Earphone sleeve and base material attached composite fabric and processing technology thereof
By modifying imidyl alcohol, fluorosilicone modified chain extender and modified cellulose nanocrystal, the problem of deformation and adhesive residue of the headphone sleeve is solved, and the headphone sleeve and substrate are realized Stable fit and high-quality processing.
Patent Information
- Application Number
- CN202410929725.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The headphone cover fabric is easily deformed due to extrusion during transportation, and the residual problems of existing adhesives affect product quality and subsequent use.
Adhesives composed of modified imidyl alcohol, fluorosilic modified chain extender and modified cellulose nanocrystals are used to reduce deformation by applying adhesive on the base material fabric and bonding with the headphone cover fabric. and binder residue.
It improves the thermal stability and bonding performance of the adhesive, reduces the residue of the adhesive during separation, and ensures the fixing effect between the headphone sleeve and the substrate and the quality of subsequent processing.
Abstract
Description
Technical Field
[0001] The present application relates to the field of composite fabric preparation, and in particular to a composite fabric formed by laminating an earphone cover to a substrate and a processing technology thereof. Background Art
[0002] Earphone covers are an accessory for earphones that are comfortable, fit the ears, and provide nearly sealed music output. The fabric used for earphone covers has a certain degree of elasticity, so it is easily squeezed and deformed during rolling, storage, and transportation, affecting product quality.
[0003] Therefore, during the processing, the earphone cover fabric needs to be bonded to the base fabric that is not easily deformed, so as to reduce the deformation of the earphone cover fabric during transportation. However, the existing adhesive has a residual problem. When the earphone cover is separated from the base fabric, it is easy for the adhesive to remain on the earphone cover, affecting subsequent use, so it needs to be improved. Summary of the invention
[0004] In order to reduce adhesive residue when an earphone cover is separated from a substrate, the present application provides a composite fabric for bonding an earphone cover to a substrate and a processing technology thereof.
[0005] The present application provides a composite fabric of an earphone cover and a substrate, and a processing technology thereof, which adopts the following technical solutions: In the first aspect, the present application provides a composite fabric of an earphone cover and a substrate, which adopts the following technical solutions: A composite fabric of an earphone cover and a substrate, the composite fabric of an earphone cover and a substrate comprising an earphone cover fabric, an adhesive layer and a substrate fabric, the adhesive layer is obtained by coating an adhesive on the substrate fabric, and the adhesive comprises the following components in parts by mass: Modified imide alcohol 10-20 parts Polyether diol 20-30 parts Isocyanate 15-25 parts 3-5 parts of fluorosilicone modified chain extender 5-10 parts of modified cellulose nanocrystals 30-40 parts of solvent Catalyst 0.1-0.2 parts Additive 0.5-1 part.
[0006] Modified imido alcohol can introduce imido structure into the adhesive, and the imido group can improve the thermal stability of the adhesive, thereby improving the adhesive performance of the adhesive and reducing the adhesive residue; fluorosilicone modified chain extender can introduce fluorine and silicon elements into the adhesive, reduce the surface energy of the adhesive, and reduce the adhesive residue; modified cellulose nanocrystals can reinforce the defects between adhesive molecules and improve its stability, thereby reducing the residue when the adhesive is removed; the composite fabric of the earphone cover and the substrate has a good fixing effect, which can reduce the deformation effect of external force on the earphone cover fabric. The adhesive has good bonding performance and stability. The adhesive is not easy to remain during separation, reducing the impact on subsequent processing and use.
[0007] Preferably, the raw materials for preparing the modified imide alcohol include maleopimaric anhydride, monoethanolamine and furfuryl alcohol.
[0008] Preferably, the raw materials for preparing the maleopimaric anhydride include rosin and maleic anhydride.
[0009] The maleic rosin anhydride obtained by modifying maleic anhydride with rosin has abundant active groups, which can improve the bonding performance and stability of the adhesive; maleic pimaric anhydride can be further reacted with monoethanolamine and furfuryl alcohol to obtain alcohol with an imide group, and the alcohol hydroxyl group can react with isocyanate to introduce the imide group into the adhesive molecule, thereby improving its stability and reducing the occurrence of residual phenomenon.
[0010] Preferably, the raw materials for preparing the fluorosilicone modified chain extender include nanofiller, perfluorosilane and long-chain diamine.
