Welding method for aluminum-titanium alloy target material assembly

By titanium permeation of the aluminum layer during the welding process of aluminum-titanium alloy target assembly, an optimized titanium permeation layer is formed, which solves the problems of insufficient welding strength and uncontrollable deformation, and achieves the welding effect of high strength and small deformation .

CN118905409APending Publication Date: 2024-11-08KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318313.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the welding method of existing aluminum-titanium alloy target components, the welding strength is insufficient and the deformation after welding cannot be effectively controlled.

Method used

The aluminum-titanium alloy target material, aluminum layer and back plate are assembled in turn, and the aluminum layer is permeated to form a titanium permeated layer with a thickness of 10-100μm, with a titanium content of 20-40%. , to optimize the connection effect, improve welding strength and reduce deformation.

Benefits of technology

The welding bonding strength of aluminum-titanium alloy target assembly is significantly improved, ensuring that the welding bonding strength is ≥150.5MPa and the deformation amount is ≤0.2mm, effectively controlling the deformation amount after welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905409A_ABST
    Figure CN118905409A_ABST
Patent Text Reader

Abstract

The invention relates to a welding method of an aluminum-titanium alloy target material assembly, in particular to the field of target material welding, and the welding method comprises the steps that after an aluminum-titanium alloy target material, an aluminum layer and a back plate are sequentially assembled, hot isostatic pressing welding is conducted, and the aluminum-titanium alloy target material assembly is obtained; wherein the aluminum layer is subjected to titanizing treatment, the thickness of the obtained titanizing layer is 10-100 [mu] m, and the content of titanium in the titanizing layer is 20-40% by mass. According to the welding method, the aluminum layer is subjected to specific titanizing treatment, the connecting effect of the aluminum-titanium alloy target and the back plate is optimized, the welding strength of the aluminum-titanium alloy target assembly is improved, and meanwhile the deformation amount of the target assembly obtained after welding is remarkably reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of target material welding, and in particular to a welding method for an aluminum-titanium alloy target material assembly. Background Art

[0002] At present, in the field of metal material welding technology, especially in the field of aluminum-titanium alloy target manufacturing, welding between the back plate and the target is a key link.

[0003] The main function of the back plate is to provide support for the target material and ensure the stability of the target material during use. In the existing technology, the target material and the back plate are usually welded by brazing. The advantages of this method are simple operation and low cost, but the welding strength is not high, and the use temperature cannot exceed 100°C, otherwise there is a risk of desoldering, which greatly limits its scope of use.

[0004] Another solution is diffusion welding. Although this method can improve welding strength and expand the operating temperature range, it will cause the target material to bulge upward and deform. Due to the high brittleness of aluminum-titanium alloy targets, it may cause cracking.

[0005] For example, CN117161534A discloses a welding method for an aluminum-titanium alloy target and an aluminum alloy back plate, comprising: an aluminum-titanium alloy target, an intermediate layer and an aluminum alloy back plate, heat treating the aluminum-titanium alloy target and the intermediate layer to obtain an aluminum-titanium alloy target-intermediate layer; applying pressure to the surface of the aluminum-titanium alloy target of the aluminum-titanium alloy target-intermediate layer, and then assembling the aluminum alloy back plate and the aluminum-titanium alloy target-intermediate layer to obtain a target assembly; placing the target assembly in a sheath for hot isostatic pressing welding. The binding method is not only complicated in process, but also has little effect on reducing the deformation after hot isostatic pressing welding.

[0006] It can be seen that the welding method of the aluminum-titanium alloy target assembly disclosed in the prior art still has the defects of insufficient welding strength and the deformation after welding cannot be effectively controlled. Summary of the invention

[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a welding method for an aluminum-titanium alloy target assembly to solve the defects of the welding method for an aluminum-titanium alloy target assembly, that is, the welding strength is insufficient and the deformation after welding cannot be effectively controlled.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a welding method for an aluminum-titanium alloy target assembly, the welding method comprising:

[0010] After assembling the aluminum-titanium alloy target, the aluminum layer and the back plate in sequence, hot isostatic pressing welding is performed to obtain an aluminum-titanium alloy target assembly;

[0011] The aluminum layer is titanium-diffused, and the thickness of the obtained titanium-diffused layer is 10-100 μm. The titanium content in the titanium-diffused layer is 20-40% by mass.

