Preparation process of balancing weight
By preparing the shell for the counterweight block in the gym, the damage to the ground during the replacement of the counterweight block is solved, the protection effect of the counterweight block and the mechanical properties of the shell are improved, and the service life is extended.
Patent Information
- Application Number
- CN202410957548.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Gym counterweights are easily damaged to the ground when replacing them, resulting in unfavorable ground maintenance.
Using a counterweight preparation process, after cutting, grinding, drilling and sandblasting the steel, nitrile rubber, styrene resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane pairs are used. The coupling agent and double 25 vulcanizer are mixed to prepare the shell to protect the counterweight and reduce damage to the ground.
Effectively protect the counterweight blocks, reduce damage to the gym floor, improve the mechanical properties and durability of the shell, and extend the service life.
Smart Images

Figure BDA0004949306190000091 
Figure BDA0004949306190000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of gym counterweights, and in particular to a preparation process of counterweights. Background Art
[0002] Counterweights usually refer to heavy objects used to increase their own weight to maintain balance. Counterweights are used in a variety of fields. Among them, counterweights used in gyms are usually used in fitness equipment to increase the weight of fitness equipment.
[0003] The counterweights of fitness equipment are usually made of steel or cast iron. During the manufacturing process, the steel is first cut, and then the ends of the cut steel blocks are grinded and then sandblasted to make the surface of the steel blocks smooth and flat. The processed counterweights are then used to increase the weight of the fitness equipment.
[0004] However, the counterweight block treated as described above is directly applied to fitness equipment. When the counterweight block on the fitness equipment is taken and placed, due to its heavy weight, the counterweight block falls heavily to the ground when the user replaces it, which can easily damage the ground and is not conducive to the maintenance of the gym floor. Summary of the invention
[0005] In order to improve the problem that the counterweight block is heavy and causes the counterweight block to fall heavily to the ground when the user replaces it, which easily causes damage to the ground, the present application provides a preparation process for the counterweight block.
[0006] In a first aspect, the present application provides a process for preparing a counterweight block, which adopts the following technical solution: A preparation process of a counterweight block comprises the following steps: (1) Cutting the steel to obtain a counterweight block, grinding and drilling the counterweight block, and then sandblasting the counterweight block to obtain a processed counterweight block; (2) Mixing nitrile rubber, styrene acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent, stearic acid and dipentadienyl vulcanizing agent to obtain a shell, and placing the treated counterweight obtained in step (1) into the shell to obtain a counterweight.
[0007] By adopting the above technical scheme, the steel is cut into the required size to obtain the counterweight block, the edges and corners of the counterweight block are grinded to make the surface of the counterweight block smooth, and then holes are drilled to facilitate the subsequent installation of the counterweight block on the fitness equipment. The sandblasting is used to remove dirt, grease, oxide layer and other substances on the surface of the counterweight block workpiece, so that the surface of the counterweight block becomes clean and convenient for subsequent processing.
[0008] A shell of a counterweight is prepared and installed on the surface of the counterweight, which not only protects the counterweight but also greatly reduces the probability of the counterweight damaging the gym floor when the counterweight is taken from or placed on fitness equipment. Among them, nitrile rubber has good tensile strength, wear resistance, oil resistance, toughening, and good compression deformation and recovery, which can enhance the elasticity, weather resistance and aging resistance of the shell, and contribute to the long-term use of the shell; styrene-acrylic resin has good compatibility and processability, and is combined with nitrile rubber to improve the mechanical strength, chemical resistance, water resistance, heat resistance and adhesion of the shell; the addition of an anti-aging agent can delay the aging of the shell and increase the durability and service life of the shell.
[0009] Modified basalt fiber has good mechanical strength, heat resistance and corrosion resistance. When mixed with nitrile rubber and styrene acrylic resin, it can increase the mechanical properties of the shell, making the shell have good tensile properties and impact resistance. Modified ceramic particles have filling and adsorption effects. When mixed with nitrile rubber, styrene acrylic resin and modified basalt fiber, the strength, heat resistance, corrosion resistance, wear resistance and weather resistance of the shell are improved.
[0010] Silane coupling agent can improve the heat resistance, wear resistance, flame retardancy, water resistance and processability of the shell, and can make the various components in the shell mixed evenly, further exert the functional role of each component, and jointly improve the comprehensive performance of the shell; stearic acid is used as a lubricant to make the various components dispersed evenly, while reducing the friction between the system and the mold and improving the fluidity during the processing; dipentadienyl vulcanizer promotes the cross-linking reaction of rubber molecules during the processing, thereby improving the corresponding performance of the shell.
