Preparation method and application of meglumine modified novel functional wood-based material

The new functional wood-based material modified by megamine solves the problem of excessive boron content in water, realizes efficient boron resource utilization and natural ecological protection, and has low cost and efficient adsorption characteristics.

CN118906165APending Publication Date: 2024-11-08QINGHAI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411107916.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently utilize boron resources, and excessive boron content in water bodies exceeds the standard poses a threat to the natural ecology.

Method used

A new functionalized wood-based material modified by megamine was prepared by epoxylation and megamine modification with wood blocks to prepare an adsorbent with high porosity and mechanical strength for different pH and Highly efficient adsorption of boron under temperature conditions.

Benefits of technology

The boron extraction in boron-rich water bodies is achieved, the boron content in the water bodies is reduced, and the production cost is low, the adsorption amount can reach more than 20mg/g, and the rapid separation effect is significant.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a meglumine-modified novel functional wood-based material, and the preparation method comprises the following steps: putting wood blocks into a reaction kettle, adding N, N-dimethylformamide, adding a catalyst, dropwise adding epoxy chloropropane in a stirring process, and reacting for a period of time after dropwise adding; cooling, dropwise adding a sodium hydroxide solution, heating, continuously reacting for a period of time, and washing to obtain an epoxy-terminated wood-based material; and putting the epoxy-terminated wood-based material into a reaction kettle, adding meglumine and N, N-dimethylformamide, heating under the protection of nitrogen, reacting for a period of time, naturally cooling to room temperature, washing and drying to obtain the meglumine-modified novel functional wood-based material. The meglumine-modified novel functional wood-based material is used for adsorbing and removing boron and has good adsorption performance. Under the conditions that the pH is 2-13 and the temperature is 10 DEG C or above, the adsorption capacity can reach 20 mg / g or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange and adsorption, and more specifically to a preparation method and application of a novel functionalized wood-based material modified by meglumine. Background Art

[0002] As an important chemical raw material, boron has a wide range of applications. Boron is crucial to the development of modern industry. It is not only important in the fields of glass, ceramics, detergents and agricultural fertilizers, but also plays a fundamental role in strategic industries such as metallurgy, aerospace, energy and national defense. At the same time, the application of organic boron compounds in the fields of medicine, functional materials, bioactive molecules, etc. also shows the chemical diversity and synthetic potential of boron. With the promotion of technological innovation, the development prospects of the boron industry are broad, which will have a positive impact on the industrial development and scientific and technological progress of my country and even the world. Therefore, the demand for boron is also increasing.

[0003] Methylglucamine is a compound containing multiple hydroxyl groups. Under appropriate conditions, it can form a stable complex with boron. It has significant effects and potential application value in the adsorption of boron, and can provide an effective solution for water treatment and boron resource recovery. In addition, based on the natural porous structure and rich chemical functional groups of wood, it can be given unique application properties through physical treatment or chemical modification.

[0004] Therefore, by utilizing the excellent selective chelation of borate by meglumine and the excellent mechanical strength, rich chemical functional groups and good pore structure of wood-based materials, a new functionalized wood-based material modified with meglumine is developed for the adsorption and removal of boron, which has broad application potential and important application value. Summary of the invention

[0005] In view of this, the present invention provides a preparation method and application of a novel functional wood-based material modified with meglumine, which can be used for the extraction of boron from boron-rich water bodies and from industrial wastewater, tap water, irrigation water and other water bodies, so as to achieve efficient utilization of boron resources or solve the threat to the natural ecology caused by excessive boron content in many water bodies.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing a novel functionalized wood-based material modified by meglumine comprises the following steps:

[0008] (1) placing a wood block in a reaction kettle, adding N,N-dimethylformamide and a catalyst, dropping epichlorohydrin during the stirring process, and reacting for a period of time after the dropping is completed; cooling, then dropping a sodium hydroxide solution, heating and continuing the reaction for a period of time, and then washing to obtain an epoxy-terminated wood-based material;

[0009] (2) The end-epoxy wood-based material is placed in a reaction kettle, and methylglucamine and N,N-dimethylformamide are added. The temperature is raised and reacted for a period of time under nitrogen protection, and the reaction is naturally cooled to room temperature. After washing and drying, a new functional wood-based material modified with methylglucamine is obtained.

[0010] Preferably, the amount of N,N-dimethylformamide added in step (1) is 200-300 mL.

[0011] Preferably, the mass ratio of the wood block, epichlorohydrin and sodium hydroxide solution in step (1) is: (30-50): (61.7-102.8): (33.4-55.6).

[0012] Preferably, the catalyst in step (1) is boron trifluoride diethyl ether.