[0012] The welding method provided by the present invention optimizes the connection effect between the aluminum-titanium alloy target and the back plate by performing a specific titanium infiltration treatment on the aluminum layer, thereby improving the welding strength of the aluminum-titanium alloy target assembly while significantly reducing the deformation of the target assembly obtained after welding.

[0013] As a preferred technical solution of the present invention, the welding surface of the aluminum-titanium alloy target is provided with threads.

[0014] Preferably, the pitch of the threads is 0.4-0.5 mm.

[0015] Preferably, the depth of the thread is 0.1-0.2 mm.

[0016] As a preferred technical solution of the present invention, the thickness of the aluminum layer is 2-4 mm.

[0017] As a preferred technical solution of the present invention, the back plate is a concave back plate.

[0018] Preferably, the aluminum-titanium alloy target and the aluminum layer are placed in the groove of the concave back plate.

[0019] Preferably, the aluminum layer is located between the aluminum-titanium alloy target and the backing plate.

[0020] Preferably, the depth of the groove in the concave back plate is equal to the sum of the thickness of the aluminum-titanium alloy target and the thickness of the aluminum layer.

[0021] As a preferred technical solution of the present invention, the temperature of the hot isostatic pressing welding is 400-500°C.

[0022] Preferably, the hot isostatic pressing welding pressure is 100-120 MPa.

[0023] As a preferred technical solution of the present invention, the hot isostatic pressing welding time is 4-6 hours.

[0024] As a preferred technical solution of the present invention, the assembling comprises: assembling the cover plate, the isolation layer, the aluminum-titanium alloy target, the aluminum layer and the back plate in sequence.

[0025] As a preferred technical solution of the present invention, the material of the cover plate includes stainless steel.

[0026] Preferably, the cover plate has a thickness of 20-30 mm.

[0027] Preferably, the isolation layer comprises a stainless steel isolation layer.

[0028] Preferably, the thickness of the isolation layer is 0.2-0.4 mm.

[0029] As a preferred technical solution of the present invention, the assembled body is placed in a sheath for degassing and then hot isostatic pressing welding is performed.

[0030] As a preferred technical solution of the present invention, the temperature of the degassing treatment is 300-400°C.

[0031] Preferably, the absolute vacuum degree of the degassing treatment is ≤0.002Pa.

[0032] Preferably, the degassing treatment time is 3-4 hours.

[0033] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0034] The welding method provided by the present invention improves the welding bonding degree of the target material obtained by welding by introducing a titanium-infiltrated aluminum layer during the welding process to strengthen the alloy phase formed during the hot isostatic pressing process, while ensuring that the target material assembly has a small deformation amount, the welding bonding strength is ≥150.5MPa, and the deformation amount is ≤0.2mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the assembly of the welding object in the embodiment of the present invention.

[0036] In the figure: 1-cover plate, 2-isolation layer, 3-aluminum-titanium alloy target, 4-aluminum layer, 5-back plate.

[0037] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0038] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0039] This embodiment provides a welding method for an aluminum-titanium alloy target assembly, the welding method comprising:

[0040] The cover plate 1, the isolation layer 2, the aluminum-titanium alloy target 3, the aluminum layer 4 and the back plate 5 are assembled, and the obtained assembly is as follows. Figure 1 As shown, the target is then degassed in the package and then hot isostatic pressing is performed to obtain an aluminum-titanium alloy target assembly;

[0041] The aluminum layer 4 is titanium-diffused, and the thickness of the obtained titanium-diffused layer is 10-100 μm. The titanium content in the titanium-diffused layer is 20-40% by mass.

[0042] Exemplarily, the mass percentage composition of the aluminum-titanium alloy target material used is: 36-38% titanium, and the balance is aluminum.

[0043] In the present invention, the titanium infiltration treatment of the aluminum layer 4 refers to titanium infiltration of the surface of the aluminum layer 4 that contacts the aluminum-titanium alloy target 3 and the back plate 5 during welding, so as to ensure the final welding effect.

[0044] In the present invention, the titanium content in the obtained titanium-diffused layer is 20-40% by mass, for example, it can be 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38% or 40%, etc., but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0045] In the present invention, the thickness of the titanium infiltrated layer is 10-100 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 660 μm, 70 μm, 880 μm, 90 μmh or 100 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0046] In the present invention, the titanium diffusion treatment method includes ion implantation, double glow plasma surface alloying, vacuum solid titanium diffusion and other commonly used methods in the field to titanium diffuse the aluminum layer 4. The specific relevant parameters can be designed according to the conventional requirements in the field to ensure that the thickness of the titanium diffusion layer of the present invention is achieved.

