Preparation and application of hydrophobic wood sponge for oil-water separation

The wood sponge prepared and loaded with polydimethylsiloxane and hydrophobic silica was solved by two chemical methods, and the problems of oil-water separation and wood resource recycling were achieved, and the oil-water separation effect was reduced. Carbon dioxide emissions.

CN118906163APending Publication Date: 2024-11-08GUANGXI UNIV FOR NATITIES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410788925.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing oil-water separation technology is difficult to effectively treat oil-containing wastewater and organic solvent emissions, and it is harmful to water resources and ecology. The recycling and utilization of wood resources has carbon dioxide emission problems.

Method used

Wood sponges were prepared by two chemical methods, and the impregnation load was carried by polydimethylsiloxane and hydrophobic silica, and hydrophobic wood sponges with high hydrophobic properties and reusability were prepared for oil-water separation.

Benefits of technology

It achieves efficient oil-water separation, improves the stability and reusability of the material, reduces carbon dioxide emissions, and the material is non-toxic and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HSA0000299541950000011
    Figure HSA0000299541950000011
  • Figure HSA0000299541950000012
    Figure HSA0000299541950000012
  • Figure HSA0000299541950000013
    Figure HSA0000299541950000013
Patent Text Reader

Abstract

The invention belongs to the technical field of oil-water separation, and discloses a method for preparing hydrophobic wood sponge, which comprises the following steps: (1) preparing waste wood into wood sponge through a two-step chemical method; and (2) loading PDMS and SiO2 onto the wood sponge through an impregnation method. The prepared PDMS / SiO2 (at) WS is adopted, the obtained wood sponge is characterized through a Fourier transform infrared spectrometer (FTIR) and an X-ray polycrystalline powder diffractometer (XRD), the optimal condition for preparing the composite wood sponge is obtained through single-factor analysis, the wood sponge is used for building a floating oil continuous collecting device, and floating oil can be rapidly separated and collected. The hydrophobicity and compressibility of the obtained wood sponge are improved, the reusability is good, the excellent oil-water separation capacity is shown, and the good application prospect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil-water separation and is a method for preparing a hydrophobic wood sponge. Background Art

[0002] Natural wood is a green, renewable resource with a unique longitudinal pore structure, excellent mechanical properties, and high chemical stability. It is primarily composed of cellulose, lignin, and hemicellulose. Simple chemical treatments can selectively remove lignin and hemicellulose from wood, followed by freeze-drying to yield a cellulose skeleton. Appropriate chemical modifications can then be made to develop wood sponges (WS) with various functional properties. The discharge of oily wastewater and organic solvents, as well as crude oil spills, pose serious risks to water resources, the environment, and even human health, and are receiving increasing attention. To address the environmental and resource challenges posed by these discharges, the use of adsorbent materials to absorb and recover oil is currently one of the most ideal and environmentally friendly methods for oil-water separation. The unique hydrophilic and lipophilic properties of wood sponges, combined with their inherently high porosity, make them suitable as efficient filtration materials for oil-water separation.

[0003] Wood sponges are made from waste wood. Forests are one of the most important ecosystems on Earth, covering over 30% of land and providing numerous renewable resources. Wood, composed of cellulose, hemicellulose, and lignin, is a building block for construction, furniture, and interior decoration, and is widely used in our daily lives. This means that wood waste is increasing, and the remaining wood is degraded by microorganisms, resulting in carbon dioxide emissions. Therefore, the recycling of wood resources is a priority, especially in order to achieve carbon neutrality.

[0004] Silica (SiO2) nanoparticles are non-toxic inorganic particles with hydrophobicity, which are often used to improve surface roughness. In order to prevent the particles from falling off during use, the multifunctional adhesive polydimethylsiloxane (PDMS) is used for waterproofing, anti-fouling, anti-freeze and anti-corrosion due to its inherent hydrophobicity and stability. Therefore, the non-toxic PDMS thin layer is an ideal choice for tightly binding inorganic particles to carbonized wood sponge. After loading it onto WS, it can evenly wrap the pore structure of the wood, giving the wood excellent superhydrophobicity. At the same time, the wood can still maintain its excellent porous structure, improving the stability and reusability of the wood.

[0005] Among the existing wood sponge preparation technologies, there are mainly two methods: chemical method and low eutectic solvent method.

[0006] In the present invention, waste wood is used as raw material to prepare wood sponge through a two-step chemical method, and then polydimethylsiloxane and silicon dioxide are loaded through an impregnation method to obtain a modified hydrophobic wood sponge, which can be used for oil-water separation. Summary of the Invention

[0007] The present invention uses wood sponge as a carrier and prepares the wood sponge through a two-step chemical method. Then, polydimethylsiloxane and hydrophobic silica are used as modified materials and loaded onto the wood sponge through a simple impregnation method to obtain a wood sponge with good hydrophobicity and high reusability, and the wood sponge is applied for oil-water separation.

