Method for preparing transition metal nanomaterial with multi-dimensional morphology in same reaction system at room temperature

By using solution self-assembly method under room temperature and using specific precursors and surfactants, the problem of poor controllability of multi-dimensional morphological nanomaterials under high temperature and high pressure in the prior art was solved, and the size and stable morphology were successfully prepared. The multidimensional cobalt nanomaterial simplifies the preparation process and has the potential for large-scale production.

CN118905238AActive Publication Date: 2024-11-08ANALYSIS & TESTING CENT CHINESE ACADEMY OF TROPICAL AGRI SCI
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411012961.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing preparation methods for multi-dimensional morphological transition metal nanomaterials require high temperature and high pressure conditions, and poor morphological controllability, making it difficult to obtain target materials with uniform size and stable morphology.

Method used

The same water-based solvent reaction system was adopted under room temperature, and the solution self-assembly method was used to combine formaldehyde and ethylenediamine as crosslinking agents such as cobalt nitrate hexahydrate, thiourea, dopamine and polyether F127, and the combination of formaldehyde and ethylenediamine as crosslinking agents , adjust the feeding order and reaction conditions of the precursor to achieve accurate regulation of the geometric morphology of N/S/Co co-doped nanomaterials, and prepare uniform size nanospheres, nanowires, nanosheets and nanoflowers.

Benefits of technology

Cobalt-doped nanomaterials with precise construction of multi-dimensional geometric morphology under room temperature conditions simplifies the preparation process, improves the morphological stability and dimensional uniformity of the material, and has the potential for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905238A_ABST
    Figure CN118905238A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a multi-dimensional morphology transition metal nano material in the same reaction system at room temperature, which comprises the following steps: dissolving polyether F127, thiourea and Co (NO3) 2.6 H2O in a mixed solution of deionized water and ethanol to obtain a solution A; then adding formaldehyde, ethidene diamine and dopamine into the solution A according to different sequences under the condition of stirring at room temperature to obtain a solution B, and continuously stirring to react until the reaction is finished; centrifuging and washing the obtained reaction substance, and then drying and crushing to obtain a brown final product. Cobalt nitrate hexahydrate, thiourea and dopamine are used as precursors, polyether F127 is used as a surfactant, formaldehyde and ethidene diamine are used as cross-linking agents, and the precursors (feeding sequence) and reaction conditions are ingeniously adjusted, so that the geometrical morphology of the N / S / Co co-doped nano material is precisely regulated and constructed; and the cobalt-doped nano material of nanospheres, nanowires, nanosheets and nanoflowers, which is uniform in size and stable in morphology, is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano material preparation, and more specifically to a method for preparing multi-dimensional transition metal nano materials in the same reaction system under room temperature. Background Art

[0002] Transition metal nanomaterials have high active surfaces, unique electron transport orbits and abundant surface vacancies, and have shown excellent catalytic activity, selectivity and stability in many catalytic reaction systems, and have become one of the hot research materials in the field of catalysis. With the continuous expansion and deepening of research, higher requirements are also put forward for the diversification of the morphology of metal nanomaterials.

[0003] The performance of transition metal nanomaterials depends largely on factors such as the composition, morphology, size and structure of nanoparticles. Therefore, the controllable preparation of transition metal nanomaterials with multidimensional morphology is one of the key directions of current nanomaterial research. Generally, nanomaterials can be divided into zero-dimensional, one-dimensional, two-dimensional and three-dimensional morphologies according to the morphological dimensions. The existing preparation methods of transition metal nanomaterials with multidimensional morphology usually require the addition of reducing agents, protective agents and etching agents in different reaction systems, which makes the preparation process cumbersome and time-consuming. In addition, the preparation process usually requires high temperature and high pressure experimental conditions, and the controllability of the material morphology is extremely low, making it difficult to obtain target materials with uniform size and stable morphology. At present, the precise design and controllable construction of the morphology of nanomaterials at the nanoscale is still one of the difficult problems in the field of nanomaterial research. Therefore, exploring and developing new methods for the preparation of metal nanomaterials with precise construction of multidimensional geometric morphology in the same reaction system under mild conditions can achieve the creation of more new nanomaterials with both structural artistry and advanced functions, which is a major breakthrough in the field of nanotechnology research. Summary of the invention