[0013] Preferably, the dripping speed of epichlorohydrin in step (1) is 20-60 drops / min;

[0014] The concentration of the sodium hydroxide solution is 20-30%.

[0015] Preferably, after the dropwise addition in step (1) is completed, the reaction period is reflux at a constant temperature of 40-80° C. for 1-6 hours;

[0016] The cooling is to cool to below 40°C;

[0017] The step of continuing the reaction for a period of time after the temperature is raised is to raise the temperature to 65-85° C. and continue the reaction at a constant temperature for 2-6 hours.

[0018] Preferably, the mass ratio of the terminal epoxy wood-based material to meglumine in step (2) is: (30-50): (65.0-108.4);

[0019] The amount of N,N-dimethylformamide added is 400-800 mL.

[0020] Preferably, in step (2), heating and reacting for a period of time under nitrogen protection is heating to 50-90° C. and reacting for 2-8 hours.

[0021] Another object of the present invention is to provide the use of the novel functionalized wood-based material modified with meglumine obtained by the preparation method of the novel functionalized wood-based material modified with meglumine in boron adsorption;

[0022] Specifically, a new functional wood-based material modified with meglumine is used to adsorb boron under the conditions of pH 2-13 and temperature >10°C.

[0023] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following technical effects:

[0024] The adsorbent prepared by the present invention uses wood as a substrate, has a low production cost, and has high material porosity and strong mechanical properties, and can achieve efficient adsorption and rapid separation of boron, with an adsorption amount of more than 20 mg / g. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] This embodiment provides a method for preparing a novel functionalized wood-based material modified with meglumine, comprising the following steps:

[0028] (1) 30 parts of wood blocks of a certain size are placed in a reactor, 200 mL of N,N-dimethylformamide (DMF) is added, and 1 part of boron trifluoride diethyl ether is added as a catalyst. During the stirring process, 61.7 parts of epichlorohydrin are added dropwise at a rate of about 60 drops / min. After the addition is completed, the mixture is refluxed at a constant temperature of 40° C. for 6 hours; then the mixture is naturally cooled to below 40° C., 33.4 parts of a 30% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 75° C. and the reaction is continued at a constant temperature for 3 hours; after washing with distilled water for 4 times, an epoxy-terminated wood-based material is obtained.

[0029] (2) 30 parts of the epoxy-terminated wood-based material were placed in a reaction kettle, and 65.0 parts of meglumine and 400 mL of DMF were added. The temperature was raised to 90° C. under nitrogen protection for reaction for 2 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 4 times and then vacuum dried or naturally air-dried to obtain a novel functional wood-based material modified with meglumine.

[0030] The obtained new functional wood-based material modified with meglumine was used as a boron adsorbent for the extraction of boron from irrigation water. Under the conditions of pH 7.5 and temperature 20°C, its adsorption capacity for HBO2 can reach 20 mg / g.

[0031] Example 2

[0032] This embodiment provides a method for preparing a novel functionalized wood-based material modified with meglumine, comprising the following steps:

[0033] (1) 50 parts of wood blocks of a certain size are placed in a reactor, 300 mL of N,N-dimethylformamide (DMF) is added, and 0.9 parts of boron trifluoride diethyl ether is added as a catalyst. During the stirring process, 102.8 parts of epichlorohydrin are added dropwise at a rate of about 50 drops / min. After the addition is completed, the mixture is refluxed at a constant temperature of 70° C. for 2 hours; then the mixture is naturally cooled to below 40° C., 55.6 parts of a 25% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 85° C. and the reaction is continued at a constant temperature for 2 hours; after washing with distilled water for 3 times, an epoxy-terminated wood-based material is obtained.

[0034] (2) 30 parts of the end-epoxy wood-based material were placed in a reaction kettle, and 65.0 parts of meglumine and 500 mL of DMF were added. The temperature was raised to 50° C. under nitrogen protection for reaction for 8 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 3 times and then vacuum dried or naturally air-dried to obtain a novel functional wood-based material modified with meglumine.

[0035] The obtained new functional wood-based material modified with meglumine was used as a boron adsorbent for the extraction of boron from salt lake brine. Under the conditions of pH 8.5 and temperature 30°C, its adsorption capacity for HBO2 can reach 33 mg / g.

[0036] Example 3

[0037] This embodiment provides a method for preparing a novel functionalized wood-based material modified with meglumine, comprising the following steps:

[0038] (1) 50 parts of wood blocks of a certain size are placed in a reactor, 300 mL of N,N-dimethylformamide (DMF) is added, and 2.5 parts of boron trifluoride diethyl ether are added as a catalyst. During the stirring process, 102.8 parts of epichlorohydrin are added dropwise at a rate of about 30 drops / min. After the addition is completed, the mixture is refluxed at a constant temperature of 80° C. for 1 hour; then the mixture is naturally cooled to below 40° C., 55.6 parts of a 20% aqueous solution of sodium hydroxide are slowly added dropwise to the mixture, and the mixture is heated to 65° C. and the reaction is continued at a constant temperature for 6 hours; after washing with distilled water for 3 times, an epoxy-terminated wood-based material is obtained.

