Longitudinal beam rear section stamping process die and process method
By using the inverted "several" shape lower die section and floating core in the stamping process of the rear section of the longitudinal beam, the problems of unevenness of the bottom surface of the longitudinal beam and the R-angle defects at the bends in the traditional stamping process are solved, and high-precision 零件成型。
Patent Information
- Application Number
- CN202411041343.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
When manufacturing parts of the back section of the longitudinal beam, traditional stamping technology is prone to unevenness on the bottom of the longitudinal beam and the extrusion R angle defects at the bends, which affects the accuracy and welding quality of the parts.
A new longitudinal beam rear stamping process mold and process method is adopted, including matching upper and lower dies. The lower die section is in an inverted "several" shape, with step surfaces and rounded corners connected, combining floating cores and The synergistic effect of the upper mold complements the cross-sectional design through specific molding steps and processes to ensure that the sheet is kept under pressure and controlled bending during molding.
The high flatness and good precision of the bottom surface of the longitudinal beam are achieved, which avoids the problem of extruded R angle protrusions, and improves the overall accuracy and welding quality of the parts.
Smart Images

Figure CN118905056A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile parts stamping, and in particular to a longitudinal beam rear section stamping process die and a process method. Background Art
[0002] The rear section of the longitudinal beam is located at the rear end of the automobile frame and is an important component that bears force and collision. In recent years, with the innovative changes in the exterior styling of vehicle models and the increasing demand for body functionality, the part features of the rear section of the longitudinal beam have changed from the previous straight to the current irregular type, and a bend has appeared at the end of the longitudinal beam. This type of part shape has brought new challenges to the stamping process of the longitudinal beam.
[0003] There are two traditional stamping processes. The first stamping process is: drawing -> trimming -> positive shaping -> side shaping -> punching. Square material is used for drawing. The upper die is a concave die and the lower die is a convex die. The part is placed on the "J"-shaped convex die. During drawing, the blank holder is first lifted up, and the blank holder and the upper die first press the flange surface. Then the middle of the sheet contacts the lower die and slowly forms downward. For parts manufactured by this type of stamping process, since the middle of the sheet is formed last, the bottom surface of the product is subjected to the extrusion stress of the two side walls, resulting in the defect of uneven bottom surface of the longitudinal beam (such as Figure 8 As shown in the figure, the parts are not properly welded, which results in deviation in the parts precision and affects the subsequent body-in-white welding precision.
[0004] The second traditional process is: blanking->forming->front shaping->side shaping->punching. Blanking sheets (special-shaped materials) are used for forming, and the parts are placed in a "U" shape in the stamping direction. During forming, the middle floating core is lifted up, and the floating core and the upper die first press the middle bottom surface, and then the sheets on both sides gradually contact the lower die to form the flange surface of the part. Parts manufactured by this type of stamping process are free-forming because the sheets are not constrained on both sides. At the corners of the parts, the sheets are freely formed without constraints in three-dimensional space, and it is easy to produce R-angle defects in the corner shaping part of the parts (such as Fig. 9 As shown in the figure, during the forming process, the material at the R angle part bows upward to form an R angle extrusion defect. After the final forming, the material overlaps here.