[0004] In view of this, the present invention provides a method for accurately constructing N / S / Co co-doped nanomaterials with multi-dimensional geometric morphology in the same water-based solvent reaction system at room temperature, based on the synthesis strategy of solution self-assembly, using hexahydrated cobalt nitrate, thiourea and dopamine as precursors, polyether F127 as surfactant, formaldehyde and ethylenediamine as cross-linking agents, by cleverly adjusting the precursors (feeding sequence) and reaction conditions, the geometric morphology of N / S / Co co-doped nanomaterials is precisely controlled and constructed, and cobalt-doped nanomaterials of nanospheres, nanowires, nanosheets and nanoflowers with uniform size and stable morphology are obtained. The preparation method involved in the present invention can effectively overcome the deficiencies in the synthesis of existing transition metal nanomaterials with multi-dimensional geometric morphology, and provide new ideas for the innovative development of transition metal nanomaterials with multi-dimensional geometric morphology.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing multi-dimensional morphology transition metal nanomaterials in a same reaction system under room temperature conditions comprises the following steps:

[0007] (1) Polyether F127, thiourea and Co(NO 3 ) 2 6H 2 O is dissolved in a mixture of deionized water and ethanol to obtain solution A;

[0008] (2) adding formaldehyde, ethylenediamine and dopamine to solution A in different orders under stirring at room temperature to obtain solution B, and continuing to stir the reaction until completion;

[0009] (3) Centrifuging and washing the reaction material obtained in step (2), and then drying and crushing to obtain a brown final product.

[0010] Further, preparation of zero-dimensional nanospheres:

[0011] In step (1), the weight ratio of polyether F127: thiourea: Co(NO 3 ) 2 6H 2 O=3:3.75:1.5, the amount of the polyether F127 in the mixed solution of deionized water and ethanol is 0.005 g / mL;

[0012] The volume ratio of deionized water: ethanol = 1:0, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0.3mL: 0.3g, the weight ratio of dopamine: polyether F127 = 1:1; dopamine, ethylenediamine, and formaldehyde were added in sequence, the stirring speed was 1250rpm, and the stirring time was 24h.

[0013] Further, one-dimensional nanowire preparation:

[0014] In step (1), the weight ratio of polyether F127: thiourea: Co(NO 3 ) 2 6H 2 O=3:3.75:1.5, the amount of the polyether F127 in the mixed solution of deionized water and ethanol is 0.005 g / mL;

[0015] The volume ratio of deionized water: ethanol = 1:1, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0mL: 0.3g, the weight ratio of dopamine: polyether F127 = 1:1; dopamine and formaldehyde were added in sequence, the stirring speed was 1250rpm, and the stirring time was 24h.

[0016] Further, preparation of two-dimensional nanosheets:

[0017] In step (1), the weight ratio of polyether F127: thiourea: Co(NO 3 )2 6H 2 O=0:3.75:1.5, the Co(NO 3 ) 2 6H 2 The amount of O in the mixture of deionized water and ethanol is 0.0025 g / mL;

[0018] Volume ratio of deionized water: ethanol = 1:0, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0.3mL: 0.3g, weight ratio of dopamine: Co(NO 3 ) 2 6H 2 O=2:1; ethylenediamine, formaldehyde and dopamine were added in sequence, with a stirring speed of 180 rpm and a stirring time of 24 h.

[0019] Further, three-dimensional nanoflower preparation:

[0020] In step (1), the weight ratio of polyether F127: thiourea: Co(NO 3 ) 2 6H 2 O=3:3.75:1.5, the amount of the polyether F127 in the mixed solution of deionized water and ethanol is 0.005 g / mL;

[0021] The volume ratio of deionized water: ethanol = 1:0, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0.3mL: 0.3g, the weight ratio of dopamine: polyether F127 = 1:1; ethylenediamine, formaldehyde, and dopamine were added in sequence, the stirring speed was 180rpm, and the stirring time was 24h.

[0022] Preferably, in step (3), the centrifugal speed is 10000 rpm and the time is 5 min; deionized water, ethanol and deionized water are added in sequence for washing.

[0023] Preferably, the drying temperature in step (3) is 80° C. and the drying time is 24 h.

[0024] It can be seen from the above technical solution that, compared with the prior art, the present invention discloses a method for preparing multi-dimensional morphology transition metal nanomaterials in the same reaction system under room temperature, which has the following beneficial effects:

[0025] The present invention uses a solution self-assembly method at room temperature to prepare cobalt metal nanomaterials with multi-dimensional morphology in the same reaction system, including zero-position nanospheres, one-dimensional nanowires, two-dimensional nanosheets, and three-dimensional nanoflowers. The synthesis method is simple and controllable, and has the potential for large-scale industrial production. The multi-dimensional cobalt metal nanomaterials prepared by the present invention have good uniformity and stability in morphology and size. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0027] Figure 1 This is a SEM image of the zero-position nanosphere prepared in Example 1;

[0028] Figure 2 This is a SEM image of the one-dimensional nanowires prepared in Example 2;

[0029] Figure 3 This is a SEM image of the two-dimensional nanosheet prepared in Example 3;

[0030] Figure 4 This is a SEM image of the three-dimensional nanoflower prepared in Example 4;