[0011] The nanofiller is initially modified by perfluorosilane, which reacts with the hydroxyl groups on the nanofiller to increase the active groups on the surface of the nanofiller. It is then further modified by long-chain diamine, which reacts with perfluorosilane to amino-modify the nanofiller, so that the nanofiller has long amino chains, which can be used as a chain extender to extend the adhesive and improve the stability of the adhesive molecules. The fluorosilicone-modified chain extender has good hydrophobicity and reaction properties, and can produce a rough microphase structure on the surface of the adhesive layer, reduce the surface energy, and make some areas of the adhesive layer surface have strong bonding and some areas weaker, thereby reducing the adhesive residue during separation while ensuring the bonding performance.
[0012] Preferably, the mass ratio of the nanofiller, perfluorosilane and long-chain diamine is (2-3):1:1.5.
[0013] The fluorosilicone modified chain extender prepared according to the above mass ratio has good reactivity, can improve the stability and bonding performance of the adhesive, and reduce the residue of the adhesive.
[0014] Preferably, the raw materials for preparing the modified cellulose nanocrystals include esterified cellulose nanocrystals and phenolamines.
[0015] Preferably, the raw materials for preparing the esterified cellulose nanocrystals include cellulose nanocrystal bodies and long-chain alkyl acids.
[0016] Preferably, the raw materials for preparing the phenolamine include catechol and triethylenediamine.
[0017] The esterified cellulose nanocrystals are modified with long-chain alkyl acids and have good hydrophobic properties. The phenolamine generated by the reaction of catechol and triethylenediamine has high reactivity and can further modify the esterified cellulose nanocrystals to reinforce the cellulose nanocrystals and improve their thermal stability, while making them have a mussel-like bionic effect and improving their adhesion properties. By doping the modified cellulose nanocrystals into the adhesive molecules, the defects of the molecular structure can be reinforced and their thermal stability can be improved. By combining the hydrophobic effect of the modified cellulose nanocrystals with the mussel bionic effect, the adhesion properties can be improved while reducing the residue during separation, and the fluorosilicone modified chain extender can be synergistically used to improve the adhesion and stability of the adhesive.
[0018] Preferably, the mass ratio of the esterified cellulose nanocrystals, catechol and triethylenediamine is (6-10):1:1.2.
[0019] The modified cellulose nanocrystals prepared according to the above mass ratio have good hydrophobicity, adhesion performance and thermal stability.
[0020] In the second aspect, the present application provides a processing technology for bonding a composite fabric between an earphone cover and a substrate, using the following technical solution: A processing technology for bonding a composite fabric of an earphone cover and a substrate, comprising the following steps: The modified imide alcohol and the polyether polyol are heated for decompression dehydration, and after cooling, anhydrous modified imide alcohol and anhydrous polyether polyol are obtained; the anhydrous modified imide alcohol, anhydrous polyether polyol, a solvent, a fluorosilicone modified chain extender and an auxiliary agent are heated, mixed and stirred to obtain a monomer mixture, isocyanate is added to the monomer mixture, the temperature is increased to react to obtain a prepolymer, a catalyst and modified cellulose nanocrystals are added to the prepolymer to react, and an adhesive is obtained after decompression degassing; the adhesive is coated on the surface of the substrate fabric to obtain an adhesive layer, and after the earphone cover fabric is bonded to the adhesive layer, it is pressed to obtain a composite fabric bonded with the earphone cover and the substrate.
[0021] The composite fabric of the earphone cover and the substrate prepared according to the above steps has a good fixing effect, can reduce the deformation effect of external force on the earphone cover fabric, and the adhesive is not easy to remain during separation, reducing the impact on subsequent processing and use.
[0022] In summary, the present application includes at least one of the following beneficial technical effects: 1. Modified imido alcohol can introduce imido structure into the adhesive. The imido group can improve the thermal stability of the adhesive, thereby improving the adhesive performance of the adhesive and reducing the adhesive residue. Fluorosilicone modified chain extender can introduce fluorine and silicon elements into the adhesive, reduce the surface energy of the adhesive, and reduce the adhesive residue. Modified cellulose nanocrystals can reinforce the defects between adhesive molecules and improve its stability, thereby reducing the residue when the adhesive is removed. The composite fabric of the earphone cover and the substrate has a good fixing effect, which can reduce the deformation effect of external force on the earphone cover fabric. The adhesive has good bonding performance and stability. The adhesive is not easy to remain during separation, reducing the impact on subsequent processing and use.
