Preparation method of rare earth doped flower-like alloy (at) COFs derived porous carbon wave-absorbing material
Through the combination of rare earth doped flower-like alloys and COFs-derived porous carbon materials, the problems of single loss mode of microwave absorption materials and narrow absorption bandwidth are solved, and the microwave absorption performance of ultra-wideband is achieved, which is suitable for stealth applications in the military and civilian fields.
Patent Information
- Application Number
- CN202410958505.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing microwave absorption materials have problems such as single energy loss mode, large filling ratio and density, and narrow microwave absorption bandwidth and functions, resulting in limited applications in military and civilian fields.
Using a combination of rare earth doped flower-like alloys and covalent organic frames (COFs) derived porous carbon materials, the preparation conditions of traditional powder covalent organic frame materials are changed to combine them with rare earth-doped flower-like FeNi alloys to form rare earth-based Doped flower-like alloy @COFs derived porous carbon absorbing materials, adjust electron migration and dipole site density, and achieve electromagnetic synergistic loss.
Significantly improves the microwave absorption performance of the material, realizes ultra-wideband absorption, covers the frequency band of 2 to 18GHz, has low RCS characteristics, is suitable for stealth applications of military equipment and electronic devices, and achieves excellent results with low filling ratio and thin thickness. Absorption effect.
Smart Images

Figure CN118905211A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a carbon wave-absorbing material. Background Art
[0002] Microwave absorbing materials can eliminate the adverse effects of electromagnetic waves on human health, electronic equipment and military security. High-performance microwave absorbing materials that are "thin, light, wide and strong" with wide absorption frequency band, strong microwave attenuation ability, low density and low thickness can be promoted and applied. Carbon-based absorbers have high conductivity, strong dielectric loss and good chemical stability, especially three-dimensional porous carbon-based electromagnetic wave absorbers have been widely developed in the field of wave absorption. The three-dimensional porous structure not only reduces the density of the material, but also improves the multiple reflections of the incident electromagnetic wave, further optimizing the impedance matching. Therefore, three-dimensional porous carbon-based absorbers are expected to achieve the goals of low density, thin thickness, wide absorption bandwidth and strong absorption. Covalent organic frameworks (COFs) are a class of organic porous crystalline materials composed of light elements such as C, O, N, and B connected by reversible strong covalent bonds (CC, CO, BO, CN, etc.). The ordered structure of COFs can produce high specific surface area and abundant nanopores, and its performance even exceeds that of metal organic frameworks and zeolites. However, the ideal microwave absorber should be a composite material that can achieve electromagnetic synergy and has excellent dielectric loss and magnetic loss capabilities.
[0003] So far, there is little research on COFs composite materials in the field of microwave absorbing materials. 3 O 4 Combined with porous COFs materials, core-shell Fe 3 O 4 @C composite material. The hollow core-shell porous structure after pyrolysis is conducive to multiple reflections and scattering of electromagnetic waves, retaining the high specific surface area and porous characteristics of COFs materials. When the thickness is 1.8mm, the effective absorption bandwidth (EAB) is only 5.2GHz, and the minimum reflection loss (RL min ) is only -50.05dB(Zhu X,Dong Y,Pan F,Xiang Z,Liu Z,Deng B,Zhang X,Shi Z,Lu W,Covalent organicframework-derived hollow core-shell Fe / Fe 3 O 4@porous carbon composites with corrosion resistance for lightweight and efficient microwave absorption, Composites Communications, 2021, 25: 100731.). Jian et al. formed two COFs by carbonyl-amine condensation polymerization and in situ coating on COF-derived Co / C hybrids, which is beneficial to improve the interfacial polarization. Among them, Co / C@p-phenylenediamine-trialdehyde pyrogallol and Co / C@1,3,5-tris(4-aminophenyl)benzene-terephthalaldehyde composites, their RL min Only -48.78dB and -50.6dB were reached (Li J, Tian W, Liu Y, Wu B, Jian X, Deng L, Achieving enhanced microwave absorption performance based on metal / covalent organic frameworks-derived heterostructures, Composites Part B: Engineering, 2022, 245: 110199.). The above studies show that due to its unique porous structure, COFs have great advantages in the field of microwave absorption. However, when a single COFs material is pyrolyzed under a protective gas, it only has a single conductive loss and cannot reasonably carry out electromagnetic synergistic loss of electromagnetic wave energy. This leads to the fact that COFs-derived composite materials often do not have broadband absorption, the working frequency band is limited, and a high filling ratio and high matching thickness are required to achieve ideal microwave absorption performance, which is not conducive to production and application in military and civilian fields. Summary of the invention
[0004] The present invention aims to solve the technical problems of existing microwave absorbing materials, namely, single energy loss mode, large filling ratio and density, narrow microwave absorption bandwidth and single function, and provide a method for preparing rare earth doped flower-shaped alloy @COFs derived porous carbon absorbing material.