[0005] Therefore, in order to solve the technical problems of uneven bottom surface of the longitudinal beam and R-angle defects easily generated in the corner shaping part of the parts encountered in the above-mentioned traditional stamping process, the present invention proposes a new longitudinal beam rear section stamping process mold and process method. Summary of the invention
[0006] The present invention provides a longitudinal beam rear section stamping process die and process method, which can solve the technical problems encountered in the traditional stamping process, such as the uneven bottom surface of the longitudinal beam and the easy generation of R angle defects in the corner molding part of the parts.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A stamping die for the rear section of a longitudinal beam, comprising an upper die and a lower die that match each other, wherein the upper die is a convex die and the lower die is a concave die; the lower die intercepts at least one lower die section, wherein the lower die section is in an inverted "J" shape according to the product structure, a step surface formed by extending outward along the product structure trend of one side wall of the "J"-shaped lower die section to form a first product flange surface, and a step surface formed by extending outward along the product structure trend of the other side wall of the "J"-shaped lower die section to form a second product flange surface, the first product flange surface and the corresponding side wall of the lower die section are transitioned by a fillet R2, and the second product flange surface and the corresponding side wall of the lower die section are connected by a fillet R1; after process supplementation of each lower die section, a process supplementary section of the lower die section is obtained, and the process supplementary section is extended along the product structure to form a process supplementary surface of the lower die; the chamfered positions of the lower die section at both ends of the "J"-shaped positive end surface are set as parting lines, and the lower die is provided with at least one elastically lifting floating core between the two parting lines;
[0009] The process supplementary cross section includes a first process supplementary flange surface, a first process supplementary side wall surface, a second process supplementary flange surface, a second process supplementary side wall surface, a third process supplementary flange surface and a fourth process supplementary flange surface;
[0010] The second product flange surface extends outward along the product structure trend to form the fourth process supplementary flange surface, the end of the fourth process supplementary flange surface extends upward to form the second process supplementary side wall surface, and the fourth process supplementary flange surface and the second process supplementary side wall surface are connected by a fillet R3; the other end of the second process supplementary side wall surface extends horizontally outward to form the second process supplementary flange surface; the second process supplementary flange surface and the second process supplementary side wall surface are connected by a fillet R4;
[0011] The first product flange surface extends outward along the product structure trend to form the third process flange supplementary surface; the end of the third process supplementary flange surface extends upward to form the first process supplementary side wall surface; the third process supplementary flange surface and the first process supplementary side wall surface are directly connected by a fillet R5; the other end of the first process supplementary side wall surface extends outward horizontally to form the first process supplementary flange surface; the first process supplementary side wall surface and the first process supplementary flange surface are connected by a fillet R6;
[0012] The first process supplementary flange surface and the second process supplementary flange surface are flush with each other.
[0013] Furthermore, the sum of the straight line lengths of the first product flange surface and the third process supplementary flange surface is 3 mm to 5 mm longer than the final trimming line of the product.
[0014] Furthermore, the sum of the straight line lengths of the second product flange surface and the fourth process supplementary flange surface is 3 mm to 5 mm longer than the final trimming line of the product.
[0015] Furthermore, the angle between the first process supplementary side wall surface and the third process supplementary flange surface is set to 90° to 100°, and the angle between the second process supplementary side wall surface and the fourth process supplementary flange surface is set to 90° to 100°.
[0016] Furthermore, the radii of the rounded corners R3 and R5 are both 3 mm to 5 mm, and the radii of the rounded corners R4 and R6 are both set to 8 mm to 15 mm.
[0017] A longitudinal beam rear section stamping process method, based on the longitudinal beam rear section stamping process die mentioned above, includes the following forming steps in the forming process:
[0018] S1: The first process supplementary flange surface and the second process supplementary flange surface are arranged horizontally and flushly, so that the sheet placed on the upper side can be placed horizontally, and the floating core between the two parting lines in the lower mold supports the sheet; wherein the sheet is a square material;
[0019] S2: The upper die is pressed downward, and the bottom of the upper die contacts the sheet material, and together with the floating core, the sheet material within the parting line is squeezed. The first pre-bending die surface is formed through the fillets R4 and R6, so that the sheet material is bent downward. After the sheet material is bent, both sides slide into the cavity formed between the first process supplementary side wall surface, the second process supplementary side wall surface and the corresponding side wall surface of the upper die. At this time, the sheet material within the parting line has been pressure-formed, and is always under pressure in the subsequent forming process to maintain the flatness of the bottom surface of the product;
[0020] S3: The upper die continues to press the sheet downward, and the sheet is guided by the fillets R1 and R2 of the convex R corners of the lower die, and the upper die matches the corresponding convex R corners to form a second pre-bending die surface, further pre-pressing the product into a "J" shape. At the same time, the upper die continues to press both sides of the sheet toward the corresponding first process flange surface and second process flange surface respectively;
[0021] S4: The upper die continues to press the sheet down to the limit position, and the two fillets on the inner side of the bottom of the lower die form the third forming die surface, so that the connecting fillets of the two side walls and the bottom of the product are formed, and the two ends of the sheet are completely aligned with the first process flange surface and the second process flange surface, so that the product is finally formed.
