each other up and down, and a gap is reserved in the middle for inserting the plate.
6. The method for cold pressing a pump runner chamber according to claim 1, characterized in that: Leave a cutting allowance on the workpiece to be processed, draw a contour cutting line on the qualified finalized workpiece, and cut the allowance according to the contour cutting line.
7. The method for cold pressing a pump runner chamber according to claim 1, characterized in that: The outer surface of the pump impeller chamber is processed by carbon arc gouging, the thickness of which is 1mm to 2mm, and the oxide layer and appearance defects on the outer surface of the shaped workpiece are polished to a whitening treatment.
8. The method for cold pressing a pump runner chamber according to claim 1, characterized in that: The plate is selected from 04Cr 13 Ni5Mo steel plate, carbon steel or 304 stainless steel.
9. The method for cold pressing a pump runner chamber according to claim 1, characterized in that: There are no defects such as cracks, bubbles, folding and inclusions on the surface of the workpiece to be processed.
Citation Information
Patent Citations
Tool device for runner chamber profiling, manufacturing method and runner chamber profiling method
CN115532944A
Thermal creep and diffusion bonding composite manufacturing method for blade front edge titanium alloy reinforced edge
CN116000195A
Spherical runner chamber with welding structure
CN218882593U
Method for manufacturing ultra high strength steel parts
KR100902857B1