[0011] Preferably, the nitrile rubber comprises 70-80 parts, styrene acrylic resin comprises 40-50 parts, anti-aging agent comprises 1-2 parts, modified basalt fiber comprises 20-30 parts, modified ceramic particles comprises 10-20 parts, silane coupling agent comprises 5-9 parts, stearic acid comprises 2-5 parts and dipentadienyl vulcanizing agent comprises 1-3 parts.
[0012] By adopting the above technical scheme, the content of each component is further limited, so that each component cooperates with each other to jointly improve the comprehensive properties of the shell, such as the mechanical properties. Within a certain dosage range, each component jointly improves the comprehensive properties of the shell, such as the mechanical strength, tear resistance, and tensile properties. Nitrile rubber and styrene acrylic resin have high tensile strength, wear resistance and elasticity, modified basalt fiber has good mechanical strength and heat resistance, and modified ceramic particles have good strength, heat resistance and wear resistance. Nitrile rubber, styrene acrylic resin, modified basalt fiber and modified ceramic particles cooperate to jointly improve the mechanical properties of the shell, which is conducive to the durability of the subsequent use of the shell.
[0013] Preferably, the method for preparing the shell comprises the following steps: mixing and kneading nitrile rubber, styrene acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent and stearic acid, kneading for 30-35 minutes at a temperature of 70-80°C, adding a dipentadienyl vulcanizing agent, heating to 180-190°C, vulcanizing for 1-2 hours, and then compression molding to obtain the shell.
[0014] By adopting the above technical scheme, nitrile rubber, styrene acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent and stearic acid are mixed evenly, firstly mixed to make the components evenly dispersed, and then a di-25 vulcanizing agent is added for vulcanization to further improve the mechanical properties of the shell, and then compression molding is performed to obtain the shell. The obtained shell has comprehensive properties such as high mechanical strength. The operation method is simple and has high processing efficiency, and can be applied to large-scale industrial production.
[0015] Preferably, the method for preparing the modified basalt fiber comprises the following steps: (1) dispersing basalt fiber in a hydrochloric acid solution, stirring for 1-2 hours, washing with water, and then dispersing in a silane coupling agent aqueous solution, continuing to stir for 20-30 minutes, filtering, and drying to obtain pretreated basalt fiber; (2) dispersing graphene in anhydrous ethanol, ultrasonicating for 1-2 hours, adding amino acids to obtain a mixed solution, stirring for 1-2 hours, and then leaching the basalt fiber treated in step (1) into the mixed solution, and drying the basalt fiber after extraction to obtain a mixture; (3) Dispersing chitosan in acetic acid solution, stirring for 10-20 minutes, and then spraying it on the surface of the mixture in step (2) to obtain modified basalt fiber.
[0016] By adopting the above technical scheme, the basalt fiber is first pretreated with hydrochloric acid to remove organic impurities on the surface of the basalt fiber, improve the surface roughness of the basalt fiber, and facilitate the subsequent mixing of the basalt fiber with other components; then it is dispersed in an aqueous solution of a silane coupling agent, and the silane coupling agent is used to pretreat the basalt fiber. The surface of the basalt fiber contains a large number of hydroxyl groups and negatively charged groups, and the silane coupling agent contains a large number of hydroxyl groups, amino groups and silane groups. A strong chemical bond is formed between the basalt fiber and the silane coupling agent, thereby improving the durability and wear resistance of the basalt fiber.
[0017] Graphene has good mechanical properties and flexibility. The surface functional groups of graphene mainly include hydrogen atoms, carboxyl groups and carbonyl groups. The surface of amino acids mainly contains amino groups, carboxyl groups, hydrogen atoms and side chain groups. The amino groups in amino acids can react with the carboxyl groups in graphene, so that the amino acids are loaded on the graphene, which improves the dispersibility of graphene and prevents the agglomeration of graphene. Then, the basalt fiber is immersed in the mixed solution, and the hydroxyl groups in the graphene react with the silane coupling agent to enable the graphene to be loaded on the surface of the basalt fiber, further improving the mechanical properties of the basalt fiber. The chitosan solution has good viscosity and mechanical properties. The chitosan solution is sprayed on the surface of the mixture so that the chitosan forms a thin film coated on the surface of the basalt fiber, thereby making the graphene and basalt fiber bond more closely, improving the performance stability of the basalt fiber, and subsequently improving the mechanical properties of the basalt fiber such as mechanical strength and tear resistance. It is implemented in the outer shell, thereby improving the corresponding performance of the outer shell.
[0018] Preferably, the mass ratio of the basalt fiber, graphene, amino acid and chitosan is 1g:10-15mg:4-7g:0.3-0.6g.
