Friction stir welding joint strong plasticizing method based on thermal coupling regulation and control
By combining cold rolling, stress removal annealing and solid solution aging heat treatment in the friction stir welding joint, the uneven distribution of enhanced phase particles and thinning of welded joints in the in-situ self-generated TiB2/2024 aluminum-based composite welded joints is solved, which is significant. Improves the mechanical and fatigue properties of the joints.
Patent Information
- Application Number
- CN202410988078.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
In-situ self-generating TiB2/2024 aluminum-based composite material has uneven distribution of enhanced phase particles after friction stir welding, which affects the mechanical properties of the joints, and the weld area is prone to thinning, resulting in poor hardness and fatigue performance of the welded joints.
The strong plasticization method of friction stir welding joints based on thermal coupling control is adopted, including friction stir welding, cold rolling, stress removal annealing and solid solution aging heat treatment. The geometric inhomogeneity of the welded joints is improved through cold rolling, and stress removal annealing reduces residual stress , solid solution aging heat treatment inhibits abnormal growth of grains in the weld area and improves the microhardness and plasticity of the joints.
It significantly improves the comprehensive mechanical properties of the welded joints, improves the uniformity of phase particles distribution, solves the problem of thinning in the weld area, improves the fatigue performance and elongation of the joints, and the microhardness distribution of the joints tends to be uniform.
Smart Images

Figure CN118905411A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stir friction welding, and in particular relates to a method for strengthening and plasticizing a stir friction welding joint based on thermal coupling regulation. Background Art
[0002] TiB2 has good wettability with aluminum matrix, making it an ideal reinforcement phase for aluminum-based composites. In-situ self-generated TiB2 aluminum-based composites have attracted widespread attention due to their many advantages such as higher strength, excellent wear resistance, and good interface bonding between particles and matrix. They are expected to be used in components such as short longitudinal beams of aircraft cargo floor, lateral supports and corner pieces of cabin floor, and have great potential to develop into the next generation of new aviation materials. Due to the size limitations of in-situ self-generated aluminum-based composites, welding operations are inevitable in some application conditions. Stir friction welding has been widely used in the welding of aluminum-based composites due to its outstanding solid-state metallurgical advantages and can completely avoid various metallurgical defects that occur during fusion welding. The high-temperature fluidity of aluminum-based composites is significantly lower than that of aluminum alloys. Therefore, the welding process window of stir friction welding of aluminum-based composites is narrower than that of aluminum alloys. At the same time, the reinforcement phase particles will gather in the upper part of the stirring zone, resulting in uneven distribution of the reinforcement phase particles, which will affect the service performance of the joint. To this end, it is urgent to provide a method that can effectively improve the uneven distribution of reinforcement phase particles and enhance the strength and plasticization of the joint. Summary of the invention
[0003] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for strengthening and plasticizing a stir friction welding joint based on thermal coupling regulation. The method can effectively improve the uneven distribution of reinforcing phase particles, which is conducive to making the hardness of the joint evenly distributed. At the same time, it can significantly improve the comprehensive mechanical properties of the welded joint.
[0004] In order to achieve the above object, the present invention provides a method for strengthening and plasticizing a friction stir welding joint based on thermal coupling regulation, comprising the following steps:
[0005] Step 1: Friction stir welding:
[0006] First, two plates to be welded are butt-jointed and clamped on a friction stir welding machine; then the stirring head is used to perform friction stir butt welding at a welding process parameter of a rotation speed of 600 to 1000 r / min and a welding speed of 100 to 300 mm / min to obtain a high-quality welded joint;
[0007] Step 2: Cold rolling:
[0008] At room temperature, the welded joint is cold-rolled twice using a rolling mill, with the rolling direction perpendicular to the welding direction, and the total deformation is controlled within a range of 15 to 35%;
[0009] Step 3: Stress relief annealing treatment:
[0010] The cold-rolled welded joint is flattened and then subjected to stress relief annealing at 150°C for 24 hours;
[0011] Step 4: Solution aging heat treatment:
[0012] The welded joints after cold rolling and stress relief annealing are subjected to solution aging heat treatment: first, solution treatment is carried out at a solution temperature of 485-510°C and a solution time of 0.8-1.2h, then furnace cooling is performed, and finally, artificial aging treatment is carried out at an aging temperature of 170-195°C and an aging time of 8-12h.
