Preparation method of metal alloy capable of improving component uniformity and metal alloy standard sample
Through vacuum continuous casting, metal water atomization powder making and powder sintering technology, the complex problems of segregation and processing of metal alloy standard samples are solved, and higher composition uniformity and processing stability are achieved, the production process is simplified and the production process is reduced. Cost and energy consumption.
Patent Information
- Application Number
- CN202410964030.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
There are complex problems in the production of existing metal alloy component analysis standard samples, resulting in poor composition uniformity and affecting the quality and fixed value of the final sample.
Using vacuum continuous casting, metal water atomization powder making, powder mixing and powder sintering technology, the composition uniformization of metal alloy standard samples is achieved by controlling the supercooling degree and geometric space mixing and forming.
Effectively suppress the segregation phenomenon of metal components, improve the uniformity of components, simplify the processing process, reduce individual differences, reduce material losses and production energy consumption, improve smelting success rate, and ensure processing stability.
Smart Images

Figure CN118905228A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of metal smelting, and in particular to a method for preparing a metal alloy with improved composition uniformity and a metal alloy standard sample. Background Art
[0002] At present, in the field of metal smelting technology, standard samples for metal alloy composition analysis are generally prepared by pyrometallurgy. The common process is: smelting → casting → peeling and grinding → turning and milling or pressing and rolling into sheets. That is, the various metal raw materials are heated to a molten state by methods such as fire smelting, induction smelting, and arc smelting. After being fully mixed to form an alloy liquid, they are cast, molded, and continuously cast according to actual needs to form metal castings. Then, according to the quality performance of the castings, the castings are peeled and polished by manual or mechanical processing to remove the outer oxide layer and segregation layer. Finally, the castings are turned and milled or pressed and punched into sheets according to the standard sample development plan to complete the preparation of the final sample.
[0003] However, the inventors of the present application have found that the existing production and manufacturing technology of standard samples for metal alloy composition analysis generally has problems such as composition segregation and complicated forming and processing procedures. Among them, composition segregation is closely related to material composition and smelting technology, especially traditional smelting technology (fire smelting, induction smelting, arc smelting, continuous casting and other technologies) has limited control over the degree of ingot segregation, and the composition homogenization effect is often unsatisfactory. The forming and processing procedures of removing the segregation layer and the oxide layer of the cast embryo by means of manual or mechanical peeling and grinding often cause composition segregation, uneven depth of the segregation layer, random processing, and pollution of the environment or tools. These instability factors will directly affect the uniformity of the color of the cast embryo to varying degrees. In addition, the quality of the cast embryo cannot be effectively controlled during the peeling and grinding process due to the need for turning, milling, cutting and grinding. In particular, the forming process of the cast embryo without effectively processing the segregation layer will affect the final quality and fixed value of the standard sample. Therefore, there is an urgent need for a method for preparing a metal alloy that can effectively suppress the segregation of metal components, make the uniformity of the produced metal alloy standard sample better than the existing traditional production technology, and improve the success rate of component homogenization. Summary of the invention
[0004] In view of the above problems, the embodiments of the present invention provide a method for preparing a metal alloy with improved composition uniformity and a metal alloy standard product, which are used to solve the problems of metal component segregation and low composition uniformity in the prior art.
[0005] According to one aspect of an embodiment of the present invention, there is provided a method for preparing a metal alloy with improved composition uniformity, the method comprising:
[0006] After the metal raw materials are weighed according to the proportion, continuous casting is performed to obtain a metal material casting embryo;
[0007] Atomizing the metal material casting embryo to obtain a suspension of metal material powder and aqueous solution;
[0008] The suspension is cleaned to clean the pollutants in the powder to obtain a cleaned liquid containing the metal material powder;
[0009] The cleaned liquid containing the metal material powder is subjected to low-temperature drying of the powder at a temperature of 65° C. to 85° C. to obtain a dried metal powder;
[0010] Screening the dried metal powder according to particle size to obtain metal powder with a mesh size within a preset mesh size range;
[0011] Mixing metal powders with mesh sizes within a preset mesh size range to obtain mixed metal powders;
[0012] The mixed metal powder is randomly sampled and placed into a powder metallurgy pressing die to press out a standard metal alloy product.