[0031] Figure 5 This is the XRD spectrum of the prepared multi-dimensional morphology target material. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] The preparation method of zero-dimensional nanospheres comprises the following steps:

[0035] Add 60 mL of deionized water to the reaction container, then weigh and add 0.3 g of polyether F127, 0.375 g of thiourea, and 0.15 g of cobalt nitrate hexahydrate in sequence, then add a magnetic stirrer for 15 minutes to allow the raw materials to fully dissolve, adjust the speed to 1250 r / min and maintain until the end of the reaction; pour in 0.3 g of dopamine hydrochloride powder and wait for 5 minutes; then add 0.3 mL of ethylenediamine at a uniform speed within 5 minutes, and wait for another 5 minutes after the addition is completed; finally, add 0.7 mL of formaldehyde to the solution at a uniform speed within 5 minutes, cover and react for 24 hours; after the reaction is completed, centrifuge and wash to obtain the product, the centrifugal washing rate is 10000 rpm, the time is 5 minutes, and deionized water, ethanol, and deionized water are added in sequence for washing; after centrifugation, place the product in an oven at 80°C for 24 hours to dry, and grind to obtain a brown powder.

[0036] Figure 1 The SEM image of the product shows that the product is a uniform zero-dimensional nanosphere with a diameter of about 200 to 300 nm.

[0037] Example 2

[0038] A method for preparing one-dimensional nanowires comprises the following steps:

[0039] Add 30mL of deionized water and 30mL of anhydrous ethanol to the reaction container, then weigh and add 0.3g of polyether F127, 0.375g of thiourea, and 0.15g of cobalt nitrate hexahydrate, then add a magnetic stirrer for 15 minutes to allow the raw materials to fully dissolve, adjust the speed to 1250r / min and maintain until the reaction is completed; pour in 0.3g of dopamine hydrochloride powder and wait for 5 minutes; then add 0.7mL of formaldehyde to the solution at a uniform speed within 5 minutes and cover the reaction for 24 hours; after the reaction is completed, centrifuge and wash to obtain the product, the centrifugal washing rate is 10000rpm, the time is 5 minutes, and deionized water, ethanol, and deionized water are added in turn for washing. After centrifugation, the product is placed in an oven at 80℃ for 24 hours and crushed to obtain a brown powder.

[0040] Figure 2 is the SEM image of the product, the product is a uniform one-dimensional nanowire with a diameter of about 200 nm.

[0041] Example 3

[0042] The method for preparing a two-dimensional nanosheet comprises the following steps:

[0043] Add 60 mL of deionized water to the reaction container, then weigh and add 0.375 g of thiourea and 0.15 g of cobalt nitrate hexahydrate in turn, then add a magnetic stirrer for 15 minutes to allow the raw materials to fully dissolve, adjust the rotation speed to 170-180 r / min and maintain until the end of the reaction; add 0.3 mL of ethylenediamine at a uniform speed within 5 minutes, and wait for 5 minutes after the addition is completed; add 0.7 mL of formaldehyde to the solution at a uniform speed within 5 minutes, and immediately pour in 0.3 g of dopamine hydrochloride powder, cover and react for 24 hours; after the reaction is completed, centrifuge and wash to obtain the product, the centrifugal washing rate is 10000 rpm, the time is 5 minutes, and deionized water, ethanol, and deionized water are added in turn for washing; after centrifugation, place the product in an oven at 80°C for 24 hours to dry, and grind to obtain a brown powder.

[0044] Figure 3 This is the SEM image of the product, which is uniform two-dimensional nanosheets with a diameter of about 400 nm.

[0045] Example 4

[0046] The method for preparing three-dimensional nanoflowers comprises the following steps:

[0047] Add 60 mL of deionized water to the reaction container, then weigh and add 0.3 g of polyether F127, 0.375 g of thiourea, and 0.15 g of cobalt nitrate hexahydrate in sequence, then add a magnetic stirring for 15 minutes to allow the raw materials to fully dissolve, adjust the rotation speed to 170-180 r / min and maintain until the end of the reaction; add 0.3 mL of ethylenediamine at a uniform speed within 5 minutes, wait for 5 minutes after the addition is completed; then add 0.7 mL of formaldehyde to the solution at a uniform speed within 5 minutes, and immediately pour in 0.3 g of dopamine hydrochloride powder, cover and react for 24 hours; after the reaction is completed, centrifuge and wash to obtain the product, the centrifugal washing rate is 10000 rpm, the time is 5 minutes, and deionized water, ethanol, and deionized water are added in sequence for washing; after centrifugation, the product is placed in an oven at 80°C for 24 hours to dry, and crushed to obtain a brown powder.

[0048] Figure 4 This is the SEM image of the product, which is uniform three-dimensional nanoflowers with a diameter of about 400 to 500 nm.