[0013] Furthermore, in order to fully improve the comprehensive mechanical properties of the welded joint, in step one, the plate to be welded is a plate made of in-situ self-generated TiB2 / 2024 aluminum-based composite material, and its thickness is 2 mm.
[0014] Furthermore, in order to effectively improve the geometric non-uniformity of the thickness of the weld joint, in step 2, during the rolling process of the weld joint, the diameter of the roller is 220 mm, the speed of the roller is 8 to 10 r / min, and the total deformation is controlled to be 15 to 35%.
[0015] Furthermore, in order to significantly improve the hardness of the weld, heat-affected zone, base material, and weld, in step 4, the heating rate of the solution treatment is 10°C / min, and the heating rate of the artificial aging is 5°C / min. At the same time, both the solution treatment and artificial aging first heat the heat treatment furnace to the specified temperature, and then place the workpiece to be treated in the furnace for heating.
[0016] As a preferred embodiment, in step 4, the solution treatment is performed by water cooling, and the artificial aging is performed by furnace cooling.
[0017] Furthermore, in order to effectively solve the problem of aggregation and unevenness of the reinforcement phase particles inside the material, in step one, the rotation speed of the stirring head is 600-1000 r / min, the welding speed is 100-300 mm / min, and the downward pressure is 0.2 mm.
[0018] Furthermore, in order to obtain high-quality welding joints, in step one, before clamping, first use a stainless steel brush to manually clean the 10 mm surface on both sides of the front and back of the welding head, then use acetone or ethanol to scrub the surface of the welding head, and then perform the clamping operation.
[0019] Furthermore, in order to obtain a weld joint with better performance, in step one, the starting end and the tail end of the obtained weld joint are removed, and the middle stably formed joint portion is retained.
[0020] The present invention discloses a welding joint strengthening and plasticizing method based on thermomechanical coupling regulation for in-situ self-generated TiB2 / 2024 aluminum-based composite material stir friction welding. Since the in-situ self-generated TiB2 / 2024 aluminum-based composite material will be significantly thinned after stir friction welding, and a recrystallization process will occur, direct heat treatment after welding may cause abnormal grain growth in the weld area. After cold rolling, the problem of weld thinning can be effectively reduced, and the weld grains that grow abnormally after post-weld heat treatment can be effectively refined, thereby significantly improving the comprehensive mechanical properties of the weld joint. Therefore, the present invention can fully improve the geometric inhomogeneity problem in the thickness of the weld joint by performing two cold rolling treatments on the weld joint. The corresponding weld joint strength can be significantly improved, and at the same time, the weld microhardness can be significantly improved. Since the elongation of the weld joint occurs in the low hardness area due to the severe strain / stress localization in the stretching process, and the rolling process further increases the inhomogeneity of the hardness distribution of the weld joint, the elongation of the joint is significantly reduced. In this way, by first flattening the weld joint and performing stress relief treatment at a temperature of 150°C for 24 hours, the residual stress introduced by the cold rolling process can be effectively reduced or eliminated. Then, through solid solution aging heat treatment, the cold-rolled weld joint structure can be recrystallized, effectively inhibiting the abnormal grain growth in the weld area caused by direct heat treatment. At the same time, the microhardness distribution of the joint tends to be uniform, which significantly improves the plasticity of the joint. After cold rolling and solid solution aging treatment, the problem of weld thinning and residual stress optimization can also be solved, which is expected to significantly improve the fatigue performance of the joint.