[0013] In an optional manner, the water atomization of the metal material casting embryo to obtain a suspension of metal material powder and aqueous solution comprises:
[0014] Taking cross-sectional samples of the metal material casting embryo, and analyzing and detecting the uniformity of the cross-sectional area of the metal material casting embryo;
[0015] When the uniformity reaches the preset requirement, the metal material casting embryo is subjected to water atomization powder making to obtain a suspension of metal material powder and aqueous solution.
[0016] In an optional manner, after taking cross-sectional samples of the metal material casting embryo and analyzing and detecting the uniformity of the cross-sectional area of the metal material casting embryo, the method further comprises:
[0017] When the uniformity does not reach the preset requirement, continuous casting is continued to obtain a metal material casting embryo.
[0018] In an optional manner, the suspension is cleaned to clean the pollutants in the powder to obtain a cleaned liquid containing the metal material powder, comprising:
[0019] The suspension is allowed to settle and the supernatant is removed;
[0020] Introduce pure water, stir thoroughly, let stand and settle, remove the supernatant, and wash away the pollutants in the powder;
[0021] The steps of introducing pure water and stirring sufficiently, standing to settle, removing the upper clear liquid, and washing the pollutants in the powder are repeated at least once to obtain a washed liquid containing the metal material powder.
[0022] In an optional manner, the cleaned liquid containing the metal material powder is subjected to low-temperature drying of the powder at a temperature of 65° C. to 85° C. to obtain the dried metal powder, comprising:
[0023] Use a glass container to load the cleaned liquid containing the metal material powder, put it into an electric drying oven, and cover the mouth of the glass container with a beaker cover glass container;
[0024] The drying temperature range of the electric drying oven is set to 65°C to 85°C, and the temperature fluctuation is maintained within the drying temperature range to dry the moisture of the powder at low temperature to obtain dried metal powder.
[0025] In an optional manner, the preset mesh count range is between 400 and 80.
[0026] In an optional manner, randomly sampling the mixed metal powder and placing it into a powder metallurgy pressing mold to press out a metal alloy standard sample blank comprises:
[0027] According to the preset strength requirement, the pressed metal alloy standard sample blank is sintered to obtain a sintered metal alloy standard sample semi-finished product.
[0028] In an optional manner, the pressed metal alloy standard sample blank is sintered according to a preset strength requirement to obtain a sintered metal alloy standard sample semi-finished product, including:
[0029] The surface of the sintered metal alloy standard sample semi-finished product is polished to obtain a polished metal alloy standard sample.
[0030] In an optional manner, the surface of the sintered metal alloy standard product is polished to obtain a polished metal alloy standard sample, comprising:
[0031] By using X-ray fluorescence spectrometry, the surface content changes of the semi-finished metal alloy standard sample after sintering are analyzed;
[0032] The surface is polished;
[0033] By using X-ray fluorescence spectrometry, the surface content changes of metal components in the semi-finished products of the standard metal alloy samples after grinding were analyzed;
[0034] determining a grinding depth according to the change;
[0035] The sintered metal alloy standard sample semi-finished product is ground according to the grinding depth to obtain a ground metal alloy standard sample.
[0036] According to another aspect of an embodiment of the present invention, a metal alloy standard sample is provided. The metal alloy standard sample is prepared by the aforementioned method for preparing a metal alloy with improved composition uniformity.
[0037] The embodiment of the present invention performs water atomization powder making on the metal material casting embryo through continuous casting to obtain a suspension of metal material powder and aqueous solution; the suspension is cleaned to clean the pollutants in the powder to obtain a cleaned liquid containing metal material powder; the cleaned liquid containing metal material powder is subjected to low-temperature drying of the powder at a temperature of 65°C to 85°C to obtain a dried metal powder; the dried metal powder is subjected to particle size screening to obtain metal powder with a mesh number within a preset mesh number range; the metal powder with a mesh number within the preset mesh number range is mixed to obtain a mixed metal powder; the mixed metal powder is randomly sampled and placed in a powder metallurgy pressing mold to press out a metal alloy standard sample blank. The embodiment of the present invention adopts a technology combining vacuum continuous casting, metal water atomization powder making, powder mixing and powder sintering to control the supercooling degree to suppress the material segregation phenomenon, and utilizes the principle of geometric space mixing and forming after the material is prepared into powder to achieve the homogenization of the composition of the metal alloy standard sample.