[0022] Furthermore, the cross-sectional length L of the sheet material = product cross-sectional length + third process supplementary flange surface length + fourth process supplementary flange surface length + fillet R3 length + fillet R5 length + first process supplementary side wall length + second process supplementary side wall length + reserved length, where the reserved length is 20 mm to 30 mm.
[0023] Furthermore, after the forming process, trimming, front shaping, side shaping and punching are also included.
[0024] The beneficial effects of the present invention are:
[0025] The present invention forms a mold surface supporting both ends of the sheet material by supplementing the flange surface in the first process and supplementing the flange surface in the second process to be flush with each other. The middle part of the sheet material is supported by the floating material core. At the beginning of the sheet material forming, the bottom surface of the product is always clamped and pressed by the floating material core 12 and the corresponding upper mold surface. When the upper mold is pressed down, the sheet material is pre-bent by using the fillet R6 and the fillet R4 as the fillet mold surface. At this time, the sheet material within the parting line has been pressure-formed and is always under pressure in the subsequent forming process. Therefore, the bottom surface of the longitudinal beam formed by the present invention has high flatness and good precision. In the process of the upper mold moving downward, the sheet material outside the parting line is formed in the cavity formed by the lower mold and the upper mold. The sheet material will be affected by the convex R angle on the mold surface to form a pre-bend, thereby limiting the forming of the sheet material in this area, so that it is within a controlled range, not completely emptied free forming. In this process, it can be understood that the convex R angle has a friction effect on the sheet material, and the side wall of the part is subjected to tensile stress upward in this direction, avoiding the side wall of the part from being squeezed downward, thereby solving the problem of the protruding R angle at the bottom. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The specific embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings, wherein:
[0027] Figure 1 It is a schematic diagram of the lower mold section and the process supplementary section in the present invention;
[0028] Figure 2 This is a schematic diagram of the initial placement of the sheet material in the forming step S1 of the present invention;
[0029] Figure 3 It is a schematic diagram of the contact between the sheet material and the upper mold in the molding step S1 of the present invention;
[0030] Figure 4 This is a schematic diagram of the first pre-bending of the sheet material by the upper die in the forming step S2 of the present invention. Figure 1 ;
[0031] Figure 5 It is a schematic diagram of the sheet material falling between the upper die and the lower die after the sheet material is pre-bent by the upper die for the first time in the forming step S2 of the present invention;
[0032] Figure 6It is a schematic diagram of the sheet material being pre-bent by the upper die for the second time in the forming step S3 of the present invention;
[0033] Figure 7 This is a schematic diagram of the final forming of the product in the forming step S4 of the present invention;
[0034] Figure 8 This is a physical picture of the uneven bottom surface of the longitudinal beam caused by traditional technology;
[0035] Fig. 9 This is a physical picture of the R corner defect caused by the traditional process;
[0036] Figure ID:
[0037] 1-upper die, 2-lower die, 3-first product flange surface, 4-second product flange surface, 5-first process supplementary flange surface, 6-first process supplementary side wall surface, 7-second process supplementary flange surface, 8-second process supplementary side wall surface, 9-third process supplementary flange surface, 10-fourth process supplementary flange surface, 11-parting line, 12-floating core, 13-sheet material. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may be a central component. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may be a central component at the same time. When a component is considered to be "set on" another component, it may be directly set on the other component or there may be a central component at the same time. When a component is referred to as being "set in the middle", it does not only mean being set in the middle, as long as it is not set at both ends within the range defined by the middle. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0041] Reference Figures 1 to 7 As shown, a longitudinal beam rear section stamping process die comprises an upper die 1 and a lower die 2 that match each other, the upper die 1 is set as a convex die, and the lower die 2 is set as a concave die; the lower die 2 intercepts at least one lower die section, such as Figure 1 As shown, the cross section of the lower die is in an inverted "J" shape according to the product structure, and the step surface formed by extending one side wall of the "J" shape of the lower die cross section outward along the product structure trend is set as the first product flange surface 3, and the step surface formed by extending the other side of the "J" shape of the lower die cross section outward along the product structure trend wall is set as the second product flange surface 4. The first product flange surface 3 and the corresponding side wall of the lower die cross section are transitioned by a fillet R2, and the second product flange surface 4 and the corresponding side wall of the lower die cross section are connected by a fillet R1; the lower die cross section is obtained after the process is supplemented for each lower die cross section. The process supplementary section of the surface is extended along the product structure to form the process supplementary surface of the lower mold 2; the chamfered positions of the lower mold section at both ends of the "J"-shaped positive end surface are set as parting lines 11, and the lower mold is located between the two parting lines 11 and is provided with at least one elastically lifting floating core 12; the floating core 12 is used to support the sheet material 13 at the beginning of molding, and in the process of continuous downward pressure of the upper mold 1 to deform the two ends of the sheet material 13, the bottom surface of the product corresponding to the middle of the "J"-shaped is always clamped and held by the floating core 12 and the corresponding upper mold surface, thereby improving the molding accuracy.