[0023] 2. The nanofiller is initially modified by perfluorosilane, which reacts with the hydroxyl groups on the nanofiller to increase the active groups on the surface of the nanofiller. The nanofiller is then further modified by long-chain diamine, which reacts with perfluorosilane to amino-modify the nanofiller, so that the nanofiller has long amino chains, which can be used as a chain extender to extend the adhesive and improve the stability of the adhesive molecules. The fluorosilicone-modified chain extender has good hydrophobicity and reaction properties, and can produce a rough microphase structure on the surface of the adhesive layer, reduce the surface energy, and make some areas of the adhesive layer have strong bonding force, while others are weak, thereby reducing the adhesive residue during separation while ensuring the bonding performance.
[0024] 3. Esterified cellulose nanocrystals are modified with long-chain alkyl acids and have good hydrophobic properties. The phenolamine generated by the reaction of catechol and triethylenediamine has high reactivity and can further modify the esterified cellulose nanocrystals to reinforce the cellulose nanocrystals and improve their thermal stability, while making them have a mussel-like bionic effect and improving their adhesion properties. By doping the modified cellulose nanocrystals into the adhesive molecules, the defects of the molecular structure can be reinforced and their thermal stability can be improved. By combining the hydrophobic effect of the modified cellulose nanocrystals with the mussel bionic effect, the adhesion properties can be improved while reducing the residue during separation, and the fluorosilicone modified chain extender can be synergistically used to improve the adhesion and stability of the adhesive. DETAILED DESCRIPTION
[0025] The embodiments and preparation examples of the present application disclose a composite fabric for bonding an earphone cover to a substrate and a processing technology thereof. The raw materials used in the present application can be obtained from commercially available raw materials unless otherwise specified. The present application is further described in detail below in conjunction with the embodiments: Raw materials description: rosin (CAS No.: 8050-09-7), maleic anhydride (CAS No.: 108-31-6), dibutyltin dilaurate (CAS No.: 77-58-7), turpentine (CAS No.: 8006-64-2), furan (CAS No.: 110-00-9), monoethanolamine (CAS No.: 141-43-5), triethylamine (CAS No.: 121-44-8), xylene (CAS No.: 1330- 20-7), hydroquinone (CAS No.: 123-31-9), furfuryl alcohol (CAS No.: 98-00-0), nano filler is nano titanium dioxide, purchased from Ningbo Jiwei Nano New Material Technology Co., Ltd., perfluorosilane is (3,3,3-trifluoropropyl) dichloromethyl silane (CAS No.: 675-62-7), toluene (CAS No.: 108-88-3), long chain diamine is 1,7-heptanediamine (CAS No.: 646-19-5), Cellulose nanocrystals were purchased from Xi'an Qiyue Biotechnology Co., Ltd. Stearic acid (CAS No.: 57-11-4), catechol (CAS No.: 120-80-9), triethylenediamine (CAS No.: 280-57-9), polyether polyol (CAS No.: 9003-11-6), solvent is dimethyl carbonate (CAS: 616-38-6), auxiliary agent is antioxidant 1010 (CAS No.: 6683-19-8), isocyanate is Isophorone diisocyanate (CAS No.: 4098-71-9), catalyst is dibutyltin dilaurate (CAS No.: 77-58-7), methyltriethoxysilane (CAS No.: 2031-67-6), ethylenediamine (CAS No.: 107-15-3), polyester diol (CAS No.: 68082-28-0), 3,3'-dichloro-4,4'-diaminodiphenylmethane (CAS No.: 101-14-4).
[0026] Preparation Example 1 Preparation of modified imido alcohol 60.4 kg of rosin, 11.53 kg of maleic anhydride and 1.2 kg of dibutyltin dilaurate were mixed and dispersed, ammonia was introduced for 15 minutes, and then the material was heated to melt, then stirred at a speed of 200 rpm and heated to 180°C. After reacting at 180°C for 4 hours, the product was cooled to 110°C and poured into turpentine oil, crystallized at room temperature, and the crystals were filtered and washed with ethanol for 3 times. The washed crystals were dried in a vacuum oven at 60°C to obtain maleopimaric anhydride.