[0038] The above description is only an overview of the technical solution of the embodiment of the present invention. In order to more clearly understand the technical means of the embodiment of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings are only used to illustrate the embodiments and are not to be considered as limiting the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings. In the accompanying drawings:
[0040] Figure 1 A schematic flow chart of a method for preparing a metal alloy with improved composition uniformity provided by an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0041] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. The following specific embodiments provide the best embodiment of the present invention. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0042] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more related listed items.
[0043] Embodiment 1:
[0044] Figure 1 FIG. 1 is a flow chart showing a method for preparing a metal alloy with improved composition uniformity provided by an embodiment of the present invention. Figure 1 As shown, the method comprises the following steps:
[0045] Step 110: After weighing the metal raw materials according to the proportion, continuous casting is performed to obtain a metal material casting embryo.
[0046] The vacuum continuous casting in the embodiment of the present invention is to use a continuous crystal crystallizer to continuously pour liquid metal at one end and continuously pull out the molding material from the other end under a vacuum environment.
[0047] In the embodiment of the present invention, the metal raw materials are weighed according to the proportion and then continuously cast under vacuum protection. Specifically, the main component metal raw materials, the intermediate alloy and other metal raw materials can be continuously cast through a continuous casting machine under argon protection to obtain a metal material casting embryo.
[0048] Step 120: The metal material casting embryo is subjected to water atomization to obtain a suspension of metal material powder and aqueous solution.
[0049] Among them, the principle of metal water atomization powder making is to use the impact of high-pressure water flow to directly break the molten metal alloy liquid into fine droplets, and quickly condense them to obtain powder.
[0050] In the embodiment of the present invention, the cross-section sampling of the metal material casting is carried out, and the uniformity of the cross-section of the metal material casting is analyzed and detected; when the uniformity reaches the preset requirement, the metal material casting is subjected to water atomization powder making to obtain a suspension of metal material powder and aqueous solution. Wherein, when the uniformity does not reach the preset requirement, continuous casting is continued to obtain a metal material casting. Specifically, the cross-section sampling of the casting is carried out, and the uniformity of the cross-section sample of the ingot is detected by X-ray fluorescence spectroscopy or other component analysis methods. When the component uniformity reaches the preliminary requirement, the ingot is subjected to water atomization powder making by a vacuum water atomization powder making machine to obtain a suspension of metal material powder and aqueous solution.
[0051] Step 130: washing the suspension to remove pollutants from the powder, and obtaining a washed liquid containing the metal material powder.
[0052] Among them, the embodiment of the present invention is to statically settle the suspension and remove the supernatant; introduce pure water, stir it thoroughly, let it stand and settle, remove the supernatant, and clean the pollutants in the powder; repeat the steps of introducing pure water and stirring it thoroughly, let it stand and settle, remove the supernatant, and clean the pollutants in the powder at least once to obtain a cleaned liquid containing metal material powder.
[0053] Specifically, in one specific implementation of the present invention, after the suspension containing metal material powder is statically precipitated, the upper clear liquid is removed, pure water is introduced and the liquid is fully stirred using a magnetic stirrer, and then left to statically precipitate. After complete precipitation, the upper clear liquid is removed again, and the above operation is repeated 3 times to fully clean the pollutants in the powder.
[0054] Step 140: The cleaned liquid containing the metal material powder is subjected to low-temperature drying at a temperature of 65° C. to 85° C. to obtain dried metal powder.
[0055] Among them, a glass container is used to load the cleaned liquid containing the metal material powder, which is placed in an electric drying oven, and the beaker-covered glass container is placed on the mouth of the glass container; the drying temperature range of the electric drying oven is set to 65°C to 85°C, and the temperature fluctuation is kept within the drying temperature range, and the powder is dried at low temperature to obtain the dried metal powder. Specifically, a glass container can be used to load the liquid containing the metal material powder, which is placed in an electric drying oven, and the beaker-covered glass container is placed on the mouth of the glass container to prevent contamination caused by falling ash during the drying process; the drying temperature range of the box is set to 65°C to 85°C, and the temperature fluctuation is kept within the set range, and the powder is dried at low temperature to avoid high-temperature internal oxidation of the metal powder material and cause component segregation.
[0056] Step 150: Screening the dried metal powder according to particle size to obtain metal powder with a mesh size within a preset mesh size range.