[0019] By adopting the above technical scheme, the mass ratio of basalt fiber, graphene, amino acid and chitosan is further limited within a certain range, thereby improving the comprehensive properties of basalt fiber such as mechanical properties. Basalt fiber itself has high stability, corrosion resistance, combustion resistance, high temperature resistance and other properties. Graphene has good mechanical properties and toughness. Amino acids change the probability of graphene agglomeration. Chitosan has good film-forming properties and mechanical properties and can coat basalt fiber, making the connection between basalt fiber, graphene and amino acid tighter. Basalt fiber, graphene, amino acid and chitosan cooperate to improve the comprehensive properties of basalt fiber such as mechanical properties.
[0020] Preferably, in step (2), the basalt fiber is immersed in the mixed solution, extracted 2-3 times, each time immersed in the mixed solution for 50-60 seconds, and the basalt fiber is dried after each extraction to obtain a mixture.
[0021] By adopting the above technical solution, the basalt fiber is extracted so that the diameter of the basalt fiber can be adjusted. The diameter of the basalt fiber is ensured, and the fiber is dried after each extraction so that the graphene is better loaded on the surface of the basalt fiber, thereby further improving the mechanical properties of the basalt fiber and subsequently improving the corresponding performance of the shell.
[0022] Preferably, the method for preparing the modified ceramic particles comprises the following steps: (1) crushing and grinding the ceramic particles, dispersing them in a sodium hydroxide solution, stirring for 1-2 hours, filtering, and drying to obtain a pretreated ceramic powder; (2) dispersing the ceramic powder obtained in step (1) in deionized water, adding carbon nanotubes, ultrasonicating for 1-2 hours, and then filtering to obtain a mixture; (3) Dissolve xanthan gum in deionized water, stir at a temperature of 80-85° C. for 1-2 hours, add starch, continue stirring to obtain a mixed solution, and then spray the mixed solution on the surface of the mixture in step (2), dry, and obtain modified ceramic particles.
[0023] By adopting the above technical solution, the ceramic particles are ground and then dispersed in a sodium hydroxide solution. The sodium hydroxide erodes the surface of the ceramic particles to a certain extent, thereby increasing the roughness of the surface of the ceramsite particles and further increasing the specific surface area of the ceramic particles. The obtained ceramic powder is helpful for compounding with other components.
[0024] Carbon nanotubes have a one-dimensional hollow tubular structure with good strength, high specific surface area, elasticity and toughness. Carbon nanotubes can be loaded in the surface pores of ceramic powder to increase the mechanical strength of ceramic powder. Xanthan gum has a certain viscosity when dissolved in deionized water. The addition of starch increases the viscosity of the xanthan gum aqueous solution. The mixture of xanthan gum and starch has a synergistic effect. A network structure is formed between the xanthan gum and starch, thereby improving the viscosity and cohesion of the system. The subsequent spraying on the surface of the mixture makes the ceramic powder and the carbon nanotubes have good adhesion, thereby increasing the performance stability of the ceramic particles, so that the modified ceramic particles have better mechanical properties and performance stability, which is subsequently helpful to improve the comprehensive performance of the shell.
[0025] Preferably, the mass ratio of the ceramic particles, carbon nanotubes and mixed liquid is 1:0.7-0.9:0.4-0.6.
[0026] By adopting the above technical scheme, the mass ratio of ceramic particles, carbon nanotubes and mixed liquid is further limited within a certain range, thereby improving the corresponding performance of the ceramic particles. The carbon nanotubes can be loaded on the surface of the ceramic particles, and the mixed liquid is sprayed on the surface of the ceramic particles to coat the ceramic particles, so that the connection between the ceramic particles and the carbon nanotubes is tighter, thereby improving the mechanical properties of the ceramic particles. Subsequently, it is implemented in the outer shell to improve the corresponding performance of the outer shell.
[0027] Preferably, the mass ratio of xanthan gum to starch is 1:0.2-0.4.
[0028] By adopting the above technical scheme, the mass ratio of xanthan gum and starch is further limited. There is a synergistic effect between xanthan gum and starch, and a network structure is formed between xanthan gum and starch, thereby improving the viscosity and cohesion of the system, making the mixed liquid more adhesive, and subsequently spraying it on the surface of ceramic particles, thereby improving the connectivity between ceramic powder and carbon nanotubes, thereby improving the corresponding performance of ceramic particles.
[0029] Preferably, the antioxidant is one or more of antioxidant 4010, antioxidant DNP, and antioxidant MB.
[0030] By adopting the above technical solution, the types of anti-aging agents are further limited. The addition of anti-aging agents can delay the aging of the shell, increase the durability and service life of the shell, and cooperate with other components so that the various raw materials cooperate with each other to jointly improve the durability of the shell.
