Preparation process and method of solder wire for circuit board
By adding antibacterial agents and other modifiers to the solder wire preparation process, the problems of bacterial reproduction and oxide layer formation in the solder wire during the welding process are solved, the solder quality and service life are improved, and the efficient performance and stability of the solder wire are achieved. sex.
Patent Information
- Application Number
- CN202411228690.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-08
AI Technical Summary
In traditional solder wire preparation technology, solder wire may come into contact with bacteria during the welding process, resulting in bacterial reproduction and oxide layer formation, affecting the welding quality and service life.
Using a preparation process of solder wire for circuit boards, by accurately weighing elements such as tin, lead, silver, and copper, and adding antioxidants, antibacterial agents, hardness enhancers, fluidity improvers, flame retardants, and viscosity regulators. and conductivity enhancers to ensure uniform melting of the alloy and avoid oxidation during cooling, and use antibacterial agents to inhibit bacterial growth.
Effectively inhibit bacterial growth, extend the service life of solder wire, improve welding quality and performance, reduce environmental pollution, and ensure the stability and reliability of the welding process.
Smart Images

Figure CN118905501A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solder wire preparation, and specifically relates to a preparation process and method of solder wire for a circuit board. Background Art
[0002] Solder wire for circuit boards is an indispensable material in the electronic assembly process and is mainly used for component welding on circuit boards. It is made of tin-based alloy and has good conductivity, wettability and fluidity, ensuring welding quality and efficiency. The main component of solder wire for circuit boards is tin, and elements such as lead, silver and copper are usually added to improve welding performance. The specifications of solder wire for circuit boards are diverse, with diameters of 0.2mm, 0.3mm, 0.5mm and other types, which can be selected according to welding process and component requirements. Solder wire is widely used in the field of electronic assembly, mainly including: Circuit board welding: used for welding between electronic components and circuit boards. Electronic equipment repair: During the repair of electronic equipment, solder wire is used to replace damaged components. Product research and development: During the product prototyping and debugging stages, solder wire is used to build and modify circuits. In short, solder wire for circuit boards plays an important role in the electronics industry. With the continuous development of electronic technology, the performance and quality of solder wire will continue to improve to meet increasingly stringent welding requirements.
[0003] However, in traditional solder wire preparation technology, the solder wire may come into contact with bacteria during the welding process. In a humid environment, this may cause bacteria to multiply on the surface of the solder wire, thus affecting the welding quality and service life. At the same time, alloy elements are easily oxidized during the melting process, resulting in the formation of an oxide layer on the surface of the solder wire, thus affecting the welding performance. Summary of the invention
[0004] The purpose of the present invention is to provide a process and method for preparing solder wire for circuit boards in order to solve the above-mentioned problems.
[0005] The technical solution adopted by the present invention is as follows: a preparation process and method of solder wire for circuit boards, the method comprising the following steps:
[0006] S1: First weigh the raw materials:
[0007] 500-550 parts by weight of pure tin.
[0008] 300-350 parts by weight of lead.
[0009] 20 to 30 parts by weight of silver.
[0010] 10 to 20 parts by weight of copper.
[0011] 5 to 10 parts by weight of gallium;
[0012] 15 to 20 parts by weight of antioxidant.
[0013] 5 to 10 parts by weight of antibacterial agent.
[0014] 10 to 14 parts by weight of hardness enhancer.
[0015] 5 to 8 parts by weight of fluidity improver.
[0016] 10 to 15 parts by weight of flame retardant.
[0017] 5 to 7 parts by weight of viscosity modifier.
[0018] 5 to 8 parts by weight of conductivity enhancer.
[0019] S2: Place the accurately weighed tin, lead, silver, copper and gallium elements into the preheated tin melting furnace in accordance with the formula ratio. Make sure the tin melting furnace is clean and dry to avoid contamination and oxidation;
[0020] S3: Start the heating system of the tin melting furnace and gradually raise the temperature to the predetermined melting point of the alloy. The melting point of tin-lead-silver-copper alloy is between 183°C and 190°C. Keep the temperature stable until all alloy elements are completely melted. Use a stirring rod to gently stir to ensure that the alloy components in the molten pool are evenly distributed;
[0021] S4: After the alloy elements are completely melted and stirred evenly, antioxidants, antibacterial agents, hardness enhancers, fluidity improvers, flame retardants, viscosity modifiers and conductivity enhancers are added in sequence. Each additive must be accurately weighed according to the formula ratio and slowly added to the molten alloy;
[0022] S5: Continue to stir thoroughly with the stirring rod to ensure that all additives are completely mixed with the alloy matrix without precipitation and agglomeration;
[0023] S6: Slowly pour the evenly stirred alloy solution into the pre-prepared solder wire mold. Avoid bubbles and splashes during the operation to ensure that the alloy solution fills the mold smoothly;
[0024] S7: Allow the alloy to cool naturally to room temperature in the mold to solidify the formed solder wire. The cooling process is carried out in a dust-free, dry and temperature-stable environment to prevent oxidation on the solder wire surface;
[0025] S8: Take the cooled solder wire out of the die and install it on the wire drawing machine. Adjust the wire drawing machine to the required solder wire diameter and start the wire drawing machine for drawing. After drawing, use a precise cutting tool to cut the solder wire into the specified length.