[0042] The process supplementary cross section includes a first process supplementary flange surface 5, a first process supplementary side wall surface 6, a second process supplementary flange surface 7, a second process supplementary side wall surface 8, a third process supplementary flange surface 9 and a fourth process supplementary flange surface 10;
[0043] The second product flange surface 4 extends outward along the product structure trend to form a fourth process supplementary flange surface 10. The end of the fourth process supplementary flange surface 10 extends upward to form a second process supplementary side wall surface 8. The fourth process supplementary flange surface 10 and the second process supplementary side wall surface 8 are connected by a fillet R3; the other end of the second process supplementary side wall surface 8 extends horizontally outward to form a second process supplementary flange surface 7; the second process supplementary flange surface 7 and the second process supplementary side wall surface 8 are connected by a fillet R4.
[0044] The first product flange surface 3 extends outward along the product structure trend to form a third process flange supplementary surface 9; the end of the third process supplementary flange surface 9 extends upward to form a first process supplementary side wall surface 6; the third process supplementary flange surface 9 and the first process supplementary side wall surface 6 are directly connected by a fillet R5; the other end of the first process supplementary side wall surface 6 extends horizontally outward to form a first process supplementary flange surface 5, and the first process supplementary side wall surface 6 and the first process supplementary flange surface 5 are connected by a fillet R6.
[0045] The first process supplementary flange surface 5 and the second process supplementary flange surface 7 are flush with each other, and this arrangement can ensure that the initial sheet material 13 is stable when placed.
[0046] The sum of the straight line lengths of the first product flange surface 3 and the third process supplementary flange surface 9 is 3mm to 5mm longer than the final trimming line of the product. The sum of the straight line lengths of the second product flange surface 4 and the fourth process supplementary flange surface 10 is 3mm to 5mm longer than the final trimming line of the product.
[0047] The included angle between the first process supplementary side wall surface 6 and the third process supplementary flange surface 9 is set to 90° to 100°, and the included angle between the second process supplementary side wall surface 8 and the fourth process supplementary flange surface 10 is set to 90° to 100°.
[0048] The radii of the rounded corners R3 and R5 are both 3 mm to 5 mm, and the radii of the rounded corners R4 and R6 are both set to 8 mm to 15 mm.
[0049] A longitudinal beam rear section stamping process method is based on the longitudinal beam rear section stamping process die mentioned above, including forming, trimming, positive shaping, side shaping, and punching; the above process die is used in the forming process, which includes the following forming steps:
[0050] S1: Figure 2 As shown, the first process supplementary flange surface 5 and the second process supplementary flange surface 7 are arranged horizontally and flush, so that the sheet 13 placed on the top can be placed horizontally, and the floating core 12 between the two parting lines 11 in the lower mold supports the sheet 13; wherein the sheet is square material; in order to ensure the control of the sheet by the convex R angle during the forming process, and uniform force and flow on both sides of the sheet, the square material needs to have sufficient cross-sectional length, and the technical formula of the cross-sectional length L of the sheet is as follows, L = product cross-sectional length + third process supplementary flange surface length + fourth process supplementary flange surface length + fillet R3 length + fillet R5 length + first process supplementary side wall length + second process supplementary side wall length + reserved length, wherein the reserved length is 20mm to 30mm.