[0031] In summary, this application has the following beneficial effects: 1. In the present application, a shell of a counterweight is prepared and installed on the surface of the counterweight, which not only protects the counterweight but also greatly reduces the probability of the counterweight damaging the gym floor when the counterweight is taken from and placed on the fitness equipment. Among them, nitrile rubber has good tensile strength, wear resistance, oil resistance, toughening, and good compression deformation and recovery, which can enhance the elasticity, weather resistance and aging resistance of the shell, and contribute to the long-term use of the shell; styrene-acrylic resin has good compatibility and processability, and is combined with nitrile rubber to improve the mechanical strength, chemical resistance, water resistance, heat resistance and adhesion of the shell; the addition of an anti-aging agent can delay the aging of the shell and increase the durability and service life of the shell.
[0032] 2. The modified basalt fiber in this application has good mechanical strength, heat resistance and corrosion resistance. When mixed with nitrile rubber and styrene-acrylic resin, it can increase the mechanical properties of the outer shell, making the outer shell have good tensile properties and impact resistance; the modified ceramic particles have filling and adsorption effects, and when mixed with nitrile rubber, styrene-acrylic resin and modified basalt fiber, the strength, heat resistance, corrosion resistance, wear resistance and weather resistance of the outer shell are improved.
[0033] 3. The silane coupling agent in the present application can improve the heat resistance, wear resistance, flame retardancy, water resistance and processability of the outer shell, and can make the various components in the outer shell mixed evenly, further exert the functional role of each component, and jointly improve the comprehensive performance of the outer shell; stearic acid is used as a lubricant to make the various components dispersed evenly, while reducing the friction between the system and the mold and improving the fluidity during the processing; the dipentadienyl vulcanizer promotes the cross-linking reaction of rubber molecules during the processing, thereby improving the corresponding performance of the outer shell. DETAILED DESCRIPTION
[0034] The present application is further described in detail below with reference to the embodiments.
[0035] The raw materials used in the examples and comparative examples can all be obtained commercially.
[0036] Preparation example of modified basalt fiber Preparation Example 1-1 The preparation method of modified basalt fiber comprises the following steps: (1) 1.3 kg of basalt fiber was dispersed in 2 L of 10% hydrochloric acid solution, stirred for 1.5 h, washed with water, and then dispersed in 3 L of 2% silane coupling agent KH-560 aqueous solution, stirred for 25 min, filtered and dried to obtain pretreated basalt fiber; (2) dispersing graphene in 1.5 L of anhydrous ethanol, ultrasonicating for 1.5 h, adding L-serine to obtain a mixed solution, stirring for 1.5 h, and then extracting the basalt fiber treated in step (1) into the mixed solution, and drying the basalt fiber after extraction to obtain a mixture; (3) Dispersing chitosan in 1 L of 8% by mass acetic acid solution, stirring for 18 min, and then spraying the mixture on the surface of the mixture in step (2) to obtain modified basalt fiber.
[0037] The mass ratio of basalt fiber, graphene, L-serine and chitosan is 1g:10mg:4g:0.3g.
[0038] In step (2), the basalt fiber is immersed in the mixed solution and extracted twice, each time being immersed in the mixed solution for 50 seconds, and the basalt fiber is dried after each extraction to obtain a mixture.
[0039] Among them, L-serine was purchased from Shandong Gushuo Biotechnology Co., Ltd.
[0040] Preparation Example 1-2 The difference from Preparation Example 1-1 is that in step (2), no graphene is added.
[0041] Preparation Example 1-3 The difference from Preparation Example 1-1 is that in step (2), L-serine is not added.
[0042] Preparation Example 1-4 The difference from Preparation Example 1-1 is that in step (3), chitosan is not added.
[0043] Preparation Example 1-5 The difference from Preparation Example 1-1 is that the mass ratio of basalt fiber, graphene, L-serine and chitosan is 1 g:15 mg:7 g:0.6 g.
[0044] In step (2), the basalt fiber is immersed in the mixed solution and extracted three times, each time being immersed in the mixed solution for 60 seconds, and the basalt fiber is dried after each extraction to obtain a mixture.
[0045] Preparation Example 1-6 The difference from Preparation Example 1-1 is that the mass ratio of basalt fiber, graphene, L-serine and chitosan is 1 g:18 mg:1 g:0.9 g.
[0046] Preparation example of modified ceramic particles Preparation Example 2-1 The preparation method of modified ceramic particles comprises the following steps: (1) 1.5 kg of ceramic particles were crushed and ground, and then dispersed in 3 L of 12% sodium hydroxide solution, stirred for 1.5 h, filtered, and dried to obtain pretreated ceramic powder; (2) dispersing the ceramic powder obtained in step (1) in 3 L of deionized water, adding carbon nanotubes, ultrasonicating for 2 h, and then filtering to obtain a mixture; (3) Dissolve xanthan gum in 0.2 L of deionized water, stir at 85° C. for 2 h, add starch, continue stirring for 1 h to obtain a mixed solution, and then spray the mixed solution on the surface of the mixture in step (2), dry, and obtain modified ceramic particles.