[0026] S9: The stretched and cut solder wire is packaged in moisture-proof and oxidation-proof packaging to ensure that the solder wire is not affected by the external environment during storage and transportation. After the packaging is completed, the preparation process of the solder wire for the entire circuit board is completed.
[0027] In a preferred embodiment, in step S1, the antioxidant is one or more of rosin, succinic acid, methyl chloride, zinc chloride, antioxidant oil or phosphate.
[0028] In a preferred embodiment, in step S1, the hardness enhancer is one or more of antimony, bismuth, tellurium or tungsten.
[0029] In a preferred embodiment, in step S1, the fluidity improver is one or more of gallium, indium, tin or lead.
[0030] In a preferred embodiment, in step S1, the flame retardant is one or more of aluminum hydroxide, phosphate, and zinc borate.
[0031] In a preferred embodiment, in step S1, the viscosity modifier is one or more of silicone oil, polyethylene glycol, fatty acid or wax.
[0032] In a preferred embodiment, in step S1, the conductivity enhancer is one or more of nickel, silver, copper or gold.
[0033] In a preferred embodiment, in step S1, the antibacterial agent comprises: 1-2 parts by weight of silver nanoparticles, 1-3 parts by weight of chitosan, 0.5-1 parts by weight of titanium dioxide nanoparticles and 0.5-1 parts by weight of polyaminopropyltriethoxysilane;
[0034] The preparation method comprises:
[0035] Step 1: Synthesize silver nanoparticles and prepare silver nitrate solution: dissolve an appropriate amount of silver nitrate in deionized water. Add reducing agent glucose or ascorbic acid to the silver nitrate solution and heat to 80-90°C under stirring to perform a reduction reaction to generate silver nanoparticles.
[0036] Step 2: Prepare chitosan solution, dissolve chitosan in dilute acetic acid solution, stir until completely dissolved, and dilute the chitosan solution to the desired concentration.
[0037] Step 3: Prepare a titanium dioxide nanoparticle suspension by dispersing the titanium dioxide nanoparticles in deionized water and using an ultrasonic disperser to ensure uniform dispersion.
[0038] Step 4: Mix the antibacterial ingredients, add the synthesized silver nanoparticles to the chitosan solution, stir evenly, add the titanium dioxide nanoparticle suspension to the above mixture, continue stirring, add the coupling agent: finally add polyaminopropyl triethoxysilane, stir evenly to form a stable antibacterial agent mixture.
[0039] Step 5: Stabilization of the antimicrobial agent, cross-linking reaction: Under mild heating conditions, chitosan and polyaminopropyltriethoxysilane are cross-linked to enhance the stability of the antimicrobial agent. The mixture is cooled to room temperature and stored under sterile conditions to obtain the antimicrobial agent.
[0040] In a preferred embodiment, in step S3, the preheating temperature of the tin melting furnace is: before adding the alloy elements, the tin melting furnace is preheated to 100-150°C.
[0041] Melting Temperature: The melting point of tin-lead-silver-copper alloy ranges between 183°C and 190°C.
[0042] Melting time: The time required for the alloy elements to completely melt is 10-30 minutes;
[0043] The heating rate was controlled at 5-10°C / min.
[0044] Stirring speed: When using a stirring rod, stir gently at a speed of 30-60 revolutions per minute to ensure that the alloy components are evenly distributed while avoiding excessive bubbles.
[0045] In a preferred embodiment, in step S4, after each additive is added, stirring is continued for 3 to 5 minutes to ensure that the additive is completely dispersed and evenly mixed.
[0046] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0047] 1. In the present invention, the solder wire may come into contact with bacteria during the welding process, especially in a humid environment. The antibacterial agent can effectively inhibit the growth of bacteria and reduce the reproduction of bacteria on the surface of the solder wire, thereby maintaining the cleanliness of the solder wire and the welding quality. By inhibiting the growth of bacteria, the antibacterial agent can extend the service life of the solder wire, reduce the corrosion and oxidation caused by bacteria, thereby improving the overall performance and service life of the solder wire. The antibacterial agent can prevent the influence of bacteria on the performance of the solder wire and ensure the stability and reliability of the welding process. By inhibiting the growth of bacteria, the antibacterial agent can reduce the corrosion and oxidation caused by bacteria, thereby reducing the pollution to the environment. In addition, the addition of the antibacterial agent helps to reduce the bacterial contamination of the solder wire during use, protecting the environment and human health. Therefore, the addition of the antibacterial agent can improve the antibacterial properties of the solder wire as a whole, inhibit bacterial growth, extend the service life, improve the welding quality, reduce environmental pollution, and is suitable for specific applications. These beneficial effects make the antibacterial agent an important part of the preparation process of the solder wire.
[0048] 2. In the present invention, by precisely controlling the ratio of alloy elements such as tin, lead, silver, copper, gallium, etc., a solder wire with specific physical and chemical properties can be prepared to meet the diverse needs of circuit board welding. The added antioxidant, hardness enhancer, fluidity improver, flame retardant, viscosity modifier and conductivity enhancer can improve the performance of the solder wire and improve the overall oxidation resistance, hardness, fluidity, flame retardancy, viscosity and conductivity of the solder wire during use. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0051] Reference Figure 1 ,
[0052] Embodiment 1:
[0053] A preparation process and method of solder wire for circuit board, the method comprising the following steps:
[0054] S1: First weigh the raw materials:
[0055] 500 parts by weight of pure tin (Sn).