[0047] In the present invention, the aluminum layer 4 includes an aluminum alloy layer, such as a 1060 aluminum alloy series aluminum alloy or other aluminum alloy layers commonly used in the art.

[0048] Specifically, the cover plate 1 is made of stainless steel.

[0049] Specifically, the thickness of the cover plate 1 is 20-30 mm, for example, it can be 20 mm, 21 mm, 22 mm, 23 mm, 24 mm, 25 mm, 26 mm, 27 mm, 28 mm, 29 mm or 30 mm, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0050] Specifically, the isolation layer 2 includes a stainless steel isolation layer.

[0051] Specifically, the thickness of the isolation layer 2 is 0.2-0.4 mm, for example, it can be 0.2 mm, 0.21 mm, 0.22 mm, 0.23 mm, 0.24 mm, 0.25 mm, 0.26 mm, 0.27 mm, 0.28 mm, 0.29 mm, 0.3 mm, 0.31 mm, 0.32 mm, 0.33 mm, 0.34 mm, 0.35 mm, 0.36 mm, 0.37 mm, 0.38 mm, 0.39 mm or 0.4 mm, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0052] In this embodiment, the stainless steel used can be selected from 304 stainless steel, 316 stainless steel, 420 stainless steel, etc.

[0053] Specifically, the welding surface of the aluminum-titanium alloy target 3 is provided with threads.

[0054] In the present invention, the cross-sectional shape of the thread, i.e., the tooth profile, is exemplarily a triangular thread, a rectangular thread, a trapezoidal thread, and a serrated thread. Corresponding to threads of different shapes, the thread depth defined in the present invention is the maximum depth of the thread.

[0055] Among them, the pitch of the thread is 0.4-0.5mm, for example, it can be 0.4mm, 0.41mm, 0.42mm, 0.43mm, 0.44mm, 0.45mm, 0.46mm, 0.47mm, 0.48mm, 0.49mm or 0.5mm, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0056] Among them, the depth of the thread is 0.1-0.2mm, for example, it can be 0.1mm, 0.11mm, 0.12mm, 0.13mm, 0.14mm, 0.15mm, 0.16mm, 0.17mm, 0.18mm, 0.19mm or 0.2mm, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0057] Specifically, the thickness of the aluminum layer 4 is 2-4 mm, for example, it can be 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, 3 mm, 3.1 mm, 3.2 mm, 3.3 mm, 3.4 mm, 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm, 3.9 mm or 4 mm, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0058] Specifically, the back plate 5 is a concave back plate.

[0059] The aluminum-titanium alloy target material 3 and the aluminum layer 4 are placed in the groove of the concave back plate.

[0060] The aluminum layer 4 is located between the aluminum-titanium alloy target 3 and the back plate 5 .

[0061] In the present invention, the material of the back plate 5 includes aluminum alloy, for example, 6061 aluminum alloy and other series aluminum alloys can be selected.

[0062] Wherein, the temperature of the degassing treatment is 300-400°C, for example, it can be 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0063] Among them, the absolute vacuum degree of the degassing treatment is ≤0.002Pa, for example, it can be 0.002Pa, 0.0018Pa, 0.002Pa, 0.0016Pa, 0.0014Pa, 0.0012Pa, 0.001Pa, 0.0008Pa, 0.0006Pa, 0.0004Pa, 0.0002Pa, 0.0001Pa or 0.00001Pa, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0064] The degassing time is 3-4 hours, for example, 3 hours, 3.1 hours, 3.2 hours, 3.3 hours, 3.4 hours, 3.5 hours, 3.6 hours, 3.7 hours, 3.8 hours, 3.9 hours or 4 hours, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0065] Among them, the temperature of the hot isostatic pressing welding is 400-500°C, for example, it can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0066] Among them, the pressure of the hot isostatic pressing welding is 100-120MPa, for example, it can be 100MPa, 102MPa, 104MPa, 106MPa, 108MPa, 110MPa, 112MPa, 114MPa, 116MPa, 118MPa or 120MPa, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0067] Among them, the hot isostatic pressing welding time is 4-6h, for example, it can be 4h, 4.2h, 4.4h, 4.6h, 4.8h, 5h, 5.2h, 5.4h, 5.6h, 5.8 or 6h, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0068] Furthermore, in the present invention, before assembling the cover plate 1, the isolation layer 2, the aluminum-titanium alloy target 3, the aluminum layer 4 and the back plate 5, each component can be optionally cleaned separately to remove surface oil, other stains and oxide layers, etc.