[0027] 30 kg of maleopimaric anhydride was dissolved in 100 L of acetone to obtain a maleopimaric anhydride solution, 34.6 kg of furan was added to the maleopimaric anhydride solution within 2 hours, and the mixture was stirred at 200 rpm under nitrogen protection for 12 hours to obtain a product mixture, the product mixture was vacuum filtered to obtain a product precipitate, the product precipitate was washed with ether and then vacuum dried in an oven at 60°C to obtain an intermediate product. 30 kg of the intermediate product was dissolved in 100 L of acetone to obtain an intermediate product solution, 22 kg of monoethanolamine and 36 kg of triethylamine were dissolved in 100 L of acetone to obtain an alcohol ammonia solution, the alcohol amine solution was added to the intermediate product solution under nitrogen protection and ice bath conditions, and the addition was completed within 2 hours to obtain a mixed reaction solution, the mixed reaction solution was gradually heated to 90 ° C and refluxed for 4 hours, and after the reaction was completed, it was cooled to 30 ° C to start crystallization, and after the crystallization was completed, vacuum filtration was obtained to obtain a crystalline product, the crystalline product was washed with isopropanol, and then dried in a vacuum oven at 60 ° C to obtain a second intermediate product. 40 kg of the second intermediate product, 220 kg of xylene and 5 g of hydroquinone were mixed, refluxed for 3 hours at 130 ° C under nitrogen protection, and the reflux was cancelled and the reaction was continued for 1 hour, and the mixture was cooled to 30 ° C to start crystallization, and a crude product was obtained by vacuum filtration, and the crude product was washed with xylene, and dried in a vacuum oven at 60 ° C to obtain maleopimaric imide.
[0028] 30 kg of maleopimaric acid imide and 6.6 kg of furfuryl alcohol were mixed and dispersed in 100 L of toluene, and refluxed at 80° C. for 12 h to obtain a mixture solution. The mixture solution was vacuum filtered, washed with ether, and dried in a vacuum oven at 60° C. to obtain a modified imido alcohol.
[0029] Example 1 Preparation of fluorosilicone modified chain extender 4.45 kg of nano titanium dioxide and 2.22 kg of (3,3,3-trifluoropropyl)dichloromethylsilane were mixed and dispersed in 200 L of toluene, stirred at 200 rpm for 2 h, then 1.2 L of deionized water was added, and the mixture was stirred and reacted at 200 rpm in a water bath at 80 ° C for 4 h, and then 3.33 kg of 1,7-heptanediamine was added. After stirring and reacting at 200 rpm in a water bath at 80 ° C for 4 h, the obtained product solution was filtered to obtain a filtrate, and the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80 ° C for 6 h to obtain a fluorosilicone modified chain extender.
[0030] Preparation of modified cellulose nanocrystals 20 kg of cellulose nanocrystals were dispersed in 50 L of deionized water to obtain a nanocrystal suspension, and then 25 L of anhydrous ethanol was added for ultrasonic dispersion for 30 min, and then 40 kg of stearic acid was added and ultrasonic dispersion was continued for 30 min to obtain a suspension reaction liquid. The suspension reaction liquid was stirred at 80 ° C at a speed of 200 rpm for 8 h, and then cooled to 30 ° C for 4 h. Anhydrous ethanol was added to terminate the reaction, and a solid product was obtained by centrifugation. The solid product was washed three times with anhydrous ethanol, and the washed solid product was dried in a 60 ° C forced air drying oven to obtain esterified cellulose nanocrystals.
[0031] 2.44 kg of catechol was dispersed in 30 L of deionized water, and stirred at 200 rpm until completely dissolved to obtain a catechol solution. 2.93 kg of triethylenediamine was added to the catechol solution, and stirred at 200 rpm for 10 min. A 1 mol / L sodium hydroxide aqueous solution was used to adjust the pH to 10.5 to obtain a phenolamine solution. 14.63 kg of esterified cellulose nanocrystals were added to the phenolamine solution, and stirred at 200 rpm for 2 h. After filtering, the modified cellulose nanocrystals were dried in a 60°C forced air drying oven to obtain modified cellulose nanocrystals.