[0047] The mass ratio of ceramic particles, carbon nanotubes and mixed liquid is 1:0.9:0.4.
[0048] The mass ratio of xanthan gum to starch is 1:0.2; the starch is corn starch.
[0049] Preparation Example 2-2 The difference from Preparation Example 2-1 is that in step (2), no carbon nanotubes are added.
[0050] Preparation Example 2-3 The difference from Preparation Example 2-1 is that in step (3), no xanthan gum is added.
[0051] Preparation Example 2-4 The difference from Preparation Example 2-1 is that in step (3), no starch is added.
[0052] Preparation Example 2-5 The difference from Preparation Example 2-1 is that the mass ratio of ceramic particles, carbon nanotubes and mixed liquid is 1:0.7:0.6.
[0053] The mass ratio of xanthan gum to starch is 1:0.4.
[0054] Preparation Example 2-6 The difference from Preparation Example 2-1 is that the mass ratio of ceramic particles, carbon nanotubes and mixed liquid is 1:0.2:0.9.
[0055] Preparation Example 2-7 The difference from Preparation Example 2-1 is that the mass ratio of xanthan gum to starch is 1:0.1. Example
[0056] Example 1 A preparation process of a counterweight block comprises the following steps: (1) Cutting the steel to obtain counterweight blocks, each counterweight block weighing 10 kg, grinding, drilling, and then sandblasting the counterweight blocks to obtain processed counterweight blocks; (2) Mixing nitrile rubber, styrene acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent KH792, stearic acid and dipentadienyl vulcanizing agent to obtain a shell, and placing the treated counterweight obtained in step (1) into the shell to obtain a counterweight.
[0057] 70kg of nitrile rubber, 40kg of styrene acrylic resin, 1kg of anti-aging agent, 30kg of modified basalt fiber, 20kg of modified ceramic particles, 5kg of silane coupling agent KH792, 2kg of stearic acid and 1kg of dipentadienyl vulcanizing agent.
[0058] The solid content of the styrene acrylic resin is 43%, and the styrene acrylic resin is polymerized by styrene, acrylic acid, methyl methacrylate and a cross-linking monomer, wherein the cross-linking monomer is glycidyl methacrylate; the nitrile rubber is purchased from Sichuan Xintianhai Chemical Co., Ltd.
[0059] The preparation method of the shell comprises the following steps: mixing and kneading nitrile rubber, styrene acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent KH792 and stearic acid, kneading for 30 minutes at a temperature of 70°C, adding a dipentadienyl vulcanizing agent, heating to 190°C, vulcanizing for 1 hour, and then compression molding to obtain the shell.
[0060] The antioxidant is antioxidant 4010.
[0061] The modified basalt fiber was prepared by using Preparation Example 1-1; the modified ceramic particles were prepared by using Preparation Example 2-1.
[0062] Example 2 A preparation process of a counterweight block, which differs from Example 1 in that 80 kg of nitrile rubber, 50 kg of styrene-acrylic resin, 2 kg of anti-aging agent, 20 kg of modified basalt fiber, 10 kg of modified ceramic particles, 9 kg of silane coupling agent KH792, 5 kg of stearic acid and 3 kg of dipentadienyl vulcanizing agent are included.
[0063] The preparation method of the shell comprises the following steps: mixing and kneading nitrile rubber, styrene-acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent KH792 and stearic acid, kneading for 35 minutes at a temperature of 80°C, adding a dipentadienyl vulcanizing agent, heating to 180°C, vulcanizing for 2 hours, and then compression molding to obtain the shell.
[0064] Example 3 A preparation process of a counterweight block, which is different from Example 1 in that the modified basalt fiber is prepared using Preparation Example 1-2.
[0065] Example 4 A preparation process of a counterweight block, which is different from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 1-3.
[0066] Example 5 A preparation process of a counterweight block, which is different from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 1-4.
[0067] Example 6 A preparation process of a counterweight block, which is different from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 1-5.
[0068] Example 7 A preparation process of a counterweight block, which is different from Example 1 in that the modified basalt fiber is prepared using Preparation Examples 1-6.
[0069] Example 8 A preparation process of a counterweight block, which differs from Example 1 in that the modified ceramic particles are prepared using 2-2.
[0070] Example 9 A preparation process of a counterweight block, which differs from Example 1 in that the modified ceramic particles are prepared using 2-3.