[0005] The preparation method of the rare earth doped flower-shaped alloy @COFs derived porous carbon absorbing material of the present invention is carried out according to the following steps:
[0006] 1. Dissolve nickel chloride hexahydrate, rare earth chloride hexahydrate and ferric chloride hexahydrate in distilled water, stir evenly, then add NaOH and continue stirring, then add hydrazine hydrate aqueous solution with a volume concentration of 80% to 85% as a reducing agent to obtain a light green solution, then pour the light green solution into a polytetrafluoroethylene-lined autoclave, and react in a drying oven at 120°C to 150°C for 8h to 10h;
[0007] The black precipitate was collected by magnetic separation, washed three times with water and three times with anhydrous ethanol to obtain black magnetic particles, and the black magnetic particles were vacuum dried at 50°C to 70°C and recorded as GFN;
[0008] The molar ratio of nickel chloride hexahydrate to ferric chloride hexahydrate is 10:(1-1.2);
[0009] The ratio of the molar amount of the rare earth chloride hexahydrate to the molar amount of nickel chloride hexahydrate and ferric chloride hexahydrate is (0.01-0.05):1;
[0010] The mass ratio of the ferric chloride hexahydrate to NaOH is 1:(5.5-6);
[0011] The mass ratio of the NaOH to the volume ratio of the hydrazine hydrate aqueous solution is 1g:(10mL-13mL);
[0012] 2. Add the GFN prepared in step 1 into a three-necked flask containing toluene, then add 3-aminopropyltriethoxysilane into the above solution under a nitrogen atmosphere, heat the oil bath to 100°C to 110°C and keep warm for 1.8h to 2.5h, then cool the black oily substance to room temperature, wash it with water 2 to 3 times, and then vacuum dry it for 12h to 24h to obtain black magnetic particles, named GFN-NH 2 ;
[0013] The mass ratio of the GFN to the volume ratio of toluene is (0.3 g to 0.4 g): (30 mL to 40 mL);
[0014] The mass ratio of the GFN to the volume ratio of 3-aminopropyltriethoxysilane is (0.3 g to 0.4 g): (1 mL to 2 mL);
[0015] 3. GFN-NH prepared in step 2 2The particles are dispersed in the co-solvent system 1, and then 2,5-dimethoxybenzene-1,4-dicarboxaldehyde monomer and acetic acid solution are added, and after ultrasonic treatment for 3min to 5min, they are transferred to a polytetrafluoroethylene-lined high-pressure reactor, and heated in a drying oven at 120°C to 130°C for 1h to 2h. After natural cooling, the sample is collected in a centrifuge tube, and washed by centrifugation with tetrahydrofuran and acetone for 2 to 3 times respectively, and dried in a vacuum drying oven for 6h to 12h to obtain magnetic particles named GFN-DMTP;
[0016] The co-solvent system 1 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1;
[0017] The GFN-NH 2 The mass ratio of the particles to the volume of the co-solvent system 1 is (0.1 g to 0.15 g): (4 mL to 4.5 mL);
[0018] The mass ratio of the 2,5-dimethoxybenzene-1,4-dicarbaldehyde monomer to the volume ratio of the co-solvent system 1 is (0.01 g to 0.02 g): (4 mL to 4.5 mL);
[0019] The GFN-NH 2 The mass ratio of the particles to the volume of the acetic acid solution is (0.1 g to 0.15 g): (2 mL to 3 mL), and the concentration of the acetic acid solution is 3 mol·L -1 ;
[0020] 4. Disperse the GFN-DMTP prepared in step 3 in the co-solvent system 2, then add 1,3,5-tri(4-aminophenyl)benzene and 2,5-dimethoxybenzene-1,4-dicarboxaldehyde to the above solution, then add acetic acid solution, and ultrasonically homogenize; pour the solution into a polytetrafluoroethylene-lined autoclave, heat the reaction at 60°C to 70°C in a drying oven for 24h to 25h, collect the sample in a centrifuge tube after natural cooling, wash it three times each with tetrahydrofuran and acetone, and then dry it in a vacuum drying oven for 6h to 12h to obtain a fluffy yellow-black product, named GFN@TAPB-DMTP-COF;
[0021] The co-solvent system 2 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1;
[0022] The mass ratio of the GFN-DMTP to the volume ratio of the co-solvent system 2 is (0.05 g to 0.06 g): (20 mL to 30 mL);
[0023] The mass ratio of the GFN-DMTP to the amount of 1,3,5-tris(4-aminophenyl)benzene is (0.05 g to 0.06 g):(0.1 mmol to 0.2 mmol);
[0024] The mass ratio of the GFN-DMTP to the amount of 2,5-dimethoxybenzene-1,4-dicarbaldehyde is (0.05 g to 0.06 g): (0.2 mmol to 0.3 mmol);
[0025] The mass ratio of the GFN-DMTP to the volume of the acetic acid solution is (0.05 g to 0.06 g): (2 mL to 3 mL), and the concentration of the acetic acid solution is 9 mol·L -1 ;
[0026] 5. In a protective gas, calcine the GFN@TAPB-DMTP-COF prepared in step 4 at 600°C to 800°C for 2h to 4h, and then naturally cool to room temperature to obtain a rare earth doped flower-shaped alloy@COFs-derived porous carbon absorbing material.