[0032] Preparation of composite fabrics for bonding earphone sleeves and substrates The modified imide alcohol and polyether polyol prepared in Preparation Example 1 were heated to 100°C for decompression dehydration, and cooled to 60°C to obtain anhydrous modified imide alcohol and anhydrous polyether polyol; 10kg of anhydrous modified imide alcohol, 20kg of anhydrous polyether polyol, 30kg of solvent, 3kg of fluorosilicone modified chain extender and 0.5kg of auxiliary agent were mixed and stirred at 60°C at a speed of 200rpm to obtain a monomer mixture, 15kg of isocyanate was added to the monomer mixture, the temperature was raised to 80°C for reaction for 6h, and a prepolymer was obtained, 0.1kg of catalyst and 5kg of modified cellulose nanocrystals were added to the prepolymer, the reaction was continued for 2h, and the adhesive was obtained after decompression degassing for 4h. The adhesive was coated on the surface of the substrate fabric to obtain an adhesive layer, and the headphone cover fabric was bonded to the adhesive layer, and then pressed to obtain a composite fabric bonded with the headphone cover and the substrate.
[0033] Example 2 Preparation of fluorosilicone modified chain extender 5.45 kg of nano titanium dioxide and 1.82 kg of (3,3,3-trifluoropropyl)dichloromethylsilane were mixed and dispersed in 200 L of toluene, stirred at 200 rpm for 2 h, then 1.2 L of deionized water was added, and the mixture was stirred and reacted at 200 rpm in a water bath at 80 ° C for 4 h, and then 2.73 kg of 1,7-heptanediamine was added, and the mixture was stirred and reacted at 200 rpm in a water bath at 80 ° C for 4 h, and the obtained product solution was filtered to obtain a filtrate, and the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80 ° C for 6 h to obtain a fluorosilicone modified chain extender.
[0034] Preparation of modified cellulose nanocrystals 20 kg of cellulose nanocrystals were dispersed in 50 L of deionized water to obtain a nanocrystal suspension, and then 25 L of anhydrous ethanol was added for ultrasonic dispersion for 30 min, and then 40 kg of stearic acid was added and ultrasonic dispersion was continued for 30 min to obtain a suspension reaction liquid. The suspension reaction liquid was stirred at 80 ° C at a speed of 200 rpm for 8 h, and then cooled to 30 ° C for 4 h. Anhydrous ethanol was added to terminate the reaction, and a solid product was obtained by centrifugation. The solid product was washed three times with anhydrous ethanol, and the washed solid product was dried in a 60 ° C forced air drying oven to obtain esterified cellulose nanocrystals.
[0035] 1.64 kg of catechol was dispersed in 30 L of deionized water, and stirred at 200 rpm until completely dissolved to obtain a catechol solution. 1.97 kg of triethylenediamine was added to the catechol solution, and stirred at 200 rpm for 10 min. A 1 mol / L sodium hydroxide aqueous solution was used to adjust the pH to 10.5 to obtain a phenolamine solution. 16.39 kg of esterified cellulose nanocrystals were added to the phenolamine solution, and stirred at 200 rpm for 2 h. After filtering, the modified cellulose nanocrystals were dried in a 60°C forced air drying oven to obtain modified cellulose nanocrystals.
[0036] Preparation of composite fabrics for bonding earphone sleeves and substrates The modified imide alcohol and polyether polyol prepared in Preparation Example 1 were heated to 100°C for decompression dehydration, and cooled to 60°C to obtain anhydrous modified imide alcohol and anhydrous polyether polyol; 20kg of anhydrous modified imide alcohol, 30kg of anhydrous polyether polyol, 40kg of solvent, 5kg of fluorosilicone modified chain extender and 1kg of auxiliary agent were mixed and stirred at 60°C at a speed of 200rpm to obtain a monomer mixture, 25kg of isocyanate was added to the monomer mixture, the temperature was raised to 80°C for reaction for 6h, and a prepolymer was obtained, 0.2kg of catalyst and 10kg of modified cellulose nanocrystals were added to the prepolymer, the reaction was continued for 2h, and the adhesive was obtained after decompression degassing for 4h. The adhesive was coated on the surface of the substrate fabric to obtain an adhesive layer, and the headphone cover fabric was bonded to the adhesive layer, and then pressed to obtain a composite fabric bonded with the headphone cover and the substrate.
