Preparation method of low-temperature composite solder based on pressure infiltration and prepared composite solder

By attaching flux to the surface of the alloy frame and forming a high vacuum environment in the limiting plate cavity, the solder can quickly fill the alloy frame, solving the problems of low processing efficiency and poor welding properties in the prior art, and achieving efficient preparation of composite solder sheets. Improves welding quality and production efficiency.

CN118905500APending Publication Date: 2024-11-08CHINA ELECTRONIC TECH GRP CORP NO 38 RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411023746.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing methods for preparing composite special-shaped solder with enhanced through-hole alloy frame structures have problems such as low processing efficiency, solder oxidation failure, poor welding properties, and difficulty in preparing large-area welding sheets.

Method used

By uniformly adhering flux on the surface of the alloy frame and forming a high vacuum environment by adjusting the gap and vacuum pumping in the limiting plate cavity, the solder can quickly fill the alloy frame, and the preparation of composite solder sheet is realized.

Benefits of technology

The filling rate and surface flatness of the solder are improved, the residual hollows and inclusions in the solder are avoided, the welding bonding rate is improved, and the preparation of large-area welding sheets is realized, which is characterized by simple and efficient production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905500A_ABST
    Figure CN118905500A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-temperature composite solder based on pressure infiltration and the prepared composite solder, and belongs to the technical field of welding materials. The preparation method comprises the following steps that a layer of scaling powder is evenly attached to the surface of a cleaned alloy framework; the alloy framework is placed in the cavities of the limiting plates, and the thickness of the welding flux is controlled by adjusting the gap between the limiting plates; the cavity containing the alloy framework is vacuumized, then inert gas is introduced, the cavity and the alloy framework are preheated to a certain temperature, and a high-vacuum negative-pressure environment is formed in the cavity in the circulating air exhaust and deflation process; and a valve of the tin dissolving groove is opened, the gaps between the limiting plates are rapidly filled with the welding flux, the framework is filled and wrapped with the welding flux alloy, and then the welding flux alloy is obtained. By means of the pressure infiltration mode, the filling rate of the solder can be increased, the loss of the solder alloy can be reduced, oxidation of the surface of the solder alloy is avoided, and preparation of the large-area solder piece with the controllable thickness can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of welding materials, and in particular relates to a method for preparing a low-temperature composite solder based on pressure infiltration and the prepared composite solder. Background Art

[0002] As the integration of devices increases, due to the long-term service under high frequency and high current density, the thermal stress caused by connection defects in welding is the main cause of device failure. Especially for devices with high-density ribbed structures, there is an urgent need to seek technological breakthroughs in connection accuracy and performance. Welding precision control, high welding rate and high strength have become key factors to improve the performance of power semiconductor devices.

[0003] Introducing a skeleton reinforcement phase into the solder is one of the effective methods to solve the above problems. The Chinese patent application document with publication number CN112091474A discloses a method for preparing a Ni alloy foam-reinforced Sn-based composite solder. The method uses an electroplating method to deposit Sn-based solder on the surface of the metal foam structure, and then remelts the Sn solder by electromagnetic induction heating and rolls it into foil. However, the solder sheet prepared by this process is severely oxidized, and the high-density foam skeleton has a low penetration rate of Sn, and gaps and inclusion defects are easily retained in the solder, which ultimately affects the solder penetration rate of the solder joint. The Chinese patent application document with publication number CN116493804A discloses a metal grid-reinforced composite material and a manufacturing method thereof. The method uses a copper grid as a through-hole intercalation material to prepare a composite solder with a high penetration rate. The preparation process requires two solder sheets to be covered on the upper and lower surfaces of the copper grid to form a sandwich structure, but this needs to be rolled multiple times, and the horizontal and vertical wires are offset during the rolling process. The three-dimensional size of the solder cannot be guaranteed, and it is difficult to prepare a large-area solder sheet. Therefore, further improvement is needed. Summary of the invention

[0004] The technical problem to be solved by the present invention is how to solve the problems faced by the existing method for preparing composite special-shaped through-hole alloy skeleton structure reinforced solder, such as low processing efficiency, solder oxidation failure, poor weldability, and difficulty in preparing large-area solder sheets.