[0071] Example 10 A preparation process of a counterweight block, which differs from Example 1 in that the modified ceramic particles are prepared using 2-4.
[0072] Embodiment 11 A preparation process of a counterweight block, which differs from Example 1 in that the modified ceramic particles are prepared using 2-5.
[0073] Example 12 A preparation process of a counterweight block, which differs from Example 1 in that the modified ceramic particles are prepared using 2-6.
[0074] Example 13 A preparation process of a counterweight block, which differs from Example 1 in that the modified ceramic particles are prepared using 2-7.
[0075] Comparative Example Comparative Example 1 A preparation process of a counterweight block, which differs from Example 1 in that modified basalt fiber is not added.
[0076] Comparative Example 2 A preparation process of a counterweight block, which differs from Example 1 in that an equal amount of modified basalt fiber is replaced by basalt fiber.
[0077] Comparative Example 3 A preparation process for a counterweight block, which differs from Example 1 in that no modified ceramic particles are added.
[0078] Comparative Example 4 A preparation process of a counterweight block, which differs from Example 1 in that an equal amount of ceramic particles are used instead of modified ceramic particles.
[0079] Performance testing The shells prepared in Examples 1-13 and Comparative Examples 1-4 were subjected to the following performance tests: Tensile strength is tested according to GB / T528-2009; Bending strength is tested according to GB / T1449-2005; Impact strength is tested according to GB / T1451-2005; Elongation at break is tested according to ASTM D638 The wear rate test was carried out according to ASTM D790; the test results are shown in Table 1.
[0080] Table 1 Test data of embodiments and comparative examples It can be seen from Table 1 that the shells prepared in Examples 1-2, Example 6, and Example 11 of the present application have excellent mechanical strength and low wear rate, among which the tensile strength of Example 1 is 15.6 MPa, the bending strength is 31.2 MPa, the impact strength is 13.5 J / m, the elongation at break is 146%, and the wear rate is 20 mg, indicating that the shell prepared in the present application has high tensile strength, bending strength, impact resistance, elongation at break and wear rate. The components in the present application cooperate with each other, so that the prepared shell has excellent mechanical properties, and the shell subsequently applied to the counterweight block has excellent mechanical properties and durability.
[0081] Graphene is not added in the preparation method of the modified basalt fiber in Example 3. It can be seen from Table 1 that compared with Example 1, the tensile strength is 10.1 MPa, the bending strength is 26.3 MPa, the impact strength is 8.0 J / m, the elongation at break is 135%, and the abrasion rate is 27 mg, indicating that the graphene in the present application has good mechanical properties and flexibility, can improve the mechanical properties of the basalt fiber, and subsequently improve the corresponding performance of the outer shell.
[0082] In the preparation method of modified basalt fiber in Example 4, no amino acid is added. It can be seen from Table 1 that compared with Example 1, the tensile strength is 11.2 MPa, the bending strength is 27.1 MPa, the impact strength is 9.1 J / m, the elongation at break is 137%, and the abrasion rate is 25 mg, indicating that the surface of the amino acid in the present application mainly contains amino groups, carboxyl groups, hydrogen atoms and side chain groups. The amino group in the amino acid can react with the carboxyl group in the graphene, so that the amino acid is loaded on the graphene, which improves the dispersibility of the graphene and prevents the agglomeration of the graphene, thereby helping the graphene to better exert the comprehensive properties such as mechanical properties, and subsequently improve the corresponding properties of the shell.
[0083] In the preparation method of modified basalt fiber in Example 5, chitosan is not added. As can be seen from Table 1, compared with Example 1, the tensile strength is 12.1 MPa, the flexural strength is 28.2 MPa, the impact strength is 10.2 J / m, the elongation at break is 139%, and the abrasion rate is 24 mg, indicating that the chitosan solution in the present application has good viscosity and mechanical properties. The chitosan solution is sprayed on the surface of the mixture so that the chitosan forms a thin film coated on the surface of the basalt fiber, thereby making the graphene and basalt fiber bond more closely, improving the performance stability of the basalt fiber, and subsequently improving the mechanical properties of the basalt fiber such as mechanical strength and tear resistance, and is applied to the outer shell, thereby improving the corresponding performance of the outer shell.
[0084] In Example 7, the mass ratio of basalt fiber, graphene, amino acid and chitosan is changed. It can be seen from Table 1 that compared with Example 1, the performance of tensile strength, flexural strength, impact strength, elongation at break and abrasion rate are better than that of Examples 3-5, but worse than that of Examples 1 and 6, indicating that graphene has good mechanical properties and toughness, amino acids change the probability of easy agglomeration of graphene, chitosan has good film-forming properties and mechanical properties, can coat basalt fiber, make the connection between basalt fiber, graphene and amino acid closer, basalt fiber, graphene, amino acid and chitosan cooperate, thereby improving the comprehensive properties of basalt fiber such as mechanical properties.