[0057] The preset mesh number range is between 400 and 80. Specifically, the dried metal powder can be screened by particle size, and metal sieves with different apertures or a vibrating powder sieving machine can be used to sieve out metal powders with mesh numbers between 400 and 80 (φ38μm~φ178μm).
[0058] Step 160: Mixing metal powders with mesh sizes within a preset mesh size range to obtain mixed metal powders.
[0059] Among them, the metal powder with a mesh size between 400 and 80 is subjected to powder mixing treatment, and if necessary, a powder mixer (V-type mixer, two-position mixer, three-dimensional mixer, double cone mixer, etc.) can be used for mechanical mixing treatment.
[0060] Step 170: Randomly sample the mixed metal powder and put it into a powder metallurgy pressing mold to press out a metal alloy standard sample blank.
[0061] In an embodiment of the present invention, the pressed metal alloy standard sample blank is sintered according to the preset strength requirements to obtain a sintered metal alloy standard sample semi-finished product. Among them, the preset strength requirements can be set accordingly by those skilled in the art according to the specific scenario, and the embodiment of the present invention does not impose any specific restrictions. Specifically, the mixed metal powder can be randomly sampled and placed in a powder metallurgy pressing mold to mechanically press out a standard sample blank. The pressing mold can be customized according to the design requirements of the standard sample development plan, and the embodiment of the present invention does not impose any specific restrictions.
[0062] After step 170, the method further includes: sintering the pressed metal alloy standard sample blank according to the preset strength requirement to obtain the sintered metal alloy standard sample semi-finished product. Specifically, the pressed standard sample specimen can be sintered at a temperature of 0.5 to 0.8 times the melting point of the material according to the requirement, so that the pressed standard sample blank has a certain strength to meet the needs of daily use.
[0063] In an embodiment of the present invention, after obtaining the sintered metal alloy standard sample semi-finished product, the method further includes: grinding the surface of the sintered metal alloy standard sample semi-finished product to obtain the ground metal alloy standard sample. After sintering, the standard sample semi-finished product can also be subjected to surface grinding if necessary to clean the shallow oxide layer and segregation layer generated during sintering, wherein the depth required for grinding can be evaluated by analyzing the change in surface content in combination with X-ray fluorescence spectroscopy. Specifically, the surface content change of the sintered metal alloy standard sample semi-finished product can be analyzed by X-ray fluorescence spectroscopy; the surface is ground; the surface content change of the metal component of the metal alloy standard sample semi-finished product after grinding is analyzed by X-ray fluorescence spectroscopy; the grinding depth is determined according to the change; according to the grinding depth, the sintered metal alloy standard sample semi-finished product is ground to obtain the ground metal alloy standard sample.
[0064] The embodiment of the present invention adopts a combination of vacuum continuous casting, metal water atomization powder making, powder mixing and powder sintering, etc., and realizes the homogenization of the composition of the metal alloy standard sample by controlling the supercooling to suppress the material segregation phenomenon and utilizing the principle of geometric space mixing and forming after the material is prepared into powder. Specifically, in a vacuum environment, a continuous crystal crystallizer is used to continuously pour liquid metal at one end, and the molding material is continuously pulled out from the other end for continuous casting; metal water atomization powder making is used, and the impact of high-pressure water flow is used to directly break the molten metal alloy liquid into fine droplets, and quickly condense to obtain powder; powder mixing and powder sintering, the powder is uniformly mixed by mechanical mixing method and formed by pressing mold, and heated to a temperature lower than the melting point of the powder component, so that bonding occurs between the powder particles, thereby obtaining better material strength.
[0065] The embodiments of the present invention, on the one hand, effectively suppress the segregation of metal components, so that the uniformity of the produced metal alloy standard samples is better than that of the existing traditional production technology, and the success rate of component homogenization is improved. On the other hand, the batch metal alloy standard samples are formed by powder pressing and powder sintering, which effectively controls the randomness of processing, reduces the individual differences between metal standard samples, saves many mechanical processing steps, and ensures the stability of the processing technology. In particular, in the production of precious metal standard samples, it can effectively reduce the material loss rate and production energy consumption, improve the smelting success rate, and control the production cost, so as to achieve efficient production of standard samples.