[0027] The present invention selects rare earth elements to adjust electron migration and dipole site density. The alloy after adding rare earth elements obtains a good coordination state of electron migration, dipole and magnetic loss, and can obtain the maximum effective absorption bandwidth. This provides new insights into the structural design of EMW nanomaterials and is an important extension of the current electromagnetic wave loss mechanism.
[0028] The present invention combines the COF material with the rare earth-doped flower-shaped FeNi alloy by changing the preparation conditions of the traditional powder single covalent organic framework material (COFs). The addition of the rare earth-doped flower-shaped FeNi alloy not only increases the magnetic loss of the material and improves the dielectric properties of the material, but also enriches the heterogeneous interface and enhances the interface polarization, which is beneficial to the attenuation loss of electromagnetic waves, so that the electric field and the magnetic field undergo exchange coupling, and the material produces a dual loss effect based on physical induction in the electromagnetic field, thereby enhancing the attenuation ability of electromagnetic waves. At the same time, the electromagnetic waves undergo multiple reflections and scattering in the holes of the COFs-derived porous carbon, so that the electromagnetic waves are converted into electrical energy and dissipated in the form of heat. On the other hand, the flower-shaped alloy magnetic particles are evenly dispersed in the nitrogen-doped carbon to form a magnetic coupling network, thereby showing better magnetic loss capacity, thereby improving the microwave absorption performance of the material.
[0029] The present invention prepares high-performance rare earth-doped flower-shaped alloy@COFs-derived porous carbon absorbing material (GFN@NPC) by introducing COF-derived porous carbon into rare earth-doped flower-shaped alloy with special microstructure using monomer-mediated strategy. The direct multiple interfaces of the flower-shaped alloy enhance the interface polarization loss, while converting electromagnetic waves into electrical energy, which is dissipated in the form of heat, increasing the conductive loss. The unique electronic transition between the 3d orbital electrons and the 4f orbital of the rare earth-doped alloy causes the local charge to rearrange, giving the material a high saturation magnetization, providing stronger additional magnetic losses, and significantly improving the electromagnetic wave absorption performance. The flower-shaped alloy and raspberry-shaped structure can significantly increase the multiple reflections and scattering of electromagnetic waves, induce electromagnetic coupling, and thus exhibit excellent electromagnetic attenuation characteristics.
[0030] The GFN@NPC absorbing material prepared by the present invention has better dielectric and magnetic properties than a single carbon material, so that the material can be used in a variety of scenarios. At the same time, the CST electromagnetic field simulation software simulates and verifies that the material has low RCS characteristics. The material is designed as a metamaterial, achieving ultra-wideband absorption of 12.24GHz, covering 76.5% of the full frequency band (2-18GHz), which can meet the application of special environments such as military equipment, electronic devices, and protective clothing, especially in stealth aircraft. It is expected to replace traditional absorbing materials. At the same time, the preparation method of the present invention is simple and low in cost, especially it can achieve ultra-wideband absorption at a lower filling ratio and thinner thickness, so it has great industrial production application and promotion value.