[0085] In the preparation method of modified ceramic particles in Example 8, carbon nanotubes are not added. As can be seen from Table 1, compared with Example 1, the tensile strength is 10.9 MPa, the bending strength is 26.7 MPa, the impact strength is 8.6 J / m, the elongation at break is 137%, and the abrasion rate is 26 mg, indicating that the carbon nanotubes of the present application have good strength, high specific surface area, elasticity and toughness, and the carbon nanotubes can be loaded in the surface pores of the ceramic powder to increase the mechanical strength of the ceramic powder, thereby contributing to the subsequent improvement of the corresponding performance of the shell.
[0086] No xanthan gum is added in the preparation method of the modified ceramic particles in Example 9. As can be seen from Table 1, compared with Example 1, the tensile strength is 11.4 MPa, the flexural strength is 27.4 MPa, the impact strength is 9.3 J / m, the elongation at break is 139%, and the abrasion rate is 25 mg, indicating that the xanthan gum of the present application has a certain viscosity when dissolved in deionized water, and is subsequently sprayed on the surface of the mixture, so that the ceramic powder and the carbon nanotubes have good adhesion, thereby increasing the performance stability of the ceramic particles, so that the modified ceramic particles have better mechanical properties and performance stability, which is subsequently helpful to improve the comprehensive performance of the shell.
[0087] In the preparation method of modified ceramic particles in Example 10, starch is not added. As can be seen from Table 1, compared with Example 1, the tensile strength is 12.5 MPa, the flexural strength is 28.6 MPa, the impact strength is 10.8 J / m, the elongation at break is 140%, and the abrasion rate is 24 mg, indicating that the mixture of xanthan gum and starch in the present application has a synergistic effect. A network structure is formed between the xanthan gum and the starch, thereby improving the viscosity and cohesion of the system. Subsequently, the mixture is sprayed on the surface, so that the ceramic powder and the carbon nanotubes have better adhesion, so that the modified ceramic particles have better mechanical properties and performance stability, which is subsequently helpful to improve the comprehensive performance of the shell.
[0088] Example 12 changes the mass ratio of ceramic particles, carbon nanotubes and the mixed liquid. It can be seen from Table 1 that compared with Example 1, the tensile strength, flexural strength, impact strength, elongation at break and abrasion rate are better than those of Examples 8-9, but worse than those of Examples 1 and 11, indicating that carbon nanotubes can be loaded on the surface of ceramic particles. The mixed liquid is sprayed on the surface of the ceramic particles to coat the ceramic particles, making the connection between the ceramic particles and the carbon nanotubes tighter, thereby improving the mechanical properties of the ceramic particles. Subsequently, it is implemented in the outer shell to improve the corresponding performance of the outer shell.
[0089] Example 13 changes the mass ratio of xanthan gum and starch. It can be seen from Table 1 that compared with Example 1, the tensile strength, flexural strength, impact strength, elongation at break and abrasion rate are better than those of Example 10, but worse than those of Example 1 and Example 11, indicating that there is a synergistic effect between xanthan gum and starch. A network structure is formed between xanthan gum and starch, thereby improving the viscosity and cohesion of the system, making the mixed liquid more adhesive, and subsequently spraying it on the surface of the ceramic particles, thereby improving the connectivity between the ceramic powder and the carbon nanotubes, thereby improving the corresponding properties of the ceramic particles.
[0090] In Comparative Example 1, no modified basalt fiber is added to the shell raw material. It can be seen from Table 1 that compared with Example 1, the tensile strength is 5.1 MPa, the flexural strength is 20.2 MPa, the impact strength is 4.0 J / m, the elongation at break is 110%, and the abrasion rate is 35 mg, indicating that the modified basalt fiber of the present application has good mechanical strength, heat resistance, and corrosion resistance. When mixed with nitrile rubber and styrene-acrylic resin, the mechanical properties of the shell can be increased, so that the shell has good tensile properties, impact resistance and other mechanical properties.
[0091] In Comparative Example 2, an equal amount of modified basalt fiber in the shell raw material is replaced by basalt fiber. It can be seen from Table 1 that compared with Example 1, the tensile strength is 6.5 MPa, the flexural strength is 21.5 MPa, the impact strength is 6.2 J / m, the elongation at break is 120%, and the abrasion rate is 32 mg, indicating that the modified basalt fiber prepared in this application has good mechanical properties, which is subsequently applied to the shell, thereby improving the mechanical properties of the shell.