[0066] Embodiment 2:
[0067] The embodiment of the present invention provides a method for preparing a metal alloy with improved composition uniformity, wherein the metal alloy is 925 silver (silver S925 metal standard sample). The method comprises the following steps:
[0068] Step 1: Accurately weigh the silver raw material (purity>99.99%), and the filler Heraeus H-220 and H-PAT at a mass ratio of 92.5%:3.75%:3.75%. The mass information is shown in Table 1.
[0069] Table 1 Raw material weighing information for preparing silver S925 samples
[0070] Silver raw materials H-220 patching H-PAT patching total Total mass (g) 1000.020 40.544 40.541 1081.105 Proportion 92.50% 3.75% 3.75% 100%
[0071] Step 2: After the raw materials and the filling materials are mixed, they are placed in a vacuum continuous casting machine, argon gas is introduced for protection, the melting temperature is set to 1100°C, the heating power is set to 70kW, and the metal mixture is continuously cast into a φ8.00mm cylindrical cast rod.
[0072] Step 3: Take cross-section samples of the cylindrical cast rod and analyze the silver content of the cross-section plane using X-ray fluorescence spectroscopy. The range of each point is within 10%. The test data is shown in Table 2.
[0073] Step 4: Physically cut the cylindrical cast rod into pieces, and put the pieces into the graphite crucible of the water atomization powder making equipment, introduce argon protection, set the temperature to 1050℃, turn on the electromagnetic stirring function, adjust the water pressure of the spray gun, let the water flow at high speed to flush the powder collecting bin wall, turn on the powder making work switch, and start metal powder making. After the powder making is completed, open the powder collecting bin to obtain the silver alloy powder suspension.
[0074] Step 5: The silver alloy powder suspension is repeatedly washed three times by stirring and keeping the suspension still for several times and removing the upper clear liquid.
[0075] Step 6: Transfer the silver alloy powder suspension to a glass container and use a box-type drying furnace at a constant temperature of 80°C to dry the powder.
[0076] Step 7: Use a 80-mesh metal screen to screen the dried silver alloy powder.
[0077] Step 8: Repeatedly transpose and mix the sieved silver alloy powder.
[0078] Step 9: Randomly take silver alloy powder and press it into a sample mold to form 30 cylindrical silver S925 metal standard samples with a diameter of 10 mm and a thickness of 0.4 mm. Use a muffle furnace with a temperature of 450°C to sinter the pressed cylindrical silver S925 metal standard samples.
[0079] Step 10: The sintered silver S925 metal standard sample semi-finished product was polished on both sides with a polishing depth of 0.05 mm, and 10 pieces were randomly selected for silver content analysis by X-ray fluorescence spectrometer. The test data is shown in Table 2.
[0080] Table 2X Fluorescence spectroscopy analysis data
[0081]
[0082]
[0083] Conclusion: From the data in Table 2, it can be found that the data of the silver content at each point in the cross section of the silver alloy rod obtained by vacuum continuous casting are quite different. It can be judged that the composition uniformity of the silver alloy rod prepared by vacuum continuous casting technology is poor. After using the embodiment of the present invention, the X-ray fluorescence spectrometry analysis results of the prepared silver alloy samples are very close, and the data range is 0.08%. Compared with the former, it can be seen that after applying the method of the embodiment of the present invention, the color uniformity of the silver alloy sample is significantly improved.
[0084] Embodiment 3:
[0085] The embodiment of the present invention provides a method for preparing a metal alloy with improved composition uniformity, wherein the metal alloy is a standard sample of silver alloy containing harmful elements. The method comprises the following steps:
[0086] Step 1: accurately weigh the silver raw material (purity> 99.99%) and the harmful element filling according to the designed composition ratio. The quality information is shown in Table 3;
[0087] Silver raw materials Leaded joint Arsenic Patching Cadmium-containing joints total Mass(g) 1000.04 3.89 3.02 1.16 1008.11
[0088] Step 2: Add the weighed metal raw materials into the vacuum continuous casting machine, introduce argon protection, set the melting temperature to 1050°C, the heating power to 75kW, and continuously cast the metal mixture into φ8.00mm cylindrical casting rods.