[0005] The present invention solves the above technical problems through the following technical means:

[0006] A first aspect of the present invention provides a method for preparing a composite solder sheet, comprising the following steps:

[0007] (1) A layer of flux is evenly attached to the surface of the cleaned alloy skeleton;

[0008] (2) placing the alloy skeleton into the cavity of the limiting plate, and controlling the solder thickness by adjusting the gap between the limiting plates;

[0009] (3) After the cavity containing the alloy skeleton is evacuated, an inert gas is introduced, and the evacuation and degassing process is circulated to preheat the cavity and the alloy skeleton to a certain temperature, and the evacuation and degassing process is circulated again to form a high vacuum negative pressure environment in the cavity;

[0010] (4) Open the valve of the tin dissolving bath to allow the solder to quickly fill the gap between the limiting plates, thereby achieving the filling and coating of the skeleton with the solder alloy, and finally remove the excess inclusions and residues at the riser to obtain a flat and integrated composite solder sheet.

[0011] Preferably, in step (1), the alloy skeleton is at least one of a two-dimensional alloy mesh and an alloy foam.

[0012] Preferably, in step (1), the matrix of the alloy skeleton is at least one of Ni, Cu, Fe, Cr, and Ti.

[0013] Preferably, in step (1), the solder flux is attached to the surface of the alloy skeleton by at least one of spraying, coating, and immersion treatment.

[0014] Preferably, in step (2), the limiting plate is at least one of a stainless steel plate, a titanium alloy plate, and a chrome-plated stainless steel plate.

[0015] Preferably, in step (2), the cavity between the limiting plates is a closed space, and the cavity space is larger than the entire alloy mesh or alloy foam.

[0016] Preferably, in step (3), the preheating temperature is between 60-200° C. (to activate the flux, increase the fluidity of the filling solder, and improve the filling rate.)

[0017] Preferably, in step (3), the preheating method is one of the heating methods such as ceramic heating plate heating, light wave tube heating, infrared radiation heating and induction heating.

[0018] Preferably, in step (3), the time for each inert gas introduction is 3-10 min, and each cycle of pumping and degassing is performed 1-5 times, and the final vacuum degree of the cavity exceeds 1×10 -1 MPa.

[0019] Preferably, in step (4), the solder is at least one of a Sn-based alloy and an In-based alloy.

[0020] A second aspect of the present invention provides a composite solder sheet obtained by the above preparation method.

[0021] The third aspect of the present invention proposes the application of the composite solder sheet in the welding of semiconductor devices, for example: packaging of power chips, precision connection of optoelectronic devices, etc.

[0022] The beneficial effects of the present invention are:

[0023] (1) Negative pressure infiltration can greatly improve the solder filling rate and surface flatness, while avoiding the residual voids and inclusions inside the solder sheet.

[0024] (2) The solder is injected into the mold cavity through valve control to quickly fill the alloy skeleton, reduce excessive loss and contamination of the solder, and make full use of the solder.

[0025] (3) By adjusting the template gap, the mass percentage of solder and alloy skeleton, the thickness of solder piece and other factors can be flexibly changed to achieve solder customization for special use scenarios.

[0026] (4) The composite solder sheet is processed and formed in a high vacuum environment to avoid the oxidation failure of the solder and effectively improve the welding rate.

[0027] (5) The product of the present invention can realize the preparation of large-area welding sheets and has the characteristics of simple and efficient production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of a method for preparing a composite solder sheet of the present invention;

[0029] Figure 2 The micrograph and element line scanning result graph of the cross section of the integral nickel-copper alloy mesh prepared in Example 1 of the present invention;

[0030] Figure 3 is a cross-sectional micrograph of the composite solder sheet prepared in Example 1 of the present invention;

[0031] Figure 4 is a cross-sectional micrograph of the composite solder sheet prepared in Example 2 of the present invention;

[0032] Figure 5 This is a comparison chart of the average tensile strength of the composite solder sheets prepared in Examples 1-3 of the present invention;

[0033] Figure 6 This is a comparison chart of the average soldering rates of the composite solder sheets prepared in Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0036] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0037] Embodiment 1:

[0038] A method for preparing a composite solder sheet, comprising the following steps:

[0039] In this example, a two-dimensional alloy mesh with a composition of Ni-20Cu (at.%) is selected as the alloy skeleton. Figure 2 As shown), the solder is SAC305 alloy solder, and the specific preparation steps are as follows:

[0040] (1) The surface of a 90 μm thick Ni-20Cu two-dimensional alloy mesh was sprayed with RF active flux;