[0051] S2: Figure 2 As shown, the upper mold 1 is pressed downward, the bottom of the upper mold 1 contacts the sheet material 13, and in the process of pressing downward, it and the floating material core 12 jointly squeeze the sheet material 13 within the parting line, as shown in FIG. Figure 3 As shown, the first pre-bending die surface is formed by the fillets R4 and R6, so that the sheet 13 is bent downward; after the sheet 13 is bent, both sides slide into the cavities formed between the first process supplementary side wall surface 6, the second process supplementary side wall surface 8 and the corresponding side wall surface of the upper die, as shown in FIG. Figures 4 to 5 As shown, at this time, the sheet material 13 within the parting line 11 has been formed by pressure, and is always under pressure in the subsequent forming process to maintain the flatness of the bottom surface of the product;
[0052] S3: The upper die 1 continues to press the sheet 13 downward. Figure 6 As shown, the rounded corners R1 and R2 in the convex R corners of the lower die 2 are guided, and the corresponding convex R corners of the upper die 1 are matched to form a second pre-bending die surface, so that the product is further pre-pressed into a "J" shape, and at the same time, the upper die 1 continues to press the two sides of the sheet 13 toward the corresponding first process flange surface 3 and second process flange surface 4 respectively;
[0053] S4: The upper die 1 continues to press the sheet 13 to the limit position, and the two fillets on the inner side of the bottom of the lower die 2 form the third forming die surface, so that the connecting fillets of the two side walls and the bottom of the product are formed, and the two ends of the sheet 13 are completely aligned with the first process flange surface 3 and the second process flange surface 4. Figure 7 As shown, the product is finally formed.
[0054] The process supplement section adopted in the present invention is different from the traditional process supplement. The traditional process supplement only extends the flange surface 3 of the first product and the flange surface 4 of the second product, resulting in the sheet 13 being in a free state during the forming process. Since the two sides of the sheet are not constrained, it is a free forming process. At the corner of the part, the sheet is freely formed without constraints in the three-dimensional space, and the defect of squeezing R angle is easy to occur at the corner molding part of the part (such as Fig. 9 As shown), that is, during the forming process, the material in the R-angle part is arched upward to form an R-angle extrusion defect; the present invention forms a mold surface supporting both ends of the sheet material 13 by supplementing the flange surface 5 through the first process and the flange surface 7 through the second process, and the middle part of the sheet material 13 is held up by the floating material core 12. At the beginning of the forming of the sheet material 13, the sheet material 13 is supported by the floating material core 12. When the upper mold 1 is pressed down, the fillet R6 and the fillet R4 are used as the fillet mold surface to pre-bend the sheet material 13. At this time, the sheet material 13 within the parting line 11 has been pressure-formed and has been under pressure during the subsequent forming process. Therefore, the bottom surface of the longitudinal beam formed by the present invention has high flatness and good precision. During the downward movement of the upper mold 1, the sheet 13 outside the parting line 11 is formed in the cavity formed by the lower mold 2 and the upper mold 1. The sheet 13 will be affected by the convex R angle on the mold surface to form a pre-bend, thereby limiting the forming of the sheet 13 in this area, so that it is within a controlled range, rather than completely free-formed. In this process, it can be understood that the convex R angle has a friction effect on the sheet 13, and the tensile stress on the side wall of the part in this direction is upward, which prevents the side wall of the part from being squeezed downward, thereby solving the problem of the protruding R angle at the bottom.
[0055] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall be included in the scope of the technical solution of the present invention.