[0039] (2) 50 parts of the epoxy-terminated wood-based material were placed in a reaction kettle, and 108.4 parts of meglumine and 800 mL of DMF were added. The temperature was raised to 60° C. under nitrogen protection for reaction for 6 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 5 times and then vacuum dried or naturally air-dried to obtain a novel functional wood-based material modified with meglumine.

[0040] The obtained new functional wood-based material modified with meglumine was used as a boron adsorbent for the extraction of boron from industrial wastewater. Under the conditions of pH 12 and temperature 20°C, its adsorption capacity for HBO2 can reach 26 mg / g.

[0041] Example 4

[0042] (1) 40 parts of wood blocks of a certain size are placed in a reactor, 250 mL of N,N-dimethylformamide (DMF) is added, and 1.5 parts of boron trifluoride diethyl ether are added as a catalyst. During the stirring process, 82.3 parts of epichlorohydrin are added dropwise at a rate of about 20 drops / min. After the addition is completed, the mixture is refluxed at a constant temperature of 65° C. for 3 hours; then the mixture is naturally cooled to below 40° C., 44.5 parts of a 25% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 80° C. and the reaction is continued at a constant temperature for 3 hours; after washing with distilled water for 4 times, the end-epoxy wood-based material is obtained.

[0043] (2) 40 parts of the epoxy-terminated wood-based material were placed in a reaction kettle, and 86.7 parts of meglumine and 700 mL of DMF were added. The temperature was raised to 70° C. under nitrogen protection for 4 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 4 times and then vacuum dried or naturally air-dried to obtain a novel functional wood-based material modified with meglumine.

[0044] The obtained new functional wood-based material modified with meglumine was used as a boron adsorbent for the extraction of boron from geothermal water. Under the conditions of pH 7.5 and temperature 60°C, its adsorption capacity for HBO2 can reach 38 mg / g.

[0045] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0046] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a novel functionalized wood-based material modified with meglumine, characterized in that: The following steps are involved: (1) placing a wood block in a reaction kettle, adding N,N-dimethylformamide and a catalyst, dropping epichlorohydrin during the stirring process, and reacting for a period of time after the dropping is completed; cooling, then dropping a sodium hydroxide solution, heating and continuing the reaction for a period of time, and then washing to obtain an epoxy-terminated wood-based material; (2) The end-epoxy wood-based material is placed in a reaction kettle, and methylglucamine and N,N-dimethylformamide are added. The temperature is raised and reacted for a period of time under nitrogen protection, and the reaction is naturally cooled to room temperature. After washing and drying, a new functional wood-based material modified with methylglucamine is obtained.

2. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: The amount of N,N-dimethylformamide added in step (1) is 200-300 mL.

3. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: The mass ratio of the wood block, epichlorohydrin and sodium hydroxide solution in step (1) is: (30-50): (61.7-102.8): (33.4-55.6).

4. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: The catalyst in step (1) is boron trifluoride diethyl ether.

5. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: The dripping speed of epichlorohydrin in step (1) is 20-60 drops / min; The concentration of the sodium hydroxide solution is 20-30%.

6. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: After the dropwise addition in step (1) is completed, the reaction period is 1-6 hours at a constant temperature of 40-80° C. under reflux; The cooling is to cool to below 40°C; The step of continuing the reaction for a period of time after the temperature is raised is to raise the temperature to 65-85° C. and continue the reaction at a constant temperature for 2-6 hours.

7. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: The mass ratio of the terminal epoxy wood-based material to meglumine in step (2) is: (30-50): (65.0-108.4); The amount of N,N-dimethylformamide added is 400-800 mL.

8. The method for preparing a novel functionalized wood-based material modified by meglumine according to claim 1, characterized in that: In step (2), the heating and reaction for a period of time under nitrogen protection is heating to 50-90° C. and reacting for 2-8 hours.

9. Use of a novel functional wood-based material modified with meglumine obtained by the method for preparing a novel functional wood-based material modified with meglumine as claimed in any one of claims 1 to 8 in boron adsorption.

10. The use of the novel functionalized wood-based material modified with meglumine according to claim 9 in boron adsorption, characterized in that: A new functional wood-based material modified with meglumine was used to adsorb boron at a pH of 2-13 and a temperature of >10°C.