[0056] 300 parts by weight of lead (Pb).
[0057] 20 parts by weight of silver (Ag).
[0058] 10 parts by weight of copper (Cu).
[0059] 5 parts by weight of gallium;
[0060] 15 parts by weight antioxidant.
[0061] 5 parts by weight of antibacterial agent.
[0062] 10 parts by weight of hardness enhancer.
[0063] 5 parts by weight of flowability improver.
[0064] 10 parts by weight of flame retardant.
[0065] 5 parts by weight of viscosity modifier.
[0066] 5 parts by weight of conductivity enhancer
[0067] S2: Place the accurately weighed tin, lead, silver, copper and gallium elements into the preheated tin melting furnace in accordance with the formula ratio. Make sure the tin melting furnace is clean and dry to avoid contamination and oxidation;
[0068] S3: Start the heating system of the tin melting furnace and gradually raise the temperature to the predetermined melting point of the alloy. The melting point of tin-lead-silver-copper alloy is approximately between 183°C and 190°C. Keep the temperature stable until all alloy elements are completely melted. Use a stirring rod to gently stir to ensure that the alloy components in the molten pool are evenly distributed;
[0069] S4: After the alloy elements are completely melted and stirred evenly, antioxidants, antibacterial agents, hardness enhancers, fluidity improvers, flame retardants, viscosity modifiers and conductivity enhancers are added in sequence. Each additive must be accurately weighed according to the formula ratio and slowly added to the molten alloy;
[0070] S5: Continue to stir thoroughly with the stirring rod to ensure that all additives are completely mixed with the alloy matrix without precipitation and agglomeration. The stirring time should be long enough to ensure that the additives are evenly distributed in the alloy;
[0071] S6: Slowly pour the evenly stirred alloy solution into the pre-prepared solder wire mold. Avoid bubbles and splashes during the operation to ensure that the alloy solution fills the mold smoothly;
[0072] S7: Allow the alloy to cool naturally to room temperature in the mold to solidify the formed solder wire. The cooling process should be carried out in a dust-free, dry and temperature-stable environment to prevent oxidation of the solder wire surface;
[0073] S8: Take the cooled solder wire out of the die and install it on the wire drawing machine. Adjust the wire drawing machine to the required solder wire diameter and start the wire drawing machine for drawing. After drawing, use a precise cutting tool to cut the solder wire into the specified length.
[0074] S9: Pack the stretched and cut solder wire in moisture-proof and oxidation-proof packaging. Use special packaging materials to ensure that the solder wire is not affected by the external environment during storage and transportation. After packaging is completed, the entire preparation process of the solder wire for the circuit board is completed.
[0075] In step S1, the antioxidant is one or more of rosin, succinic acid, methyl chloride, zinc chloride, antioxidant oil or phosphate.
[0076] In step S1, the hardness enhancer is one or more of antimony (Sb), bismuth (Bi), tellurium (Te) or tungsten (W), which can improve the hardness and mechanical strength of the solder wire, so that it can maintain better shape and strength during the welding process.
[0077] In step S1, the fluidity improver is one or more of gallium (Ga), indium (In), tin (Sn) or lead (Pb). These elements can lower the melting point of the solder and improve its fluidity, making it easier for the solder wire to wet the soldering surface during soldering.
[0078] In step S1, the flame retardant is one or more of aluminum hydroxide (Al(OH)3), phosphate, zinc borate (ZnB) or antimony oxide (Sb2O3), which can reduce the flammability of the solder wire at high temperatures and improve its flame retardant properties.
[0079] In step S1, the viscosity modifier is one or more of silicone oil, polyethylene glycol (PEG), fatty acid or wax, which can adjust the viscosity of the solder wire so that it has better fluidity and stability during the welding process.
[0080] In step S1, the conductivity enhancer is one or more of nickel (Ni), silver (Ag), copper (Cu) or gold (Au). These elements can improve the conductivity of the solder wire and are suitable for soldering electronic components that require higher conductivity.
[0081] In step S1, the antimicrobial agent includes:
[0082] 1-2 parts by weight of silver nanoparticles, 1-3 parts by weight of chitosan, 0.5-1 parts by weight of titanium dioxide nanoparticles and 0.5-1 parts by weight of polyaminopropyltriethoxysilane;
[0083] The preparation method comprises:
[0084] Step 1: Synthesize silver nanoparticles and prepare silver nitrate solution: dissolve an appropriate amount of silver nitrate in deionized water. Add reducing agent glucose or ascorbic acid to the silver nitrate solution and heat to 80-90°C under stirring to perform a reduction reaction to generate silver nanoparticles.
[0085] Step 2: Prepare chitosan solution, dissolve chitosan in dilute acetic acid solution, stir until completely dissolved, and dilute the chitosan solution to the desired concentration.
[0086] Step 3: Prepare a titanium dioxide nanoparticle suspension by dispersing the titanium dioxide nanoparticles in deionized water and using an ultrasonic disperser to ensure uniform dispersion.