Claims
1. A longitudinal beam rear section stamping process die, comprising an upper die and a lower die matching each other, wherein the upper die is a convex die and the lower die is a concave die; It is characterized in that The lower die cuts off at least one lower die section, and the lower die section is in an inverted "J" shape according to the product structure. The step surface formed by extending outward along the product structure trend of one side wall of the "J"-shaped lower die section is set as the first product flange surface, and the step surface formed by extending outward along the product structure trend of the other side wall of the "J"-shaped lower die section is set as the second product flange surface. The first product flange surface and the corresponding side wall of the lower die section are transitioned by a fillet R2, and the second product flange surface and the corresponding side wall of the lower die section are connected by a fillet R1; the process supplement section of the lower die section is obtained by process supplementation, and the process supplement section is extended along the product structure to form the process supplement surface of the lower die; the chamfered positions of the lower die section at both ends of the "J"-shaped positive end surface are set as parting lines, and the lower die is provided with at least one elastically lifting floating core between the two parting lines; The process supplementary cross section includes a first process supplementary flange surface, a first process supplementary side wall surface, a second process supplementary flange surface, a second process supplementary side wall surface, a third process supplementary flange surface and a fourth process supplementary flange surface; The second product flange surface extends outward along the product structure trend to form the fourth process supplementary flange surface; the end of the fourth process supplementary flange surface extends upward to form the second process supplementary side wall surface, and the fourth process supplementary flange surface and the second process supplementary side wall surface are connected by a fillet R3; the other end of the second process supplementary side wall surface extends outward horizontally to form the second process supplementary flange surface; the second process supplementary flange surface and the second process supplementary side wall surface are connected by a fillet R4; The first product flange surface extends outward along the product structure trend to form the third process flange supplementary surface; the end of the third process supplementary flange surface extends upward to form the first process supplementary side wall surface; the third process supplementary flange surface and the first process supplementary side wall surface are directly connected by a fillet R5; the other end of the first process supplementary side wall surface extends outward horizontally to form the first process supplementary flange surface; the first process supplementary side wall surface and the first process supplementary flange surface are connected by a fillet R6; The first process supplementary flange surface and the second process supplementary flange surface are flush with each other.
2. A longitudinal beam rear section stamping die according to claim 1, It is characterized in that The sum of the straight line lengths of the first product flange surface and the third process supplementary flange surface is 3 mm to 5 mm longer than the final trimming line of the product.
3. A longitudinal beam rear section stamping die according to claim 1, It is characterized in that The sum of the straight line lengths of the second product flange surface and the fourth process supplementary flange surface is 3 mm to 5 mm longer than the final trimming line of the product.
4. A longitudinal beam rear section stamping die according to claim 1, It is characterized in that The included angle between the first process supplementary side wall surface and the third process supplementary flange surface is set to 90° to 100°, and the included angle between the second process supplementary side wall surface and the fourth process supplementary flange surface is set to 90° to 100°.
5. The longitudinal beam rear section stamping die according to claim 1, It is characterized in that The radii of the rounded corners R3 and R4 are both 3 mm to 5 mm, and the radii of the rounded corners R4 and R6 are both set to 8 mm to 15 mm.
6. A stamping process for the rear section of a longitudinal beam, It is characterized in that A longitudinal beam rear section stamping process die according to any one of claims 1 to 7, wherein the forming process comprises the following forming steps: S1: The first process supplementary flange surface and the second process supplementary flange surface are arranged horizontally and flushly, so that the sheet placed on the upper side can be placed horizontally, and the floating core between the two parting lines in the lower mold supports the sheet; wherein the sheet is a square material; S2: The upper die is pressed downward, and the bottom of the upper die contacts the sheet material, and together with the floating core, the sheet material within the parting line is squeezed. The first pre-bending die surface is formed through the fillets R4 and R6, so that the sheet material is bent downward. After the sheet material is bent, both sides slide into the cavity formed between the first process supplementary side wall surface, the second process supplementary side wall surface and the corresponding side wall surface of the upper die. At this time, the sheet material within the parting line has been pressure-formed, and is always under pressure in the subsequent forming process to maintain the flatness of the bottom surface of the product; S3: The upper die continues to press the sheet downward, and the sheet is guided by the fillets R1 and R2 of the convex R corners of the lower die, and the upper die matches the corresponding convex R corners to form a second pre-bending die surface, further pre-pressing the product into a "J" shape. At the same time, the upper die continues to press both sides of the sheet toward the corresponding first process flange surface and second process flange surface respectively; S4: The upper die continues to press the sheet down to the limit position, and the two fillets on the inner side of the bottom of the lower die form the third forming die surface, so that the connecting fillets of the two side walls and the bottom of the product are formed, and the two ends of the sheet are completely aligned with the first process flange surface and the second process flange surface, so that the product is finally formed.
7. A longitudinal beam rear section stamping process method according to claim 6, It is characterized in that The cross-sectional length L of the sheet material = product cross-sectional length + third process supplementary flange surface length + fourth process supplementary flange surface length + fillet R3 length + fillet R5 length + first process supplementary side wall length + second process supplementary side wall length + reserved length, where the reserved length is 20 mm to 30 mm.
8. A longitudinal beam rear section stamping process method according to claim 6, It is characterized in that After the forming process, it also includes trimming, front shaping, side shaping and punching.