[0069] The cleaning operation can be carried out by acid washing, alkali washing, alcohol washing and the like. At the same time, the cleaning process can also be assisted by ultrasonic or microwave auxiliary measures to achieve effective removal of dirt.

[0070] Furthermore, in order to illustrate the good welding effect that can be achieved by the target assembly obtained by the welding method provided by the present invention, an actual example is used for illustration, as follows:

[0071] Example 1

[0072] This embodiment provides a welding method for an aluminum-titanium alloy target assembly, the welding method comprising:

[0073] The cover plate 1, the isolation layer 2, the aluminum-titanium alloy target 3, the aluminum layer 4 and the back plate 5 are assembled in sequence, and then degassed in a package, and then hot isostatic pressing welding is performed to obtain an aluminum-titanium alloy target assembly;

[0074] The material of the cover plate 1 is 304 stainless steel; the thickness of the cover plate 1 is 24 mm;

[0075] The isolation layer 2 is a 304 stainless steel isolation layer; the thickness of the isolation layer 2 is 0.3 mm;

[0076] The mass percentage composition of the aluminum-titanium alloy target material used is: 37.2% titanium, the balance is aluminum; the welding surface of the aluminum-titanium alloy target material 3 is provided with rectangular threads; the pitch of the threads is 0.47 mm; the depth of the threads is 0.15 mm;

[0077] The aluminum layer 4 has a thickness of 3 mm and is a 1060 aluminum alloy layer; the aluminum layer 4 is subjected to titanium infiltration treatment, and the thickness of the obtained titanium infiltration layer is 40 μm, and the titanium content is 30% by mass;

[0078] The back plate 5 is a concave back plate, which is a 6061 aluminum alloy back plate; the aluminum-titanium alloy target 3 and the aluminum layer 4 are placed in the groove of the concave back plate; the aluminum layer 4 is located between the aluminum-titanium alloy target 3 and the back plate 5; the depth of the groove in the concave back plate is equal to the sum of the thickness of the aluminum-titanium alloy target 3 and the thickness of the aluminum layer 4;

[0079] The temperature of the degassing treatment is 350°C; the absolute vacuum degree of the degassing treatment is 0.0005Pa; and the time of the degassing treatment is 3.5h;

[0080] The temperature of the hot isostatic pressing welding is 450° C.; the pressure of the hot isostatic pressing welding is 110 MPa; and the time of the hot isostatic pressing welding is 5 hours.

[0081] Example 2

[0082] This embodiment provides a welding method for an aluminum-titanium alloy target assembly, the welding method comprising:

[0083] The cover plate 1, the isolation layer 2, the aluminum-titanium alloy target 3, the aluminum layer 4 and the back plate 5 are assembled in sequence, and then degassed in a package, and then hot isostatic pressing welding is performed to obtain an aluminum-titanium alloy target assembly;

[0084] The material of the cover plate 1 is 316 stainless steel; the thickness of the cover plate 1 is 27 mm;

[0085] The isolation layer 2 is a 420 stainless steel isolation layer; the thickness of the isolation layer 2 is 0.35 mm;

[0086] The mass percentage composition of the aluminum-titanium alloy target material used is: 38% titanium and the balance aluminum; the welding surface of the aluminum-titanium alloy target material 3 is provided with a triangular thread; the pitch of the thread is 0.45 mm; the depth of the thread is 0.18 mm;

[0087] The aluminum layer 4 has a thickness of 3.5 mm and is a 1060 aluminum alloy layer; the aluminum layer 4 is subjected to titanium infiltration treatment, and the thickness of the obtained titanium infiltration layer is 70 μm, and the titanium content is 35% by mass;

[0088] The back plate 5 is a concave back plate, which is a 6061 aluminum alloy back plate; the aluminum-titanium alloy target 3 and the aluminum layer 4 are placed in the groove of the concave back plate; the aluminum layer 4 is located between the aluminum-titanium alloy target 3 and the back plate 5; the depth of the groove in the concave back plate is equal to the sum of the thickness of the aluminum-titanium alloy target 3 and the thickness of the aluminum layer 4;

[0089] The temperature of the degassing treatment is 380°C; the absolute vacuum degree of the degassing treatment is 0.001Pa; and the time of the degassing treatment is 3.2h;

[0090] The temperature of the hot isostatic pressing welding is 480° C.; the pressure of the hot isostatic pressing welding is 115 MPa; and the time of the hot isostatic pressing welding is 4.5 hours.