[0008] To achieve the above-mentioned purpose, the present invention provides the following solutions:

[0009] (1) Preparation of wood sponge (WS): Wood blocks were immersed in a mixed aqueous solution of NaOH and Na2SO3 at room temperature and then heated in an oil bath to remove hemicellulose. After washing with deionized water, the blocks were immersed in a mixed solution of NaClO2 and CH3COOH and heated to remove lignin. Finally, the white wood blocks were freeze-dried to obtain porous wood sponge.

[0010] (2) Preparation of PDMS / SiO2@WS: Hydroxyl-terminated polydimethylsiloxane (PDMS-OH), tetraethyl orthosilicate (TEOS), dibutyltin diisocyanate (DBTDL) catalyst, and n-hexane were added to a beaker and stirred. Next, hydrophobic silica (SiO2) was added to the above mixture and ultrasonically dispersed for 30 minutes. The WS sample was immersed in the solution and then removed to evaporate the excess solvent. Finally, the wood sponge was placed in a vacuum oven to obtain PDMS / SiO2@WS.

[0011] 1. Preferably: the concentration ratio of sodium hydroxide and sodium sulfite in step (1) is 5:1

[0012] 2. Preferably: the alkaline solution heating reaction temperature in step (1) is 100°C.

[0013] 3. Preferably: the mass ratio of sodium chlorite, acetic acid and water in step (1) is 1:1:50

[0014] 4. Preferably, the acid solution is heated at a temperature of 80°C in step (1).

[0015] 5. Specifically: The heating reaction time of the alkaline solution in step (1) is 12 hours.

[0016] 6. Specifically: the heating reaction time of the acid solution in step (1) is 5 hours.

[0017] 7. Preferably, the mass of the PDMS in step (3) is 0.5 g.

[0018] 8. Preferably, the mass of TEOS in step (3) is 0.2 g.

[0019] 9. Preferably, the mass of the DBTDL in step (3) is 0.02 g.

[0020] 10. Preferably, the mass of the silicon dioxide in step (3) is 0.2 g.

[0021] The PDMS / SiO2@WS prepared by the present invention has good hydrophobicity, retains the characteristics of wood sponge, and has high compressibility; it has strong reusability and can be used for rapid collection of oil-water separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 FT-IR images of waste wood (NW), wood sponge (WS) and PDMS / SiO2@WS;

[0023] Figure 2 XRD patterns of WS, SiO2 and PDMS / SiO2@WS;

[0024] Figure 3 From left to right: comparison of water contact angles of NW, WS, and PDMS / SiO2@WS prepared in Example 5;

[0025] Figure 4 Comparison of the contact angle and separation efficiency of PDMS / SiO2@WS prepared in Example 5 with water;

[0026] Figure 5 This is the strain-stress curve of PDMS / SiO2@WS prepared in Example 1 at a strain of 10% to 60%. DETAILED DESCRIPTION

[0027] The present invention is further described below with reference to examples:

[0028] Example 1

[0029] A method for preparing PDMS / SiO2@WS comprises the following steps:

[0030] 1) Preparation of wood sponge (WS): Cut waste wood into 15×15×15 mm 3 The wood block was cleaned with ethanol and deionized water, and the clean wood block was dissolved in 200 mL of NaOH (2.5 mol·L -1 ) and 200mL Na2SO3 (0.5mol·L -1) mixed water solution at room temperature for 12 hours, then heated in an oil bath at 100°C for 12 hours to remove hemicellulose from the wood. After rinsing with deionized water, the mixture was transferred to a round-bottom flask containing 300 mL of deionized water, 6 g of NaClO₂, and 6 g of CH₃COOH. The flask was heated at 80°C for 5 hours to remove lignin from the wood. The resulting white wood block was rinsed with deionized water and finally freeze-dried to obtain a porous wood sponge.

[0031] 2) Preparation of PDMS / SiO2@WS: 0.5g of hydroxyl-terminated polydimethylsiloxane (PDMS-OH), 0.4g of tetraethylorthosilicate (TEOS), 0.04g of dibutyltin dioxysilicate (DBTDL) catalyst, and 40g of n-hexane were added to a 250mL beaker and stirred for 15min. Next, 0.2g of hydrophobic silica (SiO2) was added to the above mixture and ultrasonically dispersed for 30min. Again, the WS sample was immersed in the solution for 10min and then removed to evaporate the excess solvent. Finally,

[0032] The wood sponge was placed in a vacuum oven and heated at 80° C. for 12 hours to obtain a wood sponge composite material.

[0033] Example 2

[0034] The difference from Example 1 is that the concentration ratio of NaOH to Na2SO3 in step (1) is 1:1, and the other parameter conditions and operating steps are the same.