[0087] Step 4: Mix the antibacterial ingredients, add the synthesized silver nanoparticles to the chitosan solution, stir evenly, add the titanium dioxide nanoparticle suspension to the above mixture, continue stirring, add the coupling agent: finally add polyaminopropyl triethoxysilane, stir evenly to form a stable antibacterial agent mixture.
[0088] Step 5: Stabilization of the antimicrobial agent, cross-linking reaction: Under mild heating conditions, chitosan and polyaminopropyltriethoxysilane are cross-linked to enhance the stability of the antimicrobial agent. The mixture is cooled to room temperature and stored under sterile conditions to obtain the antimicrobial agent.
[0089] In step S3, the tin melting furnace is preheated to a temperature of 100-150° C. before adding the alloying elements. This step helps to reduce heat loss during the melting process and prevents early oxidation of the alloying elements.
[0090] Melting temperature: The melting point range of tin-lead-silver-copper alloy should be between 183°C and 190°C. The exact melting temperature depends on the specific proportions of the elements in the alloy, and the optimal melting temperature is usually determined experimentally.
[0091] Melting time: The time required for the alloy elements to completely melt is about 10-30 minutes;
[0092] The heating rate is controlled at 5-10°C / min to avoid excessive heating resulting in uneven alloy composition or oxidation.
[0093] Stirring speed: When using a stirring rod, stir gently at a speed of 30-60 revolutions per minute to ensure that the alloy components are evenly distributed while avoiding excessive bubbles.
[0094] In step S4, after each additive is added, stirring should be continued for 3 to 5 minutes to ensure that the additive is completely dispersed and evenly mixed.
[0095] In the present invention, the solder wire may be exposed to bacteria during the welding process, especially in a humid environment. The antibacterial agent can effectively inhibit the growth of bacteria and reduce the reproduction of bacteria on the surface of the solder wire, thereby maintaining the cleanliness and welding quality of the solder wire. By inhibiting bacterial growth, the antibacterial agent can extend the service life of the solder wire, reduce corrosion and oxidation caused by bacteria, thereby improving the overall performance and service life of the solder wire. The antibacterial agent can prevent the influence of bacteria on the performance of the solder wire and ensure the stability and reliability of the welding process. By inhibiting bacterial growth, the antibacterial agent can reduce corrosion and oxidation caused by bacteria, thereby reducing pollution to the environment. In addition, the addition of the antibacterial agent helps to reduce bacterial contamination of the solder wire during use, protecting the environment and human health. Therefore, the addition of the antibacterial agent can improve the antibacterial performance of the solder wire as a whole, inhibit bacterial growth, extend the service life, improve the welding quality, reduce environmental pollution, and is suitable for specific applications. These beneficial effects make the antibacterial agent an important part of the preparation process of the solder wire.
[0096] In the present invention, by precisely controlling the ratio of alloy elements such as tin, lead, silver, copper, gallium, etc., a solder wire with specific physical and chemical properties can be prepared to meet the diverse needs of circuit board welding. The added antioxidant, hardness enhancer, fluidity improver, flame retardant, viscosity modifier and conductivity enhancer can improve the performance of the solder wire and improve the overall oxidation resistance, hardness, fluidity, flame retardancy, viscosity and conductivity of the solder wire during use.
[0097] Embodiment 2:
[0098] A preparation process and method of solder wire for circuit board, the method comprising the following steps:
[0099] S1: First weigh the raw materials:
[0100] 550 parts by weight of pure tin (Sn).
[0101] ~350 parts by weight of lead (Pb).
[0102] 30 parts by weight of silver (Ag).
[0103] 20 parts by weight of copper (Cu).
[0104] 10 parts by weight of gallium;
[0105] 20 parts by weight of antioxidant.
[0106] 10 parts by weight of antibacterial agent.
[0107] 14 parts by weight of hardness enhancer.
[0108] 8 parts by weight of flowability improver.
[0109] 15 parts by weight flame retardant.
[0110] 7 parts by weight of viscosity modifier.
[0111] 8 parts by weight of conductivity enhancer
[0112] S2: Place the accurately weighed tin, lead, silver, copper and gallium elements into the preheated tin melting furnace in accordance with the formula ratio. Make sure the tin melting furnace is clean and dry to avoid contamination and oxidation;
[0113] S3: Start the heating system of the tin melting furnace and gradually raise the temperature to the predetermined melting point of the alloy. The melting point of tin-lead-silver-copper alloy is approximately between 183°C and 190°C. Keep the temperature stable until all alloy elements are completely melted. Use a stirring rod to gently stir to ensure that the alloy components in the molten pool are evenly distributed;
[0114] S4: After the alloy elements are completely melted and stirred evenly, antioxidants, antibacterial agents, hardness enhancers, fluidity improvers, flame retardants, viscosity modifiers and conductivity enhancers are added in sequence. Each additive must be accurately weighed according to the formula ratio and slowly added to the molten alloy;
[0115] S5: Continue to stir thoroughly with the stirring rod to ensure that all additives are completely mixed with the alloy matrix without precipitation and agglomeration. The stirring time should be long enough to ensure that the additives are evenly distributed in the alloy;
[0116] S6: Slowly pour the evenly stirred alloy solution into the pre-prepared solder wire mold. Avoid bubbles and splashes during the operation to ensure that the alloy solution fills the mold smoothly;
[0117] S7: Allow the alloy to cool naturally to room temperature in the mold to solidify the formed solder wire. The cooling process should be carried out in a dust-free, dry and temperature-stable environment to prevent oxidation of the solder wire surface;
[0118] S8: Take the cooled solder wire out of the die and install it on the wire drawing machine. Adjust the wire drawing machine to the required solder wire diameter and start the wire drawing machine for drawing. After drawing, use a precise cutting tool to cut the solder wire into the specified length.