[0089] Step 3: Take samples at equal intervals from the cylindrical cast rods, and use inductively coupled plasma emission spectrometry to analyze the trace harmful elements of the obtained samples. The range of each point is within 10%. The test data is shown in Table 4;
[0090] Step 4: According to the analysis results of the inductively coupled plasma emission spectrometry, the end of the casting rod with the smaller numerical range is selected for water atomization powder making to obtain a suspension of metal material powder and aqueous solution;
[0091] Step 5: Stir the powder suspension several times and let it settle, remove the supernatant, and wash the powder suspension three times;
[0092] Step 6: Set the drying temperature of the experimental drying oven to 80°C, keep the temperature fluctuation within the range of ±5°C, and dry the powder at low temperature to avoid high-temperature internal oxidation of the metal powder material and cause component segregation;
[0093] Step 7: Use an 80-mesh metal screen to sieve the metal powder, and retain the metal powder with a mesh size smaller than 80;
[0094] Step 8: The retained metal powder is pressed into a mold to form 38 sheet metal sample blanks with a diameter of 1 cm and a thickness of 0.5 cm;
[0095] Step 9: The pressed metal sample blank was sintered at 600°C, and the surface of the sintered sample semi-finished product was polished. Samples were taken for inductively coupled plasma emission spectrometry analysis, and the analysis results of trace harmful elements were obtained and shown in Table 4.
[0096] Table 4 Comparison of analysis results by inductively coupled plasma emission spectrometry
[0097]
[0098] Among them, Table 4 is the analysis of trace harmful elements of silver alloy samples prepared by the vacuum continuous casting technology and the method of the embodiment of the present invention respectively using the traditional inductively coupled plasma emission spectrometry. From the results in Table 4, the method of the embodiment of the present invention is better than the currently commonly used traditional vacuum continuous casting technology in the uniformity of preparing metal standard samples.
[0099] Embodiment 4:
[0100] The embodiment of the present invention provides a method for preparing a metal alloy with improved composition uniformity, wherein the metal alloy is a copper-tin alloy working sample. The method comprises the following steps:
[0101] Step 1: Accurately weigh the copper raw material (purity>99.99%), the tin raw material (purity>99.99), and the zinc raw material (purity>99.70), and prepare two portions of the raw materials. The quality information of each raw material is shown in Table 5;
[0102] Table 5 Ratio of raw materials for smelting copper-tin alloy
[0103]
[0104] Step 2: Add the first weighed metal raw material into the medium frequency induction melting furnace, set the melting temperature to 1100°C, and after the metal is completely melted into alloy liquid, stir the alloy liquid with a quartz glass rod, and pour the alloy liquid into the rectangular graphite tank by pouring and pouring;
[0105] Step 3: Use a metal clamp to quickly take out the copper-tin alloy ingot for cold water quenching, sample 5 locations of the copper alloy ingot in different directions by mechanical cutting, and perform composition analysis on the 5 copper-tin alloy samples by X-ray fluorescence spectrometry;
[0106] Step 4: Put the second batch of raw materials into a vacuum continuous casting machine, introduce argon protection, set the melting temperature to 1100°C, the heating power to 70kW, and continuously cast the metal mixture into a cylindrical casting rod of φ8.00mm;
[0107] Step 5: Cut the cast rod into blocks and put them into the graphite crucible of the water atomizing powder making machine, introduce argon protection, set the temperature to 1065°C, turn on the electromagnetic stirring function, adjust the water pressure of the spray gun, and make copper-tin alloy powder. After the powder making is completed, open the powder collecting port to obtain the copper-tin alloy suspension;
[0108] Step 6: The copper-tin alloy powder suspension is repeatedly washed three times by stirring and statically stirring the suspension several times and removing the supernatant;
[0109] Step 7: drying the copper-tin alloy powder at 80° C. to remove moisture, and sieving the powder after drying to obtain copper-tin alloy powder with a particle size less than 40 mesh;
[0110] Step 8: The retained copper-tin alloy powder is molded and pressed to obtain 5 pressed copper-tin alloy metal samples, and their components are analyzed by X-ray fluorescence spectrometry.
[0111] Data analysis and comparison:
[0112] From the data results in Table 6, it can be seen that the copper-tin alloy sample prepared by the method of the embodiment of the present invention is subjected to composition analysis. The technical method combining vacuum continuous casting with metal water atomization powder making is superior to the currently commonly used traditional method (induction melting casting technology) in the uniformity of preparing metal standard samples.