[0035] Example 3

[0036] The difference from Example 1 is that in step (1), the heating temperature of the mixed solution of NaOH and Na2SO3 is 70°C, 80°C, 90°C, 100°C, and 110°C, and the other parameter conditions and operating steps are the same.

[0037] Example 4

[0038] The difference from Example 1 is that in step (1), the heating temperature of the mixed solution of sodium chlorite and acetic acid is 70°C, 75°C, 80°C, 85°C, and 90°C, and the other parameter conditions and operating steps are the same.

[0039] Example 5

[0040] The difference from Example 1 is that the masses of PDMS-OH in step (2) are 0 g, 0.5 g, 1.0 g, 1.5 g, and 2.0 g, and the remaining parameter conditions and operating steps are the same.

[0041] Example 6

[0042] The difference from Example 1 is that the masses of TEOS in step (2) are 0 g, 0.1 g, 0.2 g, 0.3 g, and 0.4 g, and the remaining parameter conditions and operating steps are the same.

[0043] Example 7

[0044] The difference from Example 1 is that the masses of DBTDL in step (2) are 0 g, 0.01 g, 0.02 g, 0.03 g, and 0.04 g, and the remaining parameters, conditions, and operating steps are the same.

[0045] Example 8

[0046] The difference from Example 1 is that the masses of SiO2 in step (2) are 0g, 0.1g, 0.2g, 0.3g, and 0.4g, and the remaining parameter conditions and operating steps are the same.

[0047] The PDMS / SiO2@WS prepared in Examples 1 to 8 above were tested and analyzed. The reagents and instruments used in the experiments are as follows:

[0048] Sodium hydroxide: Sinopharm Chemical Reagent Co., Ltd.; sodium sulfite: Sinopharm Group Chemical Reagent Co., Ltd.; acetic acid: Sinopharm Chemical Reagent Co., Ltd.; sodium hypochlorite: Shanghai MacLean Biochemical Technology Co., Ltd.; hydroxyl-terminated polydimethylsiloxane: Shanghai Aladdin Biochemical Technology Co., Ltd.; dibutyltin diisocyanate: Shanghai Aladdin Biochemical Technology Co., Ltd.; ethyl silicate: Shanghai Aladdin Biochemical Technology Co., Ltd.; hydrophobic silica: Shanghai Aladdin Biochemical Technology Co., Ltd.; freeze dryer (FD-1000): Tokyo Rikkigi Co., Ltd.; Fourier transform infrared spectrometer (MAGNA-IR550): Thermo Fisher Scientific, USA; X-ray polycrystal powder diffractometer (MinFlex600): Rigaku Corporation; universal electronic testing machine (ZQ-990B): Dongguan Jingmiao Industrial Equipment Technology Co., Ltd.

[0049] Structural analysis and oil-water separation performance of prepared PDMS / SiO2@WS:

[0050] 1. Structural analysis:

[0051] FT-IR analysis of WS and PDMS / SiO2@WS Figure 1 Compared with NW, the wood blocks treated with NaClO2 showed a significant difference in the pore size at 1590, 1505, and 1465 cm -1 The characteristic peaks at 1737 and 1245 cm-1 at 1737 and 1245 cm-2 at 1737 and 1245 cm-3 at 1737 and 1245 cm-4 at 1245 cm-5 at 1737 and 1245 cm-6 at 1245 cm-7 at 1737 and 1245 cm-8 at 1245 cm-1 at 1245 -1The peaks of the characteristic hemicellulose peaks at 1261 and 801 cm are greatly reduced, indicating that some hemicellulose has been removed. The removal of lignin and hemicellulose transforms the original wood into a flexible wood sponge. - The weak absorption peak near 1 may be related to the Si-O-Si vibration peak and Si-CH3, indicating that the wood sponge and silica have a composite effect to a certain extent.

[0052] XRD analysis of SiO2, WS, and PDMS / SiO2@WS Figure 2 As shown. SiO2 has a broad diffuse peak at approximately 2θ = 22°, which is the characteristic peak of amorphous SiO2. Wood sponge has two peaks at 16.2 degrees (corresponding to the 101 crystal plane) and 22.2 degrees (corresponding to the 002 crystal plane), indicating that cellulose molecules can survive chemical etching (characteristic peaks 101 and 002 of cellulose). These components do not have regular crystal arrangement, so they appear as broad peaks in the XRD pattern. After SiO2 is loaded onto cellulose, the characteristic peaks of cellulose do not change, but the peak intensity increases, proving that the content of this crystal plane increases and SiO2 is successfully loaded onto the wood sponge.