[0119] S9: Pack the stretched and cut solder wire in moisture-proof and oxidation-proof packaging. Use special packaging materials to ensure that the solder wire is not affected by the external environment during storage and transportation. After packaging is completed, the entire preparation process of the solder wire for the circuit board is completed.
[0120] In step S1, the antioxidant is one or more of rosin, succinic acid, methyl chloride, zinc chloride, antioxidant oil or phosphate.
[0121] In step S1, the hardness enhancer is one or more of antimony (Sb), bismuth (Bi), tellurium (Te) or tungsten (W), which can improve the hardness and mechanical strength of the solder wire, so that it can maintain better shape and strength during the welding process.
[0122] In step S1, the fluidity improver is one or more of gallium (Ga), indium (In), tin (Sn) or lead (Pb). These elements can lower the melting point of the solder and improve its fluidity, making it easier for the solder wire to wet the soldering surface during soldering.
[0123] In step S1, the flame retardant is one or more of aluminum hydroxide (Al(OH)3), phosphate, zinc borate (ZnB) or antimony oxide (Sb2O3), which can reduce the flammability of the solder wire at high temperatures and improve its flame retardant properties.
[0124] In step S1, the viscosity modifier is one or more of silicone oil, polyethylene glycol (PEG), fatty acid or wax, which can adjust the viscosity of the solder wire so that it has better fluidity and stability during the welding process.
[0125] In step S1, the conductivity enhancer is one or more of nickel (Ni), silver (Ag), copper (Cu) or gold (Au). These elements can improve the conductivity of the solder wire and are suitable for soldering electronic components that require higher conductivity.
[0126] In step S1, the antimicrobial agent includes:
[0127] 1-2 parts by weight of silver nanoparticles, 1-3 parts by weight of chitosan, 0.5-1 parts by weight of titanium dioxide nanoparticles and 0.5-1 parts by weight of polyaminopropyltriethoxysilane;
[0128] The preparation method comprises:
[0129] Step 1: Synthesize silver nanoparticles and prepare silver nitrate solution: dissolve an appropriate amount of silver nitrate in deionized water. Add reducing agent glucose or ascorbic acid to the silver nitrate solution and heat to 80-90°C under stirring to perform a reduction reaction to generate silver nanoparticles.
[0130] Step 2: Prepare chitosan solution, dissolve chitosan in dilute acetic acid solution, stir until completely dissolved, and dilute the chitosan solution to the desired concentration.
[0131] Step 3: Prepare a titanium dioxide nanoparticle suspension by dispersing the titanium dioxide nanoparticles in deionized water and using an ultrasonic disperser to ensure uniform dispersion.
[0132] Step 4: Mix the antibacterial ingredients, add the synthesized silver nanoparticles to the chitosan solution, stir evenly, add the titanium dioxide nanoparticle suspension to the above mixture, continue stirring, add the coupling agent: finally add polyaminopropyl triethoxysilane, stir evenly to form a stable antibacterial agent mixture.
[0133] Step 5: Stabilization of the antimicrobial agent, cross-linking reaction: Under mild heating conditions, chitosan and polyaminopropyltriethoxysilane are cross-linked to enhance the stability of the antimicrobial agent. The mixture is cooled to room temperature and stored under sterile conditions to obtain the antimicrobial agent.
[0134] In step S3, the tin melting furnace is preheated to a temperature of 100-150° C. before adding the alloying elements. This step helps to reduce heat loss during the melting process and prevents early oxidation of the alloying elements.
[0135] Melting temperature: The melting point range of tin-lead-silver-copper alloy should be between 183°C and 190°C. The exact melting temperature depends on the specific proportions of the elements in the alloy, and the optimal melting temperature is usually determined experimentally.
[0136] Melting time: The time required for the alloy elements to completely melt is about 10-30 minutes;
[0137] The heating rate is controlled at 5-10°C / min to avoid excessive heating resulting in uneven alloy composition or oxidation.
[0138] Stirring speed: When using a stirring rod, stir gently at a speed of 30-60 revolutions per minute to ensure that the alloy components are evenly distributed while avoiding excessive bubbles.
[0139] In step S4, after each additive is added, stirring should be continued for 3 to 5 minutes to ensure that the additive is completely dispersed and evenly mixed.