[0113] Table 6 Comparison of results of X-ray fluorescence spectroscopy analysis of copper-tin alloy samples
[0114]
[0115] The steps in the above embodiments, unless otherwise specified, should not be understood as limiting the execution order. The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0116] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a metal alloy with improved composition uniformity, characterized in that: The method comprises: After the metal raw materials are weighed according to the proportion, continuous casting is performed to obtain a metal material casting embryo; Atomizing the metal material casting embryo to obtain a suspension of metal material powder and aqueous solution; The suspension is cleaned to clean the pollutants in the powder to obtain a cleaned liquid containing the metal material powder; The cleaned liquid containing the metal material powder is subjected to low-temperature drying of the powder at a temperature of 65° C. to 85° C. to obtain a dried metal powder; Screening the dried metal powder according to particle size to obtain metal powder with a mesh size within a preset mesh size range; Mixing metal powders with mesh sizes within a preset mesh size range to obtain mixed metal powders; The mixed metal powder is randomly sampled and placed into a powder metallurgy pressing die to press out a metal alloy standard sample blank.
2. The method according to claim 1, characterized in that: The method of subjecting the metal material casting embryo to water atomization powder making to obtain a suspension of metal material powder and aqueous solution comprises: Taking cross-sectional samples of the metal material casting embryo, and analyzing and detecting the uniformity of the cross-sectional area of the metal material casting embryo; When the uniformity reaches the preset requirement, the metal material casting embryo is subjected to water atomization powder making to obtain a suspension of metal material powder and aqueous solution.
3. The method according to claim 1, characterized in that: After sampling the cross section of the metal material casting embryo and analyzing and detecting the uniformity of the cross section of the metal material casting embryo, the method further includes: When the uniformity does not reach the preset requirement, continuous casting is continued to obtain a metal material casting embryo.
4. The method according to claim 1, characterized in that: The method of washing the suspension to wash the pollutants in the powder to obtain a washed liquid containing the metal material powder comprises: The suspension is allowed to settle and the supernatant is removed; Introduce pure water, stir thoroughly, let stand and settle, remove the supernatant, and wash away the pollutants in the powder; The steps of introducing pure water and stirring sufficiently, standing to settle, removing the upper clear liquid, and washing the pollutants in the powder are repeated at least once to obtain a washed liquid containing the metal material powder.
5. The method according to claim 1, characterized in that The cleaned liquid containing the metal material powder is subjected to low-temperature drying of the powder at a temperature of 65° C. to 85° C. to obtain the dried metal powder, comprising: Use a glass container to load the cleaned liquid containing the metal material powder, put it into an electric drying oven, and cover the mouth of the glass container with a beaker cover glass container; The drying temperature range of the electric drying oven is set to 65°C to 85°C, and the temperature fluctuation is maintained within the drying temperature range to dry the moisture of the powder at low temperature to obtain dried metal powder.
6. The method according to any one of claims 1 to 5, characterized in that: The preset mesh number range is between 400 and 80.
7. The method according to any one of claims 1 to 5, characterized in that: After randomly sampling the mixed metal powder and placing it into a powder metallurgy pressing mold to press out a metal alloy standard sample blank, the method further comprises: According to the preset strength requirement, the pressed metal alloy standard sample blank is sintered to obtain a sintered metal alloy standard sample semi-finished product.
8. The method according to claim 7, characterized in that After sintering the pressed metal alloy standard sample blank according to the preset strength requirement to obtain the sintered metal alloy standard sample semi-finished product, the method further comprises: The surface of the sintered metal alloy standard sample semi-finished product is polished to obtain a polished metal alloy standard sample.
9. The method according to claim 8, characterized in that The grinding process of the surface of the sintered metal alloy standard product to obtain the ground metal alloy standard sample comprises: By using X-ray fluorescence spectroscopy, the surface content changes of the sintered metal alloy standard samples were analyzed; The surface is polished; By using X-ray fluorescence spectroscopy, the changes in the surface content of metal components of the metal alloy standard sample after grinding were analyzed; determining a grinding depth according to the change; The sintered metal alloy standard sample semi-finished product is ground according to the grinding depth to obtain a ground metal alloy standard sample.
10. A metal alloy standard sample, characterized in that: The metal alloy standard product is prepared by the method for preparing a metal alloy with improved composition uniformity as described in any one of claims 1 to 9.