[0053] 2. Static contact angle test

[0054] From left to right, the contact angles of NW, WS, SiO2@WS, and PDMS / SiO2@WS to water are shown in Figure 2. Figure 3 As shown, it can be seen that the contact angle of natural wood to water is 26.824°, and the contact angle of wood sponge is 00, which shows hydrophilicity. After loading SiO2 and PDMS, the hydrophobicity of the material is improved, and the contact angle can reach 145.071°, showing the high hydrophobicity of PDMS / SiO2@WS.

[0055] 3. Oil-water separation test

[0056] Sudan I was used to dye n-hexane, and a continuous oil absorption device was designed using PDMS / SiO2@WS as a filter membrane. This device mainly consists of three parts: PDMS / SiO2@WS, an oil collection tank, and a vacuum pump. The hose was inserted into the sponge along the direction of the wood grain; the other end of the hose was connected to the oil collection tank, and the oil collection tank was connected to the vacuum pump through the hose to obtain a continuous floating oil collection device. After the device was built, the oil separation efficiency of PDMS / SiO2@WS was tested. Figure 4 As shown in the figure, loading PDMS on SiO2@WS can improve the hydrophobicity of the material. The water contact angle of SiO2@WS material is 133.396°. The more PDMS is added, the higher the contact angle of the sponge is. However, too high a contact angle may clog the pores of the sponge and reduce the oil-water separation efficiency.

[0057] 4. Strain-stress testing

[0058] Figure 5 The stress-strain curves for PDMS / SiO2@WS at strains between 10% and 60% are shown. As can be seen, as the applied stress decreases, the strain can be completely reduced to zero, and the compressed sponge can recover to its original height, with minimal plastic deformation. The wood sponge exhibits excellent fatigue resistance, reflecting the material's excellent stability and compressibility, as well as its high reusability, which facilitates the recycling of oil-water separation materials.

[0059] Although the above describes the specific embodiments of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art on the basis of the technical solution of the present invention without any creative work are still within the scope of protection of the present invention.

Claims

1. A method for preparing a hydrophobic wood sponge for oil-water separation, characterized in that: The following steps are involved: (1) Preparation of wood sponge (WS): Cut the waste wood into 15×15×15 mm 3 The clean wood blocks were washed with ethanol and deionized water, and the clean wood blocks were precipitated in 200 mL of NaOH (2.5 mol·L -1 ) and 200mL Na2SO3 (0.5mol·L -1 ) mixed water solution at room temperature for 12 hours and then heated in an oil bath at 100°C for 12 hours to remove hemicellulose in the wood. After washing with deionized water, transfer to a round-bottom flask containing 300 mL of deionized water, NaClO2 (6 g) and CH3COOH (6 g). The flask was heated at 80°C for 5 hours to remove lignin in the wood. The obtained white wood block was washed with deionized water and finally freeze-dried to obtain a porous wood sponge. (2) Preparation of PDMS / SiO2@WS: 0.5 g of hydroxyl-terminated polydimethylsiloxane (PDMS-OH), 0.4 g of tetraethylorthosilicate (TEOS), 0.04 g of dibutyltin dioxysilicate (DBTDL) catalyst, and 40 g of n-hexane were added to a 250 mL beaker and stirred for 15 min. Secondly, 0.2 g of hydrophobic silica (SiO2) was added to the above mixture and ultrasonically dispersed for 30 min. Again, the WS sample was immersed in the solution for 10 min and then taken out to evaporate the excess solvent. Finally, the wood sponge was placed in a vacuum oven and heated at 80 °C for 12 h to obtain a wood sponge composite material.

2. The method for preparing a wood sponge according to claim 1, characterized in that: The concentration ratio of NaOH to Na2SO3 in step (1) is 5:

1.

3. The method for preparing a wood sponge according to claim 1, characterized in that: The mass ratio of sodium chlorite, acetic acid and water in step (1) is 1:1:

50.

4. The method for preparing a wood sponge according to claim 1, characterized in that: The heating temperature of the mixed solution of NaOH and Na2SO3 described in step (1) is 100°C.

5. The method for preparing a wood sponge according to claim 1, characterized in that: The heating temperature of the sodium chlorite and acetic acid mixed solution in step (1) is 80°C.

6. The method for preparing PDMS / SiO2@WS according to claim 1, characterized in that: The mass of PDMS-OH described in step (2) is 0.5 g.

7. The method for preparing PDMS / SiO2@WS according to claim 1, characterized in that: The mass of TEOS in step (2) is 0.2 g.

8. The method for preparing PDMS / SiO2@WS according to claim 1, characterized in that: The mass of DBTDL described in step (2) is 0.02 g.

9. The method for preparing PDMS / SiO2@WS according to claim 1, characterized in that: The mass of SiO2 described in step (2) is 0.2g.

10. The method for preparing PDMS / SiO2@WS according to any one of claims 6 to 9, characterized in that: The prepared PDMS / SiO2@WS was used for oil-water separation.