[0140] In the present invention, the solder wire may be exposed to bacteria during the welding process, especially in a humid environment. The antibacterial agent can effectively inhibit the growth of bacteria and reduce the reproduction of bacteria on the surface of the solder wire, thereby maintaining the cleanliness and welding quality of the solder wire. By inhibiting bacterial growth, the antibacterial agent can extend the service life of the solder wire, reduce corrosion and oxidation caused by bacteria, thereby improving the overall performance and service life of the solder wire. The antibacterial agent can prevent the influence of bacteria on the performance of the solder wire and ensure the stability and reliability of the welding process. By inhibiting bacterial growth, the antibacterial agent can reduce corrosion and oxidation caused by bacteria, thereby reducing pollution to the environment. In addition, the addition of the antibacterial agent helps to reduce bacterial contamination of the solder wire during use, protecting the environment and human health. Therefore, the addition of the antibacterial agent can improve the antibacterial performance of the solder wire as a whole, inhibit bacterial growth, extend the service life, improve the welding quality, reduce environmental pollution, and is suitable for specific applications. These beneficial effects make the antibacterial agent an important part of the preparation process of the solder wire.
[0141] In the present invention, by precisely controlling the ratio of alloy elements such as tin, lead, silver, copper, gallium, etc., a solder wire with specific physical and chemical properties can be prepared to meet the diverse needs of circuit board welding. The added antioxidant, hardness enhancer, fluidity improver, flame retardant, viscosity modifier and conductivity enhancer can improve the performance of the solder wire and improve the overall oxidation resistance, hardness, fluidity, flame retardancy, viscosity and conductivity of the solder wire during use.
[0142] Embodiment three:
[0143] A preparation process and method of solder wire for circuit board, the method comprising the following steps:
[0144] S1: First weigh the raw materials:
[0145] 530 parts by weight of pure tin (Sn).
[0146] 330 parts by weight of lead (Pb).
[0147] 25 parts by weight of silver (Ag).
[0148] 15 parts by weight of copper (Cu).
[0149] 8 parts by weight of gallium;
[0150] 18 parts by weight antioxidant.
[0151] 8 parts by weight of antibacterial agent.
[0152] 13 parts by weight of hardness enhancer.
[0153] 6 parts by weight of flowability improver.
[0154] 13 parts by weight flame retardant.
[0155] 6 parts by weight of viscosity modifier.
[0156] 6 parts by weight of conductivity enhancer.
[0157] S2: Place the accurately weighed tin, lead, silver, copper and gallium elements into the preheated tin melting furnace in accordance with the formula ratio. Make sure the tin melting furnace is clean and dry to avoid contamination and oxidation;
[0158] S3: Start the heating system of the tin melting furnace and gradually raise the temperature to the predetermined melting point of the alloy. The melting point of tin-lead-silver-copper alloy is approximately between 183°C and 190°C. Keep the temperature stable until all alloy elements are completely melted. Use a stirring rod to gently stir to ensure that the alloy components in the molten pool are evenly distributed;
[0159] S4: After the alloy elements are completely melted and stirred evenly, antioxidants, antibacterial agents, hardness enhancers, fluidity improvers, flame retardants, viscosity modifiers and conductivity enhancers are added in sequence. Each additive must be accurately weighed according to the formula ratio and slowly added to the molten alloy;
[0160] S5: Continue to stir thoroughly with the stirring rod to ensure that all additives are completely mixed with the alloy matrix without precipitation and agglomeration. The stirring time should be long enough to ensure that the additives are evenly distributed in the alloy;
[0161] S6: Slowly pour the evenly stirred alloy solution into the pre-prepared solder wire mold. Avoid bubbles and splashes during the operation to ensure that the alloy solution fills the mold smoothly;
[0162] S7: Allow the alloy to cool naturally to room temperature in the mold to solidify the formed solder wire. The cooling process should be carried out in a dust-free, dry and temperature-stable environment to prevent oxidation of the solder wire surface;
[0163] S8: Take the cooled solder wire out of the die and install it on the wire drawing machine. Adjust the wire drawing machine to the required solder wire diameter and start the wire drawing machine for drawing. After drawing, use a precise cutting tool to cut the solder wire into the specified length.
[0164] S9: Pack the stretched and cut solder wire in moisture-proof and oxidation-proof packaging. Use special packaging materials to ensure that the solder wire is not affected by the external environment during storage and transportation. After packaging is completed, the entire preparation process of the solder wire for the circuit board is completed.
[0165] In step S1, the antioxidant is one or more of rosin, succinic acid, methyl chloride, zinc chloride, antioxidant oil or phosphate.
[0166] In step S1, the hardness enhancer is one or more of antimony (Sb), bismuth (Bi), tellurium (Te) or tungsten (W), which can improve the hardness and mechanical strength of the solder wire, so that it can maintain better shape and strength during the welding process.
[0167] In step S1, the fluidity improver is one or more of gallium (Ga), indium (In), tin (Sn) or lead (Pb). These elements can lower the melting point of the solder and improve its fluidity, making it easier for the solder wire to wet the soldering surface during soldering.
[0168] In step S1, the flame retardant is one or more of aluminum hydroxide (Al(OH)3), phosphate, zinc borate (ZnB) or antimony oxide (Sb2O3), which can reduce the flammability of the solder wire at high temperatures and improve its flame retardant properties.
[0169] In step S1, the viscosity modifier is one or more of silicone oil, polyethylene glycol (PEG), fatty acid or wax, which can adjust the viscosity of the solder wire so that it has better fluidity and stability during the welding process.