[0041] (2) Adjust the upper and lower gaps of the stainless steel limit plate cavity to 110 μm, and then place the alloy mesh between the two stainless steel limit plate cavities;

[0042] (3) The stainless steel cavity is first evacuated with a vacuum pump, and then argon gas is introduced into the stainless steel cavity for 5 minutes. The argon valve is closed and the evacuation is continued. This process is repeated three times. The cavity and the alloy mesh are then preheated to 150°C using a ceramic heating plate to activate the flux, increase the fluidity of the filling solder, and improve the filling rate. The evacuation and degassing process is repeated again to make the vacuum degree of the mold cavity exceed 1×10 -1 MPa, forming a high vacuum negative pressure environment;

[0043] (4) Then, the valve of the tin dissolving tank is opened to allow the molten SAC305 alloy solder to quickly fill the gaps between the stainless steel cavities at a rate of 0.2 kg / s. After 5 minutes of infiltration, the solder fills and covers the alloy mesh. Finally, the excess inclusions and residues at the riser are removed to obtain a composite solder sheet with a smooth surface (such as Figure 3 shown).

[0044] The Ni-20Cu alloy mesh warp and weft wires are fully integrated with the SAC305 solder. The tensile strength test results of the Ni-20Cu / SAC305 composite solder sheet prepared in this embodiment are as follows: Figure 5 As shown, the tensile strength can reach 82.14MPa, which is 82.53% higher than that of traditional pure SAC305 solder sheet.

[0045] When the Ni-20Cu / SAC305 composite solder sheet prepared in this embodiment is used in the packaging of power chips and the precision connection of optoelectronic devices, it can effectively prevent overflow and avoid the generation of voids. The sample welding rate is calculated by taking the average value of three samples under the same welding parameters, such as Figure 6 As shown, the upper part of the picture is the original picture of the ultrasonic scanning test result, and the lower part is the test result figure calculated by the image processing software ImageJ. After ultrasonic scanning (C-SAM) test analysis, it can be known that the welding rate of the prepared samples can reach 95%.

[0046] Embodiment 2:

[0047] A method for preparing a composite solder sheet, comprising the following steps:

[0048] In this example, a two-dimensional alloy mesh with a composition of Ni-20Cu (at.%) is selected as the alloy skeleton, and the solder is Sn-37Pb alloy solder. The specific preparation steps are as follows:

[0049] (1) The surface of a 90 μm thick Ni-20Cu alloy mesh was coated with RF active flux;

[0050] (2) The upper and lower gaps of the titanium alloy limiting plate cavity are adjusted to 100 μm; then the alloy mesh is placed between the two titanium alloy limiting plate cavities;

[0051] (3) The titanium alloy cavity was first evacuated using a vacuum pump, and then argon was introduced into the titanium alloy cavity for 3 min. The argon valve was closed and the evacuation was continued. This process was repeated five times. The cavity and the alloy mesh were then preheated to 60 °C using a light wave tube to activate the flux, increase the fluidity of the filling solder, and improve the filling rate. The evacuation and degassing process was repeated again to make the vacuum degree of the mold cavity exceed 1×10 -1 MPa, forming a high vacuum negative pressure environment;

[0052] (4) Then, the valve of the tin bath was opened to allow the molten Sn-37Pb alloy solder to quickly fill the gaps between the titanium alloy cavities at a rate of 0.2 kg / s. After 5 minutes of infiltration, the solder alloy filled and coated the alloy mesh. Finally, the excess inclusions and residues at the riser were removed to obtain a composite solder sheet with a smooth surface (such as Figure 4 shown).

[0053] The warp and weft wires of the Ni-20Cu alloy mesh and the Sn-37Pb solder are fully integrated. The tensile strength test results of the Ni-20Cu / Sn-37Pb composite solder sheet prepared in this embodiment are as follows: Figure 5 As shown, the tensile strength can reach 68.9MPa, which is 64.1% higher than that of traditional pure Sn-37Pb solder sheets.

[0054] When the Ni-20Cu / Sn-37Pb composite solder sheet prepared in this embodiment is used in the packaging of power chips and the precision connection of optoelectronic devices, it can effectively prevent overflow and avoid the generation of voids. After ultrasonic scanning (C-SAM) test analysis, it can be seen that the welding rate of the prepared samples can reach 95%.