[0021] In summary, the present invention significantly improves the comprehensive mechanical properties of the in-situ self-generated TiB2 / 2024 aluminum-based composite material stir friction welding joint through the coupling effect of "cold rolling + heat treatment", and solves the thinning problem of the stir friction welding weld area. At the same time, the "cold rolling + heat treatment" process improves the residual stress distribution of the joint, which is expected to improve the fatigue performance of the joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the cross-sectional macroscopic morphology of the welded joint;
[0023] Figure 2 This is a cross-sectional macroscopic morphology of the joint obtained under the "cold rolling + heat treatment" condition of the present invention;
[0024] Figure 3 It is a schematic diagram of the position distribution of the microhardness test points of the welded joint obtained by the present invention;
[0025] Figure 4 It is the cross-sectional microhardness distribution diagram of the welded and “cold rolled + heat treated” joints;
[0026] Figure 5 is the geometrical dimensions of the tensile test specimen of the welded joint obtained by the present invention;
[0027] Figure 6 It is a bar graph of tensile properties of welded and “cold rolled + heat treated” joints. DETAILED DESCRIPTION
[0028] The present invention is further described below.
[0029] like Figures 1 to 6 As shown, the present invention provides a method for strengthening and plasticizing a friction stir welding joint based on thermal coupling regulation, comprising the following steps:
[0030] Step 1: Friction stir welding:
[0031] First, two plates to be welded are butt-jointed and clamped on a friction stir welding machine; then the stirring head is used to perform friction stir butt welding at a welding process parameter of a rotation speed of 600 to 1000 r / min and a welding speed of 100 to 300 mm / min to obtain a high-quality welded joint;
[0032] As a preferred embodiment, the stirring head is moved in a direction parallel to the joint of the workpiece to be welded to complete the friction stir welding operation of the material to be welded;
[0033] Step 2: Cold rolling:
[0034] At room temperature, the welded joint is cold-rolled twice using a rolling mill, with the rolling direction perpendicular to the welding direction, and the total deformation is controlled within a range of 15 to 35%;
[0035] Step 3: stress relief annealing treatment;
[0036] The cold-rolled welded joint is flattened and then subjected to stress relief annealing at 150°C for 24 hours;
[0037] As a preferred embodiment, a cold rolling mill is used to flatten the welded joint;
[0038] Step 4: Aging heat treatment after welding:
[0039] The welded joints after cold rolling and stress relief annealing are subjected to solution aging heat (T6) treatment: first, solution treatment is carried out at a solution temperature of 485-510°C and a solution time of 0.8-1.2h, then furnace cooling is performed, and finally, artificial aging treatment is carried out at an aging temperature of 170-195°C and an aging time of 8-12h.
[0040] In order to fully improve the comprehensive mechanical properties of the welded joint, in step 1, the plate to be welded is a plate made of in-situ self-generated TiB2 / 2024 aluminum-based composite material, and its thickness is 2 mm.
[0041] In order to effectively improve the geometric non-uniformity of the thickness of the weld joint, in step 2, during the cold rolling of the weld joint, the diameter of the roller is 220 mm, the speed of the roller is 8-10 r / min, and the total deformation is controlled to be 15-35%.
[0042] In order to significantly improve the hardness of the weld, heat-affected zone, base material and weld, in step 4, the heating rate of the solution treatment is 10°C / min, and the heating rate of the artificial aging is 5°C / min. At the same time, both the solution treatment and artificial aging first heat the heat treatment furnace to the specified temperature, and then place the workpiece to be treated in the furnace for heating.
[0043] As a preferred embodiment, in step 4, the solution treatment is performed by water cooling, and the artificial aging is performed by furnace cooling.
[0044] In order to effectively solve the problem of uneven aggregation of reinforcement phase particles inside the material, in step one, the rotation speed of the stirring head is 600-1000r / min, the welding speed is 100-300mm / min, and the downward pressure is 0.2mm.
[0045] In order to obtain high-quality welding joints, in step one, before clamping, first use a stainless steel brush to manually clean the 10 mm surface on both sides of the front and back of the welding head, then use acetone or ethanol to scrub the surface of the welding head, and then perform the clamping operation.
[0046] In order to obtain a welding joint with better performance, in step one, the starting end and the tail end of the obtained welding joint are removed, and the middle stably formed joint part is retained.