[0031] Beneficial effects of the present invention:
[0032] 1. Unique preparation method: The present invention adopts a monomer-mediated growth strategy and calcination to construct a raspberry-like GFN@NPC composite material with multiple non-uniform interfaces, which causes the 4f electrons to transition to the 3d orbit, resulting in ferromagnetic coupling and high spin. At the same time, the long-range magnetic diffraction generated inside the anisotropic flower-shaped alloy makes the rare earth-doped FeNi 10 The alloy exhibits strong magnetic losses;
[0033] 2. Excellent electromagnetic wave absorption ability: The present invention can effectively control electromagnetic parameters by changing the ratio of COFs-derived porous carbon and magnetic alloy. This layered structure of porous carbon and magnetic alloy induces multiple electromagnetic wave scattering and reflection, while increasing the contact surface between the two phases, enriching the interface polarization effect, and significantly improving the electromagnetic wave absorption performance. Therefore, the GFN@NPC composite material with good impedance matching and strong attenuation ability shows an ultra-wide EAB (up to 6GHz). The present invention improves impedance matching while achieving a synergistic effect of electromagnetic loss, thereby obtaining ideal electromagnetic wave absorption performance, so that the obtained composite absorbing material can achieve excellent lightweight microwave absorption performance at a lower coating thickness after being mixed with paraffin, and obtains extremely strong microwave absorption response in the full frequency band;
[0034] 3. Broad application prospects: The present invention can obtain more than 90% wave absorption efficiency in the whole frequency band through electromagnetic synergy; CST electromagnetic field simulation software simulates and analyzes the maximum reduction value of radar stealth performance at 0° is 29.75dB·m 2 , which means that the obtained material has excellent radar wave attenuation characteristics, can suppress the reflection of electromagnetic waves from the PEC surface, and has broad application prospects in the military field. Through the construction of metamaterials, ultra-wideband absorption of 12.24GHz is achieved at a thickness of 6mm, which can meet most practical application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The X-ray diffraction patterns of the products of Experiments 1 to 3;
[0036] Figure 2 This is the SEM image of GFN prepared in step 1 of experiment 1;
[0037] Figure 3 This is the SEM image of GFN@NPC-1 prepared in Experiment 1;
[0038] Figure 4 This is the SEM image of GFN@NPC-2 prepared in Experiment 2;
[0039] Figure 5 The vibrating sample magnetometer magnetic analysis diagram of the products of Tests 1 to 3;
[0040] Figure 6 The electron hologram and magnetic flux distribution line diagram of GFN@NPC-2 prepared for experiment 2;
[0041] Figure 7 The effective bandwidth of GFN@NPC-1 prepared in experiment 1 at different thicknesses;
[0042] Figure 8The effective bandwidth of GFN@NPC-2 prepared in Experiment 2 at different thicknesses;
[0043] Fig. 9 A diagram showing the simulation results of the electromagnetic metamaterial constructed for Experiment 3;
[0044] Fig.10 This is the RCS reduction value diagram for step 7 of test 1;
[0045] Fig.11 The RCS calculation results of step 7 of test 1 Figure 3 Vittu;
[0046] Fig.12 This is the RCS reduction value diagram for step 7 of test 2;
[0047] Fig.13 The RCS calculation results of step 7 of test 2 are shown in Figure 2. Figure 3 Vittu. DETAILED DESCRIPTION
[0048] Specific implementation method 1: This implementation method is a method for preparing a rare earth doped flower-shaped alloy @COFs derived porous carbon absorbing material, which is specifically carried out in the following steps:
[0049] 1. Dissolve nickel chloride hexahydrate, rare earth chloride hexahydrate and ferric chloride hexahydrate in distilled water, stir evenly, then add NaOH and continue stirring, then add 70% to 80% hydrazine hydrate aqueous solution as a reducing agent to obtain a light green solution, then pour the light green solution into a polytetrafluoroethylene-lined autoclave, and react at 120°C to 150°C in a drying oven for 8h to 10h;
[0050] The black precipitate was collected by magnetic separation, washed three times with water and three times with anhydrous ethanol to obtain black magnetic particles, and the black magnetic particles were vacuum dried at 50°C to 70°C and recorded as GFN;
[0051] The molar ratio of nickel chloride hexahydrate to ferric chloride hexahydrate is 10:(1-1.2);
[0052] The ratio of the molar amount of the rare earth chloride hexahydrate to the molar amount of nickel chloride hexahydrate and ferric chloride hexahydrate is (0.01-0.05):1;