[0091] Example 3

[0092] This embodiment provides a welding method for an aluminum-titanium alloy target assembly, the welding method comprising:

[0093] The cover plate 1, the isolation layer 2, the aluminum-titanium alloy target 3, the aluminum layer 4 and the back plate 5 are assembled in sequence, and then degassed in a package, and then hot isostatic pressing welding is performed to obtain an aluminum-titanium alloy target assembly;

[0094] The material of the cover plate 1 is 420 stainless steel; the thickness of the cover plate 1 is 20 mm;

[0095] The isolation layer 2 is a 304 stainless steel isolation layer; the thickness of the isolation layer 2 is 0.4 mm;

[0096] The mass percentage composition of the aluminum-titanium alloy target material used is: 36.5% titanium, the balance is aluminum; the welding surface of the aluminum-titanium alloy target material 3 is provided with a triangular thread; the pitch of the thread is 0.4mm; the depth of the thread is 0.1mm;

[0097] The aluminum layer 4 has a thickness of 2 mm and is a 1060 aluminum alloy layer; the aluminum layer 4 is subjected to titanium infiltration treatment, and the thickness of the obtained titanium infiltration layer is 100 μm, and the titanium content is 20% by mass;

[0098] The back plate 5 is a concave back plate, which is a 6061 aluminum alloy back plate; the aluminum-titanium alloy target 3 and the aluminum layer 4 are placed in the groove of the concave back plate; the aluminum layer 4 is located between the aluminum-titanium alloy target 3 and the back plate 5; the depth of the groove in the concave back plate is equal to the sum of the thickness of the aluminum-titanium alloy target 3 and the thickness of the aluminum layer 4;

[0099] The temperature of the degassing treatment is 300°C; the absolute vacuum degree of the degassing treatment is 0.002Pa; and the time of the degassing treatment is 4h;

[0100] The temperature of the hot isostatic pressing welding is 500° C.; the pressure of the hot isostatic pressing welding is 100 MPa; and the time of the hot isostatic pressing welding is 4 hours.

[0101] Example 4

[0102] This embodiment provides a welding method for an aluminum-titanium alloy target assembly, the welding method comprising:

[0103] The cover plate 1, the isolation layer 2, the aluminum-titanium alloy target 3, the aluminum layer 4 and the back plate 5 are assembled in sequence, and then degassed in a package, and then hot isostatic pressing welding is performed to obtain an aluminum-titanium alloy target assembly;

[0104] The material of the cover plate 1 is 316 stainless steel; the thickness of the cover plate 1 is 30 mm;

[0105] The isolation layer 2 is a 304 stainless steel isolation layer; the thickness of the isolation layer 2 is 0.2 mm;

[0106] The mass percentage composition of the aluminum-titanium alloy target material used is: 36% titanium and the balance aluminum; the welding surface of the aluminum-titanium alloy target material 3 is provided with rectangular threads; the pitch of the threads is 0.5 mm; the depth of the threads is 0.2 mm;

[0107] The aluminum layer 4 has a thickness of 4 mm and is a 1060 aluminum alloy layer; the aluminum layer 4 is subjected to titanium infiltration treatment, and the thickness of the obtained titanium infiltration layer is 10 μm, and the titanium content is 40% by mass;

[0108] The back plate 5 is a concave back plate, which is a 6061 aluminum alloy back plate; the aluminum-titanium alloy target 3 and the aluminum layer 4 are placed in the groove of the concave back plate; the aluminum layer 4 is located between the aluminum-titanium alloy target 3 and the back plate 5; the depth of the groove in the concave back plate is equal to the sum of the thickness of the aluminum-titanium alloy target 3 and the thickness of the aluminum layer 4;

[0109] The temperature of the degassing treatment is 400°C; the absolute vacuum degree of the degassing treatment is 0.0015Pa; the time of the degassing treatment is 3h;

[0110] The temperature of the hot isostatic pressing welding is 400° C.; the pressure of the hot isostatic pressing welding is 120 MPa; and the time of the hot isostatic pressing welding is 6 hours.