[0170] In step S1, the conductivity enhancer is one or more of nickel (Ni), silver (Ag), copper (Cu) or gold (Au). These elements can improve the conductivity of the solder wire and are suitable for soldering electronic components that require higher conductivity.
[0171] In step S1, the antimicrobial agent includes:
[0172] 1-2 parts by weight of silver nanoparticles, 1-3 parts by weight of chitosan, 0.5-1 parts by weight of titanium dioxide nanoparticles and 0.5-1 parts by weight of polyaminopropyltriethoxysilane;
[0173] The preparation method comprises:
[0174] Step 1: Synthesize silver nanoparticles and prepare silver nitrate solution: dissolve an appropriate amount of silver nitrate in deionized water. Add reducing agent glucose or ascorbic acid to the silver nitrate solution and heat to 80-90°C under stirring to perform a reduction reaction to generate silver nanoparticles.
[0175] Step 2: Prepare chitosan solution, dissolve chitosan in dilute acetic acid solution, stir until completely dissolved, and dilute the chitosan solution to the desired concentration.
[0176] Step 3: Prepare a titanium dioxide nanoparticle suspension by dispersing the titanium dioxide nanoparticles in deionized water and using an ultrasonic disperser to ensure uniform dispersion.
[0177] Step 4: Mix the antibacterial ingredients, add the synthesized silver nanoparticles to the chitosan solution, stir evenly, add the titanium dioxide nanoparticle suspension to the above mixture, continue stirring, add the coupling agent: finally add polyaminopropyl triethoxysilane, stir evenly to form a stable antibacterial agent mixture.
[0178] Step 5: Stabilization of the antimicrobial agent, cross-linking reaction: Under mild heating conditions, chitosan and polyaminopropyltriethoxysilane are cross-linked to enhance the stability of the antimicrobial agent. The mixture is cooled to room temperature and stored under sterile conditions to obtain the antimicrobial agent.
[0179] In step S3, the tin melting furnace is preheated to a temperature of 100-150° C. before adding the alloying elements. This step helps to reduce heat loss during the melting process and prevents early oxidation of the alloying elements.
[0180] Melting temperature: The melting point range of tin-lead-silver-copper alloy should be between 183°C and 190°C. The exact melting temperature depends on the specific proportions of the elements in the alloy, and the optimal melting temperature is usually determined experimentally.
[0181] Melting time: The time required for the alloy elements to completely melt is about 10-30 minutes;
[0182] The heating rate is controlled at 5-10°C / min to avoid excessive heating resulting in uneven alloy composition or oxidation.
[0183] Stirring speed: When using a stirring rod, stir gently at a speed of 30-60 revolutions per minute to ensure that the alloy components are evenly distributed while avoiding excessive bubbles.
[0184] In step S4, after each additive is added, stirring should be continued for 3 to 5 minutes to ensure that the additive is completely dispersed and evenly mixed.
[0185] In the present invention, the solder wire may be exposed to bacteria during the welding process, especially in a humid environment. The antibacterial agent can effectively inhibit the growth of bacteria and reduce the reproduction of bacteria on the surface of the solder wire, thereby maintaining the cleanliness and welding quality of the solder wire. By inhibiting bacterial growth, the antibacterial agent can extend the service life of the solder wire, reduce corrosion and oxidation caused by bacteria, thereby improving the overall performance and service life of the solder wire. The antibacterial agent can prevent the influence of bacteria on the performance of the solder wire and ensure the stability and reliability of the welding process. By inhibiting bacterial growth, the antibacterial agent can reduce corrosion and oxidation caused by bacteria, thereby reducing pollution to the environment. In addition, the addition of the antibacterial agent helps to reduce bacterial contamination of the solder wire during use, protecting the environment and human health. Therefore, the addition of the antibacterial agent can improve the antibacterial performance of the solder wire as a whole, inhibit bacterial growth, extend the service life, improve the welding quality, reduce environmental pollution, and is suitable for specific applications. These beneficial effects make the antibacterial agent an important part of the preparation process of the solder wire.
[0186] In the present invention, by precisely controlling the ratio of alloy elements such as tin, lead, silver, copper, gallium, etc., a solder wire with specific physical and chemical properties can be prepared to meet the diverse needs of circuit board welding. The added antioxidant, hardness enhancer, fluidity improver, flame retardant, viscosity modifier and conductivity enhancer can improve the performance of the solder wire and improve the overall oxidation resistance, hardness, fluidity, flame retardancy, viscosity and conductivity of the solder wire during use.