[0092] In Comparative Example 3, no modified ceramic particles are added to the shell raw material. It can be seen from Table 1 that compared with Example 1, the tensile strength is 5.7 MPa, the flexural strength is 20.6 MPa, the impact strength is 5.1 J / m, the elongation at break is 115%, and the abrasion rate is 34 mg, indicating that the modified ceramic particles of the present application have filling and adsorption effects, and are mixed with nitrile rubber, styrene acrylic resin and modified basalt fiber to improve the strength, heat resistance, corrosion resistance, wear resistance and weather resistance of the shell.
[0093] In Comparative Example 4, an equal amount of ceramic particles are used to replace the modified ceramic particles in the shell raw material. It can be seen from Table 1 that compared with Example 1, the tensile strength is 6.9 MPa, the flexural strength is 21.8 MPa, the impact strength is 6.7 J / m, the elongation at break is 124%, and the abrasion rate is 31 mg, indicating that the modified ceramic particles prepared in the present application have good mechanical properties, which are subsequently applied to the shell, thereby improving the mechanical properties of the shell.
[0094] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A process for preparing a counterweight, characterized in that: The steps include: (1) Cutting the steel to obtain a counterweight block, grinding and drilling the counterweight block, and then sandblasting the counterweight block to obtain a processed counterweight block; (2) Mixing nitrile rubber, styrene acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent, stearic acid and dipentadienyl vulcanizing agent to obtain a shell, and placing the treated counterweight obtained in step (1) into the shell to obtain a counterweight.
2. The process for preparing a counterweight according to claim 1, characterized in that: The nitrile rubber comprises 70-80 parts, styrene-acrylic resin comprises 40-50 parts, anti-aging agent comprises 1-2 parts, modified basalt fiber comprises 20-30 parts, modified ceramic particles comprises 10-20 parts, silane coupling agent comprises 5-9 parts, stearic acid comprises 2-5 parts and dipentadienyl vulcanizing agent comprises 1-3 parts.
3. The process for preparing a counterweight according to claim 1, characterized in that: The preparation method of the shell comprises the following steps: mixing and kneading nitrile rubber, styrene-acrylic resin, anti-aging agent, modified basalt fiber, modified ceramic particles, silane coupling agent and stearic acid, kneading for 30-35 minutes at a temperature of 70-80°C, adding a dipentadienyl vulcanizing agent, heating to 180-190°C, vulcanizing for 1-2 hours, and then compression molding to obtain the shell.
4. The process for preparing a counterweight according to claim 1, characterized in that: The preparation method of the modified basalt fiber comprises the following steps: (1) Dispersing the basalt fiber in a hydrochloric acid solution, stirring for 1-2 hours, washing with water, and then dispersing it in a silane coupling agent aqueous solution, continuing to stir for 20-30 minutes, filtering, and drying to obtain pretreated basalt fiber; (2) dispersing graphene in anhydrous ethanol, ultrasonicating for 1-2 hours, adding amino acids to obtain a mixed solution, stirring for 1-2 hours, and then extracting the basalt fiber treated in step (1) into the mixed solution, and drying the basalt fiber after extraction to obtain a mixture; (3) Dispersing chitosan in acetic acid solution, stirring for 10-20 minutes, and then spraying the mixture on the surface of step (2) to obtain modified basalt fiber.
5. The process for preparing a counterweight according to claim 4, characterized in that: The mass ratio of the basalt fiber, graphene, amino acid and chitosan is 1g:10-15mg:4-7g:0.3-0.6g.
6. The process for preparing a counterweight according to claim 4, characterized in that: In step (2), the basalt fiber is immersed in the mixed solution and extracted 2-3 times, each time being immersed in the mixed solution for 50-60 seconds, and the basalt fiber is dried after each extraction to obtain a mixture.
7. The process for preparing a counterweight according to claim 1, characterized in that: The preparation method of the modified ceramic particles comprises the following steps: (1) Crush and grind the ceramic particles, disperse them in a sodium hydroxide solution, stir for 1-2 hours, filter, and dry to obtain a pretreated ceramic powder; (2) dispersing the ceramic powder obtained in step (1) in deionized water, adding carbon nanotubes, ultrasonicating for 1-2 hours, and then filtering to obtain a mixture; (3) Dissolve xanthan gum in deionized water, stir at a temperature of 80-85° C. for 1-2 hours, add starch, continue stirring to obtain a mixed solution, and then spray the mixed solution on the surface of the mixture in step (2), dry, and obtain modified ceramic particles.
8. The process for preparing a counterweight according to claim 7, characterized in that: The mass ratio of the ceramic particles, carbon nanotubes and mixed liquid is 1:0.7-0.9:0.4-0.
6.
9. The process for preparing a counterweight according to claim 7, characterized in that: The mass ratio of the xanthan gum to the starch is 1:0.2-0.
4.