[0111] Comparative Example 1

[0112] The only difference from Example 1 is that the aluminum layer is not subjected to titanium infiltration treatment.

[0113] Comparative Example 2

[0114] The only difference from Example 1 is that the titanium-infiltrated layer is replaced by a titanium foil of equal thickness.

[0115] Comparative Example 3

[0116] The only difference from Example 1 is that the aluminum layer is replaced by a pure aluminum layer (with a purity of 99.5%) of equal thickness.

[0117] Comparative Example 4

[0118] The only difference from Example 1 is that the thickness of the titanium-infiltrated layer in the aluminum layer is 5 μm.

[0119] Comparative Example 5

[0120] The only difference from Example 1 is that the titanium content in the titanium-infiltrated layer in the aluminum layer is 10% by mass.

[0121] Comparative Example 6

[0122] The only difference from Example 1 is that the titanium content in the titanium-infiltrated layer in the aluminum layer is 60% by mass.

[0123] The target material assemblies obtained in the examples and comparative examples were tested for welding performance and deformation, and the results are shown in Table 1 below.

[0124] Table 1

[0125]

[0126]

[0127] It can be seen from Table 1 that in the solution provided by the present invention, by performing a specific titanium infiltration treatment on the aluminum layer, the connection effect between the aluminum-titanium alloy target and the back plate is optimized, the welding strength of the aluminum-titanium alloy target assembly is improved, and the deformation of the target assembly obtained after welding is significantly reduced.

[0128] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0129] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0130] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0131] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A welding method for an aluminum-titanium alloy target assembly, characterized in that: The welding method comprises: After assembling the aluminum-titanium alloy target, the aluminum layer and the back plate in sequence, hot isostatic pressing welding is performed to obtain an aluminum-titanium alloy target assembly; The aluminum layer is titanium-diffused, and the thickness of the obtained titanium-diffused layer is 10-100 μm. The titanium content in the titanium-diffused layer is 20-40% by mass.

2. The welding method according to claim 1, characterized in that The welding surface of the aluminum-titanium alloy target is provided with threads; Preferably, the pitch of the threads is 0.4-0.5 mm; Preferably, the depth of the thread is 0.1-0.2 mm.

3. The welding method according to claim 1 or 2, characterized in that: The thickness of the aluminum layer is 2-4 mm.

4. The welding method according to any one of claims 1 to 3, characterized in that: The back plate is a concave back plate; Preferably, the aluminum-titanium alloy target and the aluminum layer are placed in the groove of the concave back plate; Preferably, the aluminum layer is located between the aluminum-titanium alloy target and the backing plate; Preferably, the depth of the groove in the concave back plate is equal to the sum of the thickness of the aluminum-titanium alloy target and the thickness of the aluminum layer.

5. The welding method according to any one of claims 1 to 4, characterized in that: The temperature of the hot isostatic pressing welding is 400-500°C; Preferably, the hot isostatic pressing welding pressure is 100-120 MPa.

6. The welding method according to any one of claims 1 to 5, characterized in that: The hot isostatic pressing welding time is 4-6 hours.

7. The welding method according to any one of claims 1 to 6, characterized in that: The assembly comprises: assembling a cover plate, an isolation layer, an aluminum-titanium alloy target, an aluminum layer and a back plate in sequence.

8. The welding method according to claim 7, characterized in that: The material of the cover plate includes stainless steel; Preferably, the thickness of the cover plate is 20-30 mm; Preferably, the isolation layer comprises a stainless steel isolation layer; Preferably, the thickness of the isolation layer is 0.2-0.4 mm.

9. The welding method according to any one of claims 1 to 8, characterized in that: The assembled body is placed in a sheath for degassing and then hot isostatic pressing welding is performed.

10. The welding method according to claim 9, characterized in that: The temperature of the degassing treatment is 300-400°C; Preferably, the absolute vacuum degree of the degassing treatment is ≤0.002Pa; Preferably, the degassing treatment time is 3-4 hours.