[0055] Embodiment 3:

[0056] A method for preparing a composite solder sheet, comprising the following steps:

[0057] In this example, a two-dimensional alloy mesh with a composition of Ni-20Cu (at.%) is selected as the alloy skeleton, and the solder is SAC305 alloy solder. The specific preparation steps are as follows:

[0058] (1) The surface of a 200 μm thick Ni-20Cu alloy mesh was immersed in RF active flux;

[0059] (2) The upper and lower gaps of the stainless steel cavity were adjusted to 220 μm, and then the alloy mesh was placed between the two stainless steel cavities;

[0060] (3) The stainless steel cavity was evacuated for the first time using a vacuum pump, and then argon was introduced into the stainless steel cavity for 10 min. The argon valve was closed and the evacuation was continued. This process was repeated twice. The cavity and the alloy mesh were then preheated to 220 °C using infrared radiation heating to activate the flux, increase the fluidity of the filling solder, and improve the filling rate. The evacuation and degassing process was repeated again to make the vacuum degree of the mold cavity exceed 1×10 -1 MPa, forming a high vacuum negative pressure environment;

[0061] (4) Then, the valve of the tin bath was opened to allow the molten SAC305 alloy solder to quickly fill the gaps between the stainless steel cavities at a rate of 0.2 kg / s. After 5 minutes of infiltration, the solder alloy filled and coated the alloy mesh. Finally, the excess inclusion residues at the riser were removed to obtain a composite solder with a smooth and integrated surface.

[0062] The Ni-20Cu alloy mesh warp and weft wires are fully integrated with the SAC305 solder. The tensile strength test results of the Ni-20Cu / SAC305 composite solder sheet prepared in this embodiment are as follows: Figure 5 As shown, the tensile strength can reach 64.98MPa, which is 44.4% higher than that of traditional pure SAC305 solder sheet.

[0063] When the Ni-20Cu / SAC305 composite solder sheet prepared in this embodiment is used in the packaging of power chips and the precision connection of optoelectronic devices, it can effectively prevent overflow and avoid the generation of voids. According to ultrasonic scanning (C-SAM) test analysis, the welding rate of the prepared samples can reach 91%.

[0064] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a composite solder sheet, characterized in that: The steps include: (1) A layer of flux is evenly attached to the surface of the cleaned alloy skeleton; (2) placing the alloy skeleton into the cavity of the limiting plate, and controlling the solder thickness by adjusting the gap between the limiting plates; (3) After the cavity containing the alloy skeleton is evacuated, an inert gas is introduced, and the evacuation and degassing process is circulated to preheat the cavity and the alloy skeleton to a certain temperature, and the evacuation and degassing process is circulated again to form a high vacuum negative pressure environment in the cavity; (4) Open the valve of the tin dissolving bath to allow the solder to quickly fill the gap between the limiting plates, thereby achieving the filling and coating of the skeleton with the solder alloy, and finally remove the excess inclusions and residues at the riser to obtain a flat and integrated composite solder sheet.

2. The method for preparing the composite solder sheet according to claim 1, characterized in that: In step (1), the alloy skeleton is at least one of a two-dimensional alloy mesh and an alloy foam.

3. The method for preparing the composite solder sheet according to claim 1, characterized in that: In step (1), the matrix of the alloy skeleton is at least one of Ni, Cu, Fe, Cr, and Ti.

4. The method for preparing the composite solder sheet according to claim 1, characterized in that: In step (1), the soldering flux is attached to the surface of the alloy skeleton by at least one of spraying, coating, and immersion treatment.

5. The method for preparing the composite solder sheet according to claim 1, characterized in that: In step (2), the limiting plate is at least one of a stainless steel plate, a titanium alloy plate, and a chrome-plated stainless steel plate.

6. The method for preparing a composite solder sheet according to claim 1, characterized in that: In step (3), the preheating temperature is between 60-200° C.; the preheating method is one of the heating methods such as ceramic heating plate heating, light wave tube heating, infrared radiation heating and induction heating.

7. The method for preparing a composite solder sheet according to claim 1, characterized in that: In step (3), the time for each inert gas introduction is 3-10 min, and each cycle of pumping and degassing is performed 1-5 times, and the final vacuum degree of the cavity exceeds 1×10 -1 MPa.

8. The method for preparing a composite solder sheet according to claim 1, characterized in that: In step (4), the solder is at least one of a Sn-based alloy and an In-based alloy.

9. The composite solder sheet obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the composite solder sheet according to claim 9 in semiconductor device welding.