[0187] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0188] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A process and method for preparing solder wire for circuit boards, characterized in that: The method comprises the following steps: S1: First weigh the raw materials: 500-550 parts by weight of pure tin; 300-350 parts by weight of lead; 20-30 parts by weight of silver; 10 to 20 parts by weight of copper; 5 to 10 parts by weight of gallium; 15 to 20 parts by weight of antioxidant; 5 to 10 parts by weight of an antibacterial agent; 10 to 14 parts by weight of a hardness enhancer; 5 to 8 parts by weight of a fluidity improver; 10 to 15 parts by weight of flame retardant; 5 to 7 parts by weight of viscosity modifier; 5 to 8 parts by weight of conductivity enhancer; S2: Place accurately weighed tin, lead, silver, copper and gallium elements into the preheated tin melting furnace in order according to the formula ratio; ensure that the tin melting furnace is clean and dry to avoid contamination and oxidation; S3: Start the heating system of the tin melting furnace and gradually raise the temperature to the predetermined melting point of the alloy; the melting point of the tin-lead-silver-copper alloy is between 183°C and 190°C; keep the temperature stable until all the alloy elements are completely melted; use a stirring rod to gently stir to ensure that the alloy components in the molten pool are evenly distributed; S4: After the alloy elements are completely melted and stirred evenly, antioxidants, antibacterial agents, hardness enhancers, fluidity improvers, flame retardants, viscosity modifiers and conductivity enhancers are added in sequence; slowly added to the molten alloy; S5: Continue to stir thoroughly with the stirring rod to ensure that all additives are completely mixed with the alloy matrix without precipitation and agglomeration; S6: Slowly pour the evenly stirred alloy solution into the pre-prepared solder wire mold; avoid bubbles and splashes during the operation to ensure that the alloy solution fills the mold smoothly; S7: Allow the alloy to cool naturally to room temperature in the mold to solidify the formed solder wire; the cooling process is carried out in a dust-free, dry and temperature-stable environment to prevent oxidation of the solder wire surface; S8: Take the cooled solder wire out of the mold and install it on the wire drawing machine; adjust the wire drawing machine to the required solder wire diameter, and start the wire drawing machine for drawing; after the drawing is completed, use a precise cutting tool to cut the solder wire into a specified length; S9: The stretched and cut solder wire is packaged in moisture-proof and anti-oxidation packaging to ensure that the solder wire is not affected by the external environment during storage and transportation; after the packaging is completed, the entire preparation process of the solder wire for the circuit board is completed.
2. The process and method for preparing a solder wire for a circuit board according to claim 1, characterized in that: In step S1, the antioxidant is one or more of rosin, succinic acid, methyl chloride, zinc chloride, antioxidant oil or phosphate.
3. The process and method for preparing a solder wire for a circuit board according to claim 1, characterized in that: In the step S1, the hardness enhancer is one or more of antimony, bismuth, tellurium or tungsten.
4. The process and method for preparing a solder wire for a circuit board according to claim 1, characterized in that: In the step S1, the fluidity improver is one or more of gallium, indium, tin or lead.
5. The process and method for preparing solder wire for circuit board according to claim 1, characterized in that: In the step S1, the flame retardant is one or more of aluminum hydroxide, phosphate, and zinc borate.
6. The process and method for preparing a solder wire for a circuit board according to claim 1, characterized in that: In the step S1, the viscosity modifier is one or more of silicone oil, polyethylene glycol, fatty acid or wax.
7. The process and method for preparing solder wire for circuit board according to claim 1, characterized in that: In step S1, the conductivity enhancer is one or more of nickel, silver, copper or gold.
8. The process and method for preparing solder wire for circuit board according to claim 1, characterized in that: In step S1, the antibacterial agent includes: 1-2 parts by weight of silver nanoparticles, 1-3 parts by weight of chitosan, 0.5-1 parts by weight of titanium dioxide nanoparticles and 0.5-1 parts by weight of polyaminopropyltriethoxysilane; The preparation method comprises: Step 1: Synthesize silver nanoparticles and prepare a silver nitrate solution: dissolve an appropriate amount of silver nitrate in deionized water; add a reducing agent, glucose or ascorbic acid, to the silver nitrate solution, heat to 80-90° C. under stirring conditions, perform a reduction reaction, and generate silver nanoparticles; Step 2: Prepare a chitosan solution, dissolve chitosan in a dilute acetic acid solution, stir until completely dissolved, and dilute the chitosan solution to a desired concentration; Step 3: preparing a titanium dioxide nanoparticle suspension, dispersing the titanium dioxide nanoparticles in deionized water, and treating with an ultrasonic disperser to ensure uniform dispersion; Step 4: Mix the antibacterial components, add the synthesized silver nanoparticles to the chitosan solution, stir evenly, add the titanium dioxide nanoparticle suspension to the above mixture, continue stirring, add the coupling agent: finally add polyaminopropyl triethoxysilane, stir evenly, and form a stable antibacterial agent mixture; Step 5: Stabilization of the antibacterial agent, cross-linking reaction: Under mild heating conditions, chitosan and polyaminopropyltriethoxysilane are cross-linked to enhance the stability of the antibacterial agent; the mixture is cooled to room temperature and stored under sterile conditions to obtain the antibacterial agent.
9. The process and method for preparing solder wire for circuit board according to claim 1, characterized in that: In step S3, the tin melting furnace is preheated to 100-150° C. before adding the alloying elements; Melting temperature: The melting point of tin-lead-silver-copper alloy ranges from 183°C to 190°C; Melting time: The time required for the alloy elements to completely melt is 10-30 minutes; The heating rate is controlled at 5-10℃ / min; Stirring speed: When using a stirring rod, stir gently at a speed of 30-60 revolutions per minute to ensure that the alloy components are evenly distributed while avoiding excessive bubbles.
10. The process and method for preparing solder wire for circuit board according to claim 1, characterized in that: In step S4, after each additive is added, stirring is continued for 3 to 5 minutes to ensure that the additive is completely dispersed and evenly mixed.