[0049] Figure 5 The XRD spectrum of the prepared multi-dimensional morphology target material is Figure 5 It can be seen that the diffraction peaks of the target material are consistent with the calibration cards Co (JCPDS card no. 15-0806) and Co 9 S 8 The diffraction peaks of (JCPDS card no.75-2023) are basically consistent. The diffraction peaks at diffraction angles 2θ = 44.3°, 51.4° and 75.8° correspond to the (111), (200) and (220) crystal planes of Co, respectively; the diffraction peaks at diffraction angles 2θ = 15.8°, 30.29°, 31.6°, 39.99°, 47.96° and 52.47° correspond to the (111), (200) and (220) crystal planes of Co, respectively. 9 S 8 The above results preliminarily prove that the prepared target material contains both Co and Co 9 S 8 Two crystalline phases.

[0050] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The above description of the disclosed embodiments enables professionals and technicians in this field to implement or use the present invention. Various modifications to these embodiments will be obvious to professionals and technicians in this field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will comply with the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature, characterized in that: The following steps are involved: (1) dissolving polyether F127, thiourea and Co(NO3)2·6H2O in a mixture of deionized water and ethanol to obtain solution A; (2) adding formaldehyde, ethylenediamine and dopamine to solution A in different orders under stirring at room temperature to obtain solution B, and continuing to stir the reaction until completion; (3) Centrifuging and washing the reaction material obtained in step (2), and then drying and crushing to obtain a brown final product.

2. The method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature according to claim 1, characterized in that: Preparation of zero-dimensional nanospheres: In step (1), the weight ratio of polyether F127:thiourea:Co(NO3)2·6H2O=3: 3.75:1.5, the amount of the polyether F127 in the mixed solution of deionized water and ethanol is 0.005 g / mL; The volume ratio of deionized water: ethanol = 1:0, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0.3mL: 0.3g, the weight ratio of dopamine: polyether F127 = 1:1; dopamine, ethylenediamine, and formaldehyde were added in sequence, the stirring speed was 1250rpm, and the stirring time was 24h.

3. The method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature according to claim 1, characterized in that: One-dimensional nanowire preparation: In step (1), the weight ratio of polyether F127:thiourea:Co(NO3)2·6H2O=3: 3.75:1.5, the amount of the polyether F127 in the mixed solution of deionized water and ethanol is 0.005 g / mL; The volume ratio of deionized water: ethanol = 1:1, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0mL: 0.3g, the weight ratio of dopamine: polyether F127 = 1:1; dopamine and formaldehyde were added in sequence, the stirring speed was 1250rpm, and the stirring time was 24h.

4. The method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature according to claim 1, characterized in that: Preparation of 2D nanosheets: In step (1), the weight ratio of polyether F127:thiourea:Co(NO3)2·6H2O=0:3.75:1.5, and the amount of Co(NO3)2·6H2O in the mixed solution of deionized water and ethanol is 0.0025 g / mL; The volume ratio of deionized water: ethanol = 1:0, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0.3mL: 0.3g, the weight ratio of dopamine: Co(NO3)2·6H2O = 2:1; ethylenediamine, formaldehyde, and dopamine were added in sequence, the stirring speed was 180rpm, and the stirring time was 24h.

5. The method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature according to claim 1, characterized in that: Preparation of three-dimensional nanoflowers: In step (1), the weight ratio of polyether F127:thiourea:Co(NO3)2·6H2O=3: 3.75:1.5, the amount of the polyether F127 in the mixed solution of deionized water and ethanol is 0.005 g / mL; The volume ratio of deionized water: ethanol = 1:0, formaldehyde: ethylenediamine: dopamine = 0.7mL: 0.3mL: 0.3g, the weight ratio of dopamine: polyether F127 = 1:1; ethylenediamine, formaldehyde, and dopamine were added in sequence, the stirring speed was 180rpm, and the stirring time was 24h.

6. The method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature according to claim 1, characterized in that: The centrifugal speed in step (3) is 10000 rpm and the time is 5 min; deionized water, ethanol and deionized water are added in sequence for washing.

7. The method for preparing multi-dimensional transition metal nanomaterials in a same reaction system under room temperature according to claim 1, characterized in that: The drying temperature in step (3) is 80° C. and the drying time is 24 h.

Citation Information

Patent Citations

  • Method for preparing metal sulfide / amine-hybrid nanomaterials and metal sulfide nanomaterials

    CN107572581A

  • Cobalt-sulfur compound / nitrogen-sulfur-doped carbon composite catalyst and preparation method thereof

    CN109888307A

  • Non-equilibrium state nanowire and preparation method thereof

    CN111137926A

  • Carbon-based composite material and preparation method and application thereof

    CN111889070A

  • Preparation method of sodium ion cobalt sulfide nanowire

    CN114394627A