[0037] Example 3 Preparation of fluorosilicone modified chain extender 5 kg of nano titanium dioxide and 2 kg of (3,3,3-trifluoropropyl)dichloromethylsilane were mixed and dispersed in 200 L of toluene, stirred at 200 rpm for 2 h, then 1.2 L of deionized water was added, and the mixture was stirred and reacted at 200 rpm in a water bath at 80 ° C for 4 h, and then 3 kg of 1,7-heptanediamine was added. After stirring and reacting at 200 rpm in a water bath at 80 ° C for 4 h, the obtained product solution was filtered to obtain a filtrate, and the filtrate was washed with anhydrous ethanol, and the washed filtrate was dried in an oven at 80 ° C for 6 h to obtain a fluorosilicone modified chain extender.
[0038] Preparation of modified cellulose nanocrystals 20 kg of cellulose nanocrystals were dispersed in 50 L of deionized water to obtain a nanocrystal suspension, and then 25 L of anhydrous ethanol was added for ultrasonic dispersion for 30 min, and then 40 kg of stearic acid was added and ultrasonic dispersion was continued for 30 min to obtain a suspension reaction liquid. The suspension reaction liquid was stirred at 80 ° C at a speed of 200 rpm for 8 h, and then cooled to 30 ° C for 4 h. Anhydrous ethanol was added to terminate the reaction, and a solid product was obtained by centrifugation. The solid product was washed three times with anhydrous ethanol, and the washed solid product was dried in a 60 ° C forced air drying oven to obtain esterified cellulose nanocrystals.
[0039] 1.96 kg of catechol was dispersed in 30 L of deionized water, and stirred at 200 rpm until completely dissolved to obtain a catechol solution. 2.35 kg of triethylenediamine was added to the catechol solution, and stirred at 200 rpm for 10 min. A 1 mol / L sodium hydroxide aqueous solution was used to adjust the pH to 10.5 to obtain a phenolamine solution. 15.69 kg of esterified cellulose nanocrystals were added to the phenolamine solution, and stirred at 200 rpm for 2 h. After filtering, the modified cellulose nanocrystals were dried in a 60°C forced air drying oven to obtain modified cellulose nanocrystals.
[0040] Preparation of composite fabrics for bonding earphone sleeves and substrates The modified imide alcohol and polyether polyol prepared in Preparation Example 1 were heated to 100°C for decompression dehydration, and cooled to 60°C to obtain anhydrous modified imide alcohol and anhydrous polyether polyol; 15kg of anhydrous modified imide alcohol, 25kg of anhydrous polyether polyol, 35kg of solvent, 4kg of fluorosilicone modified chain extender and 0.75kg of auxiliary agent were mixed and stirred at 60°C at a speed of 200rpm to obtain a monomer mixture, 20kg of isocyanate was added to the monomer mixture, the temperature was raised to 80°C for reaction for 6h, and a prepolymer was obtained, 0.15kg of catalyst and 7.5kg of modified cellulose nanocrystals were added to the prepolymer, and the reaction was continued for 2h, and the adhesive was obtained after decompression degassing for 4h. The adhesive was coated on the surface of the substrate fabric to obtain an adhesive layer, and the headphone cover fabric was bonded to the adhesive layer, and then pressed to obtain a composite fabric bonded with the headphone cover and the substrate.
[0041] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, the amount of nanofiller used is 3.75 kg, the amount of perfluorosilane used is 2.5 kg, and the amount of long-chain diamine used is 3.75 kg.
[0042] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the amount of nanofiller used is 5.83 kg, the amount of perfluorosilane used is 1.67 kg, and the amount of long-chain diamine used is 2.5 kg.
[0043] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, perfluorosilane is replaced by methyltriethoxysilane when preparing the fluorosilicone modified chain extender.
[0044] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that in Example 7, the long-chain diamine is replaced by ethylenediamine when preparing the fluorosilicone modified chain extender.
[0045] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that maleopimaric anhydride is replaced by maleic anhydride when preparing the modified imido alcohol in Example 8.
[0046] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, the amount of esterified cellulose nanocrystals used is 12.9 kg, the amount of catechol used is 3.23 kg, and the amount of triethylenediamine used is 3.87 kg.
[0047] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, the amount of esterified cellulose nanocrystals used is 16.9 kg, the amount of catechol used is 1.41 kg, and the amount of triethylenediamine used is 1.69 kg.