[0053] The mass ratio of the ferric chloride hexahydrate to NaOH is 1:(5.5-6);
[0054] The mass ratio of the NaOH to the volume ratio of the hydrazine hydrate aqueous solution is 1g:(10mL-13mL);
[0055] 2. Add the GFN prepared in step 1 into a three-necked flask containing toluene, then add 3-aminopropyltriethoxysilane into the above solution under a nitrogen atmosphere, heat the oil bath to 100°C to 110°C and keep warm for 1.8h to 2.5h, then cool the black oily substance to room temperature, wash it with water 2 to 3 times, and then vacuum dry it for 12h to 24h to obtain black magnetic particles, named GFN-NH 2 ;
[0056] The mass ratio of the GFN to the volume ratio of toluene is (0.3 g to 0.4 g): (30 mL to 40 mL);
[0057] The mass ratio of the GFN to the volume ratio of 3-aminopropyltriethoxysilane is (0.3 g to 0.4 g): (1 mL to 2 mL);
[0058] 3. GFN-NH prepared in step 2 2 The particles are dispersed in the co-solvent system 1, and then 2,5-dimethoxybenzene-1,4-dicarboxaldehyde monomer and acetic acid solution are added, and after ultrasonic treatment for 3min to 5min, they are transferred to a polytetrafluoroethylene-lined high-pressure reactor, and heated in a drying oven at 120°C to 130°C for 1h to 2h. After natural cooling, the sample is collected in a centrifuge tube, and washed by centrifugation with tetrahydrofuran and acetone for 2 to 3 times respectively, and dried in a vacuum drying oven for 6h to 12h to obtain magnetic particles named GFN-DMTP;
[0059] The co-solvent system 1 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1;
[0060] The GFN-NH 2 The mass ratio of the particles to the volume of the co-solvent system 1 is (0.1 g to 0.15 g): (4 mL to 4.5 mL);
[0061] The mass ratio of the 2,5-dimethoxybenzene-1,4-dicarbaldehyde monomer to the volume ratio of the co-solvent system 1 is (0.01 g to 0.02 g): (4 mL to 4.5 mL);
[0062] The GFN-NH 2 The mass ratio of the particles to the volume of the acetic acid solution is (0.1 g to 0.15 g): (2 mL to 3 mL), and the concentration of the acetic acid solution is 3 mol·L -1 ;
[0063] 4. Disperse the GFN-DMTP prepared in step 3 in the co-solvent system 2, then add 1,3,5-tri(4-aminophenyl)benzene and 2,5-dimethoxybenzene-1,4-dicarboxaldehyde to the above solution, then add acetic acid solution, and ultrasonically homogenize; pour the solution into a polytetrafluoroethylene-lined autoclave, heat the reaction at 60°C to 70°C in a drying oven for 24h to 25h, collect the sample in a centrifuge tube after natural cooling, wash it three times each with tetrahydrofuran and acetone, and then dry it in a vacuum drying oven for 6h to 12h to obtain a fluffy yellow-black product, named GFN@TAPB-DMTP-COF;
[0064] The co-solvent system 2 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1;
[0065] The mass ratio of the GFN-DMTP to the volume ratio of the co-solvent system 2 is (0.05 g to 0.06 g): (20 mL to 30 mL);
[0066] The mass ratio of the GFN-DMTP to the amount of 1,3,5-tris(4-aminophenyl)benzene is (0.05 g to 0.06 g):(0.1 mmol to 0.2 mmol);
[0067] The mass ratio of the GFN-DMTP to the amount of 2,5-dimethoxybenzene-1,4-dicarbaldehyde is (0.05 g to 0.06 g): (0.2 mmol to 0.3 mmol);
[0068] The mass ratio of the GFN-DMTP to the volume of the acetic acid solution is (0.05 g to 0.06 g): (2 mL to 3 mL), and the concentration of the acetic acid solution is 9 mol·L -1 ;
[0069] 5. In a protective gas, calcine the GFN@TAPB-DMTP-COF prepared in step 4 at 600°C to 800°C for 2h to 4h, and then naturally cool to room temperature to obtain a rare earth doped flower-shaped alloy@COFs-derived porous carbon absorbing material.
[0070] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the magnetic separation described in step 1 is to place a magnet at the bottom of the glass container to absorb the alloy, and then pour out the water. The rest is the same as specific implementation method 1.
[0071] Specific embodiment 3: This embodiment is different from specific embodiment 1 or 2 in that the hexahydrated rare earth chloride salt described in step 1 is gadolinium chloride hexahydrate, lanthanum chloride hexahydrate, cerium chloride hexahydrate, neodymium chloride hexahydrate or samarium chloride hexahydrate. The rest is the same as specific embodiment 1 or 2.
[0072] Specific embodiment 4: This embodiment is different from any one of specific embodiments 1 to 3 in that the heating rate in step 5 is 2°C / min to 5°C / min. The rest is the same as any one of specific embodiments 1 to 3.
[0073] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that: in step 5, calcination is performed at 700° C. for 2 h. Other aspects are the same as those of specific embodiment 4.
[0074] Specific implementation example 6: This implementation example is different from specific implementation example 5 in that the protective gas in step 5 is nitrogen or argon. The rest is the same as specific implementation example 5.