[0047] The present invention will be further described with reference to comparative examples and embodiments:
[0048] Comparative Example 1:
[0049] Use a stainless steel brush to manually clean the 10 mm surface on both sides of the front and back of the welding joint, then scrub the surface of the welding joint with acetone or ethanol, and then clamp the two plates to be welded on the machine tool of the friction stir welding machine.
[0050] A gantry-type friction stir welding machine was used to perform friction stir welding with welding parameters of a stirring head speed of 600-1000 r / min, a welding speed of 100-300 mm / min, and a downward pressure of 0.2 mm to obtain high-quality welded joints.
[0051] A 40×10 mm microhardness specimen was cut perpendicular to the weld direction from the weld joint in this comparative example, and after mounting, grinding and polishing, a Vickers hardness tester (HVS-1000 digital microhardness tester) was used to perform microhardness testing. The lateral spacing was set to 0.5 mm, the test pressure was 500 g, and the dwell time was 15 s. The test points were arranged symmetrically on both sides with the weld as the center, such as Figure 3 The Vickers hardness test method is carried out in accordance with GB / T4340.1-2009 "Metal Vickers hardness test Part 1: Test method".
[0052] The hardness distribution diagram of the welded joint obtained by the test is shown in Figure 4 As shown. The microhardness distribution of the cross section of the welded joint shows a double "W-type" distribution feature. There are two low-hardness zones in the heat-affected zone on the advancing side and the retreating side, and the hardness of the stirred zone is lower than that of the base material. The low-hardness zone of the welded joint is mainly caused by the coarsening of the precipitate phase during the welding thermal cycle. In addition, the two sides of the double "W-type" are not strictly symmetrically distributed. This is because the heat generation on both sides of the welded joint during the stir friction welding process is not exactly the same, resulting in different welding thermal cycles experienced by both sides of the welded joint.
[0053] According to GB / T13298-2015 "Methods for Metal Microstructure Inspection", the metallographic structure of the joint metallographic specimen was inspected, and Keller reagent (2.5ml HNO3+1.5ml HCl+1.0ml HF+95ml H2O) was used for corrosion, and the corrosion time was set to 20s. After corrosion treatment, the Axis Scope A1 optical microscope was used to observe the macroscopic morphology and metallographic structure of the welded joint. Figure 2 As shown in the figure, the stirring zone and heat-affected zone are darker, and the base material area is brighter. The flow behavior of the material can be clearly observed, from the inside to the outside, they are the stirring zone, heat-affected zone, and base material. The stirring zone is a typical funnel shape and has obvious onion ring structure characteristics.
[0054] According to the national standard of metal tensile test GB / T 228.1-2010 "Metallic material tensile test part 1: Room temperature test method", the tensile specimen is cut perpendicular to the weld direction. The size of the tensile specimen is as follows: Figure 5 The tensile properties of the welded joint are shown in Figure 6 As shown, the maximum tensile strength is 412.94 MPa, the maximum yield strength is 289.91 MPa, and the elongation is 4.89%.
[0055] Embodiment 2:
[0056] Use a stainless steel brush to manually clean the 10 mm surface on both sides of the front and back of the welding joint, then scrub the surface of the welding joint with acetone or ethanol, and then clamp the two plates to be welded on the machine tool of the friction stir welding machine.
[0057] A gantry-type friction stir welding machine was used to perform friction stir welding with a stirring head speed of 600-1000 r / min, a welding speed of 100-300 mm / min, and a downward pressure of 0.2 mm to obtain high-quality welded joints.
[0058] Use a wire cutting machine to remove the start and end of the welding joint, leaving the middle part of the stable joint. Then use acetone or alcohol to carefully clean and remove oil stains.
[0059] The welding joint is rolled by cold rolling equipment, the rolling deformation direction is perpendicular to the weld direction, the roller speed is 8-10r / min, and the deformation of the welding joint reaches 15-35% through two cold rolling processes.
[0060] Because cold rolling introduces excessive deformation and residual stress, the weld joint after rolling is flattened using a plate press and subjected to stress relief treatment at a temperature of 150°C for 24 hours to reduce residual deformation and lower or eliminate residual stress.