[0048] Embodiment 11 Example 11 is based on Example 3. The only difference between Example 11 and Example 3 is that in Example 11, the esterified cellulose nanocrystals used in preparing the modified cellulose nanocrystals are replaced with cellulose nanocrystals.
[0049] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that in Example 12, the phenolamine used in preparing modified cellulose nanocrystals is replaced by catechol.
[0050] Example 13 Example 13 is based on Example 3. The only difference between Example 13 and Example 3 is that in Example 13, the phenolamine used in preparing modified cellulose nanocrystals is replaced by triethylenediamine.
[0051] Comparative Example 1 Comparative Example 1 is based on Example 3, and the only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, the modified imide alcohol is replaced by polyester diol.
[0052] Comparative Example 2 Comparative Example 2 is based on Example 3. The only difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the fluorosilicone modified chain extender is replaced by 3,3'-dichloro-4,4'-diaminodiphenylmethane.
[0053] Comparative Example 3 Comparative Example 3 is based on Example 3, and the only difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, the modified cellulose nanocrystals are replaced by cellulose nanocrystals.
[0054] Performance testing (1) GB / T2792-2014 Test method for peel strength of adhesive tape was selected as the standard, and the 180° peel strength of the adhesive was tested using a desktop tensile testing machine. Three samples were prepared for each test specimen, and the average value was taken after measurement. The results were recorded in Table 1.
[0055] (2) Residue test: 10 samples of 20 cm*20 cm were cut from the composite fabric, the earphone cover fabric was separated from the base fabric, and the adhesive residue was observed. The results are recorded in Table 1.
[0056] Table 1 Test results of peeling force and adhesive residue of composite fabrics Test results Peel force (N / 25mm) Binder residue Example 1 20.3 No residue Example 2 20.6 No residue Example 3 21.1 No residue Example 4 18.7 No residue Example 5 19.3 No residue Example 6 20.2 A small amount of residue Example 7 18.2 No residue Example 8 17.6 A small amount of residue Example 9 20.5 A small amount of ginseng remains Example 10 15.4 No residue Embodiment 11 23.6 Some residue Example 12 17.2 No residue Example 13 18.3 No residue Comparative Example 1 23.2 Serious residual Comparative Example 2 19.9 Serious residual Comparative Example 3 17.8 Some residue It can be seen from Table 1 that the peeling force of Examples 1-3 is greater than 20.3N / 25mm, and there is no adhesive residue after separation. It can be seen that the adhesive prepared in the present application has good bonding performance and stability, can effectively bond composite fabrics, reduce fabric deformation, and achieve no adhesive residue, which is beneficial to subsequent processing and use.
[0057] As can be seen from Table 1, the only difference between Examples 4 and 5 and Example 3 is that the mass ratio of nanofiller, perfluorosilane and long-chain diamine in Example 4 is 1.5:1:1.5, and the mass ratio of nanofiller, perfluorosilane and long-chain diamine in Example 5 is 3.5:1:1.5. Compared with Example 3, the adhesion performance of Examples 4 and 5 is reduced; this is because the mass ratio of nanofiller, perfluorosilane and long-chain diamine is not within the specified range, so that the stability and reactivity of the fluorosilicone modified chain extender are reduced, thereby affecting the adhesion performance and stability of the adhesive.
[0058] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that: in Example 6, perfluorosilane is replaced by methyltriethoxysilane when preparing the fluorosilicone modified chain extender, and in Example 7, long-chain diamine is replaced by ethylenediamine when preparing the fluorosilicone modified chain extender. Compared with Example 3, the adhesion performance and stability of Examples 6 and 7 are reduced; this is because perfluorosilane is replaced by methyltriethoxysilane, lacking the introduction of fluorine atoms, the surface energy of the fluorosilicone modified chain extender is increased, and it is easy to have adhesive residues during separation; when the long-chain diamine is replaced by ethylenediamine, the reaction performance of the fluorosilicone modified chain extender is reduced due to the steric hindrance between molecules, thereby reducing the stability and adhesion performance.
[0059] As can be seen from Table 1, the only difference between Example 8 and Example 3 is that in Example 8, maleopimaric anhydride is replaced by maleic anhydride when preparing the modified imido alcohol. Compared with Example 3, Example 8 replaces maleopimaric anhydride with maleic anhydride, lacks the modification treatment of rosin, and the thermal stability and adhesion performance of the modified imido alcohol are reduced, thereby reducing the stability and adhesion performance of the adhesive.
[0060] As can be seen from Table 1, the only difference between Examples 9 and 10 and Example 3 is that the mass ratio of esterified cellulose nanocrystals, catechol and triethylenediamine in Example 9 is 4:1:1.2, and the mass ratio of esterified cellulose nanocrystals, catechol and triethylenediamine in Example 10 is 12:1:1.2. Compared with Example 3, the adhesion performance and stability of Examples 9 and 10 are reduced; this is because the mass ratio of esterified cellulose nanocrystals, catechol and triethylenediamine is not within the specified range, and too much or too little phenolamine grafting will affect the balance between the hydrophobic effect and the adhesion effect in the modified cellulose nanocrystals, thereby affecting its adhesion performance and stability.
[0061] As can be seen from Table 1, the only difference between Examples 11, 12, and 13 and Example 3 is that in Example 11, the esterified cellulose nanocrystals used in preparing the modified cellulose nanocrystals are replaced with cellulose nanocrystals, in Example 12, the phenolamines used in preparing the modified cellulose nanocrystals are replaced with catechol, and in Example 13, the phenolamines used in preparing the modified cellulose nanocrystals are replaced with triethylenediamine. Compared with Example 3, the adhesion performance and stability of Examples 11, 12, and 13 are reduced; this is because the esterified cellulose nanocrystals are replaced with cellulose nanocrystals, and the cellulose nanocrystals lack the modification treatment of long-chain alkyl acids, and the hydrophobic performance is reduced; if no catechol or triethylenediamine is added, the mussel biomimetic effect is weakened, and its adhesion performance is reduced. These changes will affect the interaction balance between the hydrophobic effect and the adhesion performance in the modified cellulose nanocrystals, thereby affecting the adhesion performance and stability of the binder, resulting in the presence of residues.
[0062] As can be seen from Table 1, the only difference between Comparative Example 1 and Example 3 is that: in Comparative Example 1, the modified imide alcohol is replaced by polyester diol. Compared with Example 3, the stability of Comparative Example 1 is significantly reduced and the residue is serious. This is because the modified imide alcohol is replaced by polyester diol. The polyester diol has good adhesion properties, but the heat resistance is worse than that of the modified imide alcohol, so that the stability is reduced and it is easier to produce residue during separation.
[0063] As can be seen from Table 1, the only difference between Comparative Example 2 and Example 3 is that: in Comparative Example 2, the fluorosilicone modified chain extender is replaced by 3,3'-dichloro-4,4'-diaminodiphenylmethane. Compared with Example 3, Comparative Example 2 replaces the fluorosilicone modified chain extender with a conventional chain extender. Although the presence of phenyl can improve the hydrophobic properties to a certain extent, the lack of the introduction of fluorine atoms and filler particles has limited effect on the reduction of surface energy, thereby affecting its stability and residual condition, and it is more likely to produce residues on the surface.
[0064] As can be seen from Table 1, the only difference between Comparative Example 3 and Example 3 is that the modified cellulose nanocrystals are replaced by cellulose nanocrystals in Comparative Example 3. Compared with Example 3, the adhesion performance and stability of Comparative Example 3 are significantly reduced; this is because the modified cellulose nanocrystals are replaced by cellulose nanocrystals, and the cellulose nanocrystals lack long-chain alkyl acid modification and phenolamine modification, and the hydrophobicity and adhesion properties are reduced, the adhesion performance of the binder is reduced, and the residual binder is increased.
[0065] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A composite fabric formed by laminating an earphone cover with a substrate, Features: The headphone cover and substrate laminated composite fabric comprises a headphone cover fabric, an adhesive layer and a substrate fabric, wherein the adhesive layer is obtained by coating an adhesive on the substrate fabric, and the adhesive comprises the following components in parts by weight: Modified imide alcohol 10-20 parts Polyether diol 20-30 parts Isocyanate 15-25 parts 3-5 parts of fluorosilicone modified chain extender 5-10 parts of modified cellulose nanocrystals 30-40 parts of solvent Catalyst 0.1-0.2 parts Additive 0.5-1 part.
2. The headphone cover and substrate laminated composite fabric according to claim 1, Features: The raw materials for preparing the modified imide alcohol include maleopimaric anhydride, monoethanolamine and furfuryl alcohol.
3. The composite fabric of the earphone cover and