[0075] The present invention is verified by the following tests:
[0076] Experiment 1: This experiment is a method for preparing a rare earth doped flower-shaped alloy@porous carbon absorbing material, which is specifically carried out in the following steps:
[0077] 1. Dissolve 0.5704 g of nickel chloride hexahydrate, 0.0294 g of gadolinium chloride hexahydrate and 0.0649 g of ferric chloride hexahydrate in 48 mL of distilled water, stir evenly, then add 0.384 g of NaOH and continue stirring, then add 5 mL of 80% by volume hydrazine hydrate aqueous solution as a reducing agent to obtain a light green solution, then pour the light green solution into a polytetrafluoroethylene-lined autoclave, and react at 120° C. in a drying oven for 10 hours;
[0078] The black precipitate was collected by magnetic separation, washed three times with water and three times with anhydrous ethanol, respectively, to obtain black magnetic particles, which were vacuum dried at 60° C. for 12 h and recorded as GFN; the magnetic separation was performed by placing a magnet at the bottom of a glass container to absorb the alloy, and then pouring out the water;
[0079] 2. 0.3 g of GFN prepared in step 1 was added to a three-necked flask containing 40 mL of toluene, and then 1 mL of 3-aminopropyltriethoxysilane was added to the above solution under a nitrogen atmosphere. The oil bath was heated to 100 ° C and kept warm for 2 h. The black oily substance was then cooled to room temperature and washed with water three times, and then vacuum dried for 12 h to obtain black magnetic particles, named GFN-NH 2 ;
[0080] 3. Add 0.15 g of GFN-NH prepared in step 2 2 The particles were dispersed in 4.5 mL of co-solvent system 1, and 0.01 g of 2,5-dimethoxybenzene-1,4-dicarboxaldehyde monomer and 3 mL of acetic acid solution (3 mol·L -1), after ultrasonication for 5 min, transferred to a polytetrafluoroethylene-lined autoclave, heated in a drying oven at 120 ° C for 1 h, collected the sample in a centrifuge tube after natural cooling, washed by centrifugation with tetrahydrofuran and acetone for 3 times each, and dried in a vacuum drying oven for 6 h to obtain magnetic particles named GFN-DMTP;
[0081] The co-solvent system 1 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1;
[0082] 4. Disperse 0.0526 g of GFN-DMTP prepared in step 3 in 27 mL of co-solvent system 2, then add 0.18 mmol of 1,3,5-tris(4-aminophenyl)benzene and 0.27 mmol of 2,5-dimethoxybenzene-1,4-dicarboxaldehyde to the above solution, and then add 3 mL of acetic acid solution, and ultrasonically homogenize; pour the solution into a polytetrafluoroethylene-lined autoclave, heat the reaction at 60 ° C in a drying oven for 24 hours, collect the sample in a centrifuge tube after natural cooling, wash it three times with tetrahydrofuran and acetone respectively, and then dry it in a vacuum drying oven for 6 hours to obtain a fluffy yellow-black product, named GFN@TAPB-DMTP-COF;
[0083] The co-solvent system 2 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1;
[0084] The concentration of the acetic acid solution is 3 mol·L -1 ;
[0085] 5. Under nitrogen protection, the GFN@TAPB-DMTP-COF prepared in step 4 was calcined at 700°C for 2h, and then naturally cooled to room temperature to obtain rare earth doped flower-shaped alloy@COFs derived porous carbon absorbing material GFN@NPC-1; the heating rate in step 5 was 2°C / min;
[0086] 6. The rare earth doped flower-shaped alloy @COFs derived porous carbon absorbing material prepared in Experiment 1 was immersed in melted paraffin as a substrate (the mass ratio of the absorbing material to the paraffin was 1:1) to form a ring, in which the absorbing material accounted for 50wt.% of the total mass of the ring. The electromagnetic parameters of the absorbing material were measured by a vector network analyzer. According to the transmission line theory, the reflection loss of the material to the electromagnetic wave was calculated by the following equation;
[0087]
[0088] 7. The radar stealth performance of the rare earth doped flower-shaped alloy @COFs derived porous carbon absorbing material prepared in Experiment 1 was simulated using CST electromagnetic field simulation software, and the reduction in its radar cross-sectional area was calculated using the following formula.
[0089]
[0090] Experiment 2: This experiment differs from Experiment 1 in that the amount of 1,3,5-tris(4-aminophenyl)benzene used in step 4 is 0.36 mmol, and the amount of 2,5-dimethoxybenzene-1,4-dicarboxaldehyde used is 0.54 mmol; the product of step 5 is recorded as GFN@NPC-2. The rest is the same as Experiment 1.
[0091] Experiment 3: This experiment differs from Experiment 1 in that the amount of 1,3,5-tris(4-aminophenyl)benzene used in step 4 is 0.09 mmol, and the amount of 2,5-dimethoxybenzene-1,4-dicarboxaldehyde used is 0.135 mmol; the product of step 5 is recorded as GFN@NPC-0.5. The rest is the same as Experiment 1.
[0092] Figure 1 The X-ray diffraction patterns of the products of Experiments 1 to 3, wherein GFN is the product of Step 1 of Experiment 1, and it can be seen that alloy and nitrogen-doped carbon-derived peaks are displayed, with almost no impurity peaks, indicating that the purity is high. The product of the present invention is stable and is conducive to industrial production and promotion.
[0093] Figure 2 This is the SEM image of the GFN prepared in step 1 of experiment 1. The flower-like GFN structure can be seen from the image.
[0094] Figure 3 This is the SEM image of GFN@NPC-1 prepared in experiment 1. From the image, we can see that it is a structure of COF-derived porous carbon coated on the flower-shaped alloy, and it can be seen that part of the flower-shaped alloy is distributed outside the carbon matrix.
[0095] Figure 4 This is the SEM image of GFN@NPC-2 prepared in Experiment 2. From the image, we can see that it is a flower-like alloy structure completely coated with COF-derived porous carbon, and it can be seen that the flower-like alloy and porous carbon form a "raspberry"-like structure.
[0096] Figure 5 The vibrating sample magnetometer magnetic analysis diagram of the products of experiments one to three, among which GFN is the product of step one of experiment one. It can be seen that it has excellent magnetic loss capability, and its magnetic saturation intensity is up to 53emu / g.
[0097] Figure 6Electron hologram and magnetic flux distribution line diagram of GFN@NPC-2 prepared for experiment 2. The micro-scale flower-shaped GFN sample acts as a magnetically activated antenna, emitting strong magnetic flux lines that penetrate the outer carbon layer and interact with adjacent magnetic units through magnetic coupling. In addition, when the radiation directions of the magnetic flux lines are opposite, long-range magnetic diffraction is achieved. Stray magnetic line loops can establish a huge magnetic network, further dissipating EMW energy.
[0098] Figure 7 The effective bandwidth of GFN@NPC-1 prepared in Experiment 1 at different thicknesses (calculated in Step 6) is obtained from Figure 7 It can be seen that the effective absorption bandwidth of the material reaches 6.52GHz at an ultra-thin thickness of only 1.9mm. By adjusting the thickness, an absorption efficiency of more than 90% can be obtained in the entire frequency band.
[0099] Figure 8 The effective bandwidth of GFN@NPC-2 prepared in Experiment 2 at different thicknesses (calculated in Step 6) is Figure 8 It can be seen that the minimum reflection loss is -69.6 dB at 17.5 GHz (converted into microwave absorptivity, about 99.9999% of the electromagnetic waves are absorbed), and the thickness is 1.68 mm.
[0100] Experiment 3: Constructing an electromagnetic metamaterial based on GFN@NPC-2 prepared in Experiment 2: The electromagnetic parameters of the absorbing material obtained by the vector network analyzer test were imported into the CST electromagnetic field simulation software, the frequency was set to 2-18 GHz, the boundary was set to a periodic boundary, and a three-layer gradient metamaterial was constructed. The side length and height of the bottom layer were 12 mm × 2 mm, the side length and height of the second layer were 10 mm × 2 mm, and the side length and height of the third layer were 8 mm × 2 mm.
[0101] Fig. 9 This is the simulation result of the electromagnetic metamaterial constructed in Experiment 3. The metamaterial exhibits excellent electromagnetic wave absorption performance, exceeding 76% of the entire frequency band and achieving ultra-wideband absorption of 12.24 GHz. The reflection loss reduction value is greater than -10 dB, showing potential for practical application.
[0102] Fig.10 This is the RCS reduction value diagram for step 7 of test 1. Fig.11 The RCS calculation results of step 7 of test 1 Figure 3 From the figure, it can be seen that at an angle of 0°, the maximum RCS reduction value of the rare earth doped flower-shaped alloy@COFs derived porous carbon absorber is 22.11dB·m 2 , demonstrating its excellent radar stealth performance, showing potential for practical application, and has broad application prospects in the military field.
[0103] Fig.12 This is the RCS reduction value diagram for step 7 of test 2. Fig.13 The RCS calculation results of step 7 of test 2 are shown in Figure 2. Figure 3 From the figure, we can see that the maximum RCS reduction value is 29.75dB·m 2 .
Claims
1. A method for preparing a rare earth doped flower-shaped alloy @COFs derived porous carbon absorbing material, characterized in that The preparation method of the rare earth doped flower-shaped alloy@COFs derived porous carbon absorber is carried out according to the following steps:
1. Dissolve nickel chloride hexahydrate, rare earth chloride hexahydrate and ferric chloride hexahydrate in distilled water, stir evenly, then add NaOH and continue stirring, then add hydrazine hydrate aqueous solution with a volume concentration of 80% to 85% as a reducing agent to obtain a light green solution, then pour the light green solution into a polytetrafluoroethylene-lined autoclave, and react in a drying oven at 120°C to 150°C for 8h to 10h; The black precipitate was collected by magnetic separation, washed three times with water and three times with anhydrous ethanol to obtain black magnetic particles, and the black magnetic particles were vacuum dried at 50°C to 70°C and recorded as GFN; The molar ratio of nickel chloride hexahydrate to ferric chloride hexahydrate is 10:(1-1.2); The ratio of the molar amount of the rare earth chloride hexahydrate to the molar amount of nickel chloride hexahydrate and ferric chloride hexahydrate is (0.01-0.05):1; The mass ratio of the ferric chloride hexahydrate to NaOH is 1:(5.5-6); The mass ratio of the NaOH to the volume ratio of the hydrazine hydrate aqueous solution is 1g:(10mL-13mL); 2. Add the GFN prepared in step 1 into a three-necked flask containing toluene, then add 3-aminopropyltriethoxysilane into the above solution under a nitrogen atmosphere, heat the oil bath to 100°C to 110°C and keep warm for 1.8h to 2.5h, then cool the black oily substance to room temperature, wash it with water 2 to 3 times, and then vacuum dry it for 12h to 24h to obtain black magnetic particles, named GFN-NH2; The mass ratio of the GFN to the volume ratio of toluene is (0.3 g to 0.4 g): (30 mL to 40 mL); The mass ratio of the GFN to the volume ratio of 3-aminopropyltriethoxysilane is (0.3 g to 0.4 g): (1 mL to 2 mL); 3. Disperse the GFN-NH2 particles prepared in step 2 in the co-solvent system 1, add 2,5-dimethoxybenzene-1,4-dicarboxaldehyde monomer and acetic acid solution, transfer to a polytetrafluoroethylene-lined autoclave after ultrasonic treatment for 3min to 5min, heat and react at 120°C to 130°C in a drying oven for 1h to 2h, collect the sample in a centrifuge tube after natural cooling, wash with tetrahydrofuran and acetone by centrifugation for 2 to 3 times respectively, and dry in a vacuum drying oven for 6h to 12h to obtain magnetic particles named GFN-DMTP; The co-solvent system 1 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1; The mass ratio of the GFN-NH2 particles to the volume ratio of the co-solvent system 1 is (0.1 g to 0.15 g): (4 mL to 4.5 mL); The mass ratio of the 2,5-dimethoxybenzene-1,4-dicarbaldehyde monomer to the volume ratio of the co-solvent system 1 is (0.01 g to 0.02 g): (4 mL to 4.5 mL); The mass ratio of the GFN-NH2 particles to the volume of the acetic acid solution is (0.1 g to 0.15 g): (2 mL to 3 mL), and the concentration of the acetic acid solution is 3 mol·L -1 ; 4. Disperse the GFN-DMTP prepared in step 3 in the co-solvent system 2, then add 1,3,5-tri(4-aminophenyl)benzene and 2,5-dimethoxybenzene-1,4-dicarboxaldehyde to the above solution, then add acetic acid solution, and ultrasonically homogenize; pour the solution into a polytetrafluoroethylene-lined autoclave, heat the reaction at 60°C to 70°C in a drying oven for 24h to 25h, collect the sample in a centrifuge tube after natural cooling, wash it three times each with tetrahydrofuran and acetone, and then dry it in a vacuum drying oven for 6h to 12h to obtain a fluffy yellow-black product, named GFN@TAPB-DMTP-COF; The co-solvent system 2 is a mixture of 1,4-dioxane, n-butanol and methanol in a volume ratio of 4:4:1; The mass ratio of the GFN-DMTP to the volume ratio of the co-solvent system 2 is (0.05 g to 0.06 g): (20 mL to 30 mL); The mass ratio of the GFN-DMTP to the amount of 1,3,5-tris(4-aminophenyl)benzene is (0.05 g to 0.06 g):(0.1 mmol to 0.2 mmol); The mass ratio of the GFN-DMTP to the amount of 2,5-dimethoxybenzene-1,4-dicarbaldehyde is (0.05 g to 0.06 g): (0.2 mmol to 0.3 mmol); The mass ratio of the GFN-DMTP to the volume of the acetic acid solution is (0.05 g to 0.06 g): (2 mL to 3 mL), and the concentration of the acetic acid solution is 9 mol·L -1 ; 5. In a protective gas, calcine the GFN@TAPB-DMTP-COF prepared in step 4 at 600°C to 800°C for 2h to 4h, and then naturally cool to room temperature to obtain a rare earth doped flower-shaped alloy@COFs-derived porous carbon absorbing material.
2. The method for preparing a rare earth doped flower-shaped alloy@COFs derived porous carbon absorbing material according to claim 1, characterized in that The magnetic separation described in step 1 is to place a magnet at the bottom of the glass container to absorb the alloy, and then pour out the water.
3. The method for preparing a rare earth doped flower-shaped alloy@COFs derived porous carbon absorbing material according to claim 1, characterized in that The rare earth chloride hexahydrate described in step 1 is gadolinium chloride hexahydrate, lanthanum chloride hexahydrate, cerium chloride hexahydrate, neodymium chloride hexahydrate or samarium chloride hexahydrate.
4. The method for preparing a rare earth doped flower-shaped alloy@COFs derived porous carbon absorbing material according to claim 1, characterized in that The heating rate in step five is 2°C / min to 5°C / min.
5. The method for preparing a rare earth doped flower-shaped alloy@COFs derived porous carbon absorbing material according to claim 1, characterized in that In step 5, calcination is carried out at 700°C for 2h.