[0061] The welded joints that have been cold rolled and stress relief annealed are subjected to solution aging heat treatment: first, the solution is treated at a solution temperature of 485-510°C and a solution time of 0.8-1.2h, then cooled, and finally artificially aged at an aging temperature of 170-195°C and a time of 8-12h. The solution treatment is water-cooled, and the artificial aging is furnace-cooled. The heating rate of the solution treatment is 10°C / min, and the heating rate of the artificial aging is 5°C / min.
[0062] A 40×10 mm microhardness specimen was cut perpendicular to the weld direction from the joint after "cold rolling + heat treatment" in this embodiment, and after mounting, grinding and polishing, a Vickers hardness tester (HVS-1000 digital microhardness tester) was used for hardness testing. The lateral spacing was set to 0.5 mm, the test pressure was 500 g, and the dwell time was 15 s. The test points were arranged symmetrically on both sides with the weld as the center, such as Figure 3 The Vickers hardness test method is carried out in accordance with GB / T4340.1-2009 "Metal Vickers hardness test Part 1: Test method".
[0063] The hardness distribution diagram of the welded joint obtained by the test is shown in Figure 4After "cold rolling + heat treatment", compared with the welded state, the microhardness distribution on the cross section of the welded joint tends to be uniform, and the hardness of the heat affected zone, stirring zone, and base material zone tends to be consistent.
[0064] According to GB / T13298-2015 "Methods for Metal Microstructure Inspection", the metallographic structure of the joint metallographic specimen was inspected, and Keller reagent (2.5ml HNO3+1.5ml HCl+1.0ml HF+95ml H2O) was used for corrosion, and the corrosion time was set to 20s. After corrosion treatment, the Axis Scope A1 optical microscope was used to observe the macroscopic morphology and metallographic structure of the welded joint. Figure 2 As shown in the figure, compared with the welded state, the thickness of the welded joint is significantly thinner, eliminating the problem of thinning in the weld zone of the stir friction welding. In addition, the microstructure of each area of the welded joint has obvious changes, the interface between the weld core zone, the heat affected zone and the parent metal zone is significantly weakened, and the structure of the welded joint tends to be uniform, which is the result of the organizational transformation of the welded joint under the action of thermal-mechanical coupling.
[0065] According to the national standard of metal tensile test GB / T 228.1-2010 "Metallic material tensile test part 1: Room temperature test method", the tensile specimen is cut perpendicular to the weld direction. The size of the tensile specimen is as follows: Figure 5 As shown in Figure 2, after “cold rolling + heat treatment”, the tensile properties of the welded joint are as follows: Figure 6 As shown, the maximum tensile strength is 395.01MPa and the maximum yield strength is 250.05MPa, which is slightly lower than that of the welded state. However, its elongation is as high as 15.83%, which is more than 3 times that of the welded state (4.89%), exceeding the parent material level.
[0066] The present invention discloses a method for strengthening and plasticizing a welded joint based on thermomechanical coupling regulation for friction stir welding of in-situ self-generated TiB2 / 2024 aluminum-based composite materials. Since the in-situ self-generated TiB2 / 2024 aluminum-based composite material will have a significant problem of weld thinning after friction stir welding, and a recrystallization process will occur, direct heat treatment after welding may cause abnormal grain growth in the weld area. After cold rolling, the problem of weld thinning can be effectively solved, and the work hardening effect can be introduced, thereby significantly improving the tensile strength and yield strength of the welded joint, but the elongation of the joint is significantly reduced. Therefore, the present invention can fully improve the geometric inhomogeneity of the welded joint thickness by performing two cold rolling processes on the welded joint, and the strength of the corresponding welded joint can be significantly improved. In order to reduce the residual stress and residual deformation caused by cold rolling, the welded joint is subjected to stress relief annealing after cold rolling. In addition, in order to solve the problem of decreased elongation of the joint caused by cold rolling. The cold-rolled joint is subjected to solution aging heat treatment to eliminate the abnormal grain growth in the weld zone (stirring zone) caused by direct post-weld heat treatment, and to achieve uniform regulation of the cross-sectional structure and microhardness of the joint, thereby improving or eliminating stress / strain localization in the low hardness zone during the stretching process, thereby significantly improving the elongation of the joint.
[0067] In summary, the present invention significantly improves the comprehensive mechanical properties of the in-situ self-generated TiB2 / 2024 aluminum-based composite material stir friction welded joint, especially the plasticity (uniform deformation) of the joint, through the coupling effect of "cold rolling + heat treatment"; solves the thinning problem of the stir friction welding weld zone, optimizes the residual stress distribution of the joint, and is expected to significantly improve the fatigue performance of the joint. Specifically, by Figure 6 From the bar graph in the figure, it can be clearly seen that compared with the tensile properties of the welded joint, the welded joint obtained by the present invention has a slightly reduced strength while significantly improving the elongation of the joint. The elongation of the joint is 3 times that of the welded joint and is better than that of the original parent material.
Claims
1. A method for strengthening and plasticizing a friction stir welding joint based on thermal-mechanical coupling regulation. It is characterized in that The following steps are involved: Step 1: Friction stir welding; First, two plates to be welded are butt-jointed and clamped on a friction stir welding machine; then the stirring head is used to perform friction stir butt welding at a welding process parameter of a rotation speed of 600 to 1000 r / min and a welding speed of 100 to 300 mm / min to obtain a high-quality welded joint; Step 2: cold rolling; At room temperature, the welded joint is cold-rolled twice using a rolling mill, with the rolling direction perpendicular to the welding direction, and the total deformation is controlled within a range of 15 to 35%; Step 3: stress relief annealing treatment; The cold-rolled welded joint is flattened and then subjected to stress relief annealing at 150°C for 24 hours; Step 4: solution aging heat treatment; The welded joints after cold rolling and stress relief annealing are subjected to solution aging heat treatment: first, solution treatment is carried out at a solution temperature of 485-510°C and a solution time of 0.8-1.2h, then furnace cooling is performed, and finally, artificial aging treatment is carried out at an aging temperature of 170-195°C and an aging time of 8-12h.
2. According to the method for strengthening and plasticizing a friction stir welding joint based on thermal coupling control according to claim 1, It is characterized in that In step 1, the plate to be welded is in-situ self-generated TiB 2 / The plate is made of 2024 aluminum-based composite material and has a thickness of 2mm.
3. According to the method for strengthening and plasticizing a friction stir welding joint based on thermal coupling control according to claim 1, It is characterized in that In step 2, during the rolling process of the welded joint, the diameter of the roller is 220 mm, the rotation speed of the roller is 8-10 r / min, and the total deformation is controlled to be 15-35%.
4. According to the method for strengthening and plasticizing a friction stir welding joint based on thermal coupling control according to claim 1, It is characterized in that In step 4, the heating rate of the solution treatment is 10°C / min, and the heating rate of the artificial aging is 5°C / min. At the same time, both the solution treatment and artificial aging are to first heat the heat treatment furnace to a specified temperature, and then place the workpiece to be treated in the furnace for heating.
5. According to the method for strengthening and plasticizing a friction stir welding joint based on thermal coupling control according to claim 1, It is characterized in that In step 4, the solution treatment adopts water cooling, and the artificial aging adopts furnace cooling.
6. According to claim 1, a method for strengthening and plasticizing a friction stir welding joint based on thermal coupling regulation, It is characterized in that In step one, the rotation speed of the stirring head is 600-1000 r / min, the welding speed is 100-300 mm / min, and the downward pressure is 0.2 mm.
7. According to claim 1, a method for strengthening and plasticizing a friction stir welding joint based on thermal coupling regulation, It is characterized in that In step one, before clamping, first use a stainless steel brush to manually clean the 10 mm surface on both sides of the front and back of the welding head, then use acetone or ethanol to scrub the surface of the welding head, and then perform the clamping operation.
8. According to claim 1, a method for strengthening and plasticizing a friction stir welding joint based on thermal coupling regulation, It is characterized in that In step one, the starting end and the tail end of the obtained welding joint are removed, and the middle stably formed joint portion is retained.
Citation Information
Cited By
High-strength welding method for friction stir welding joint of 7XXX series aluminum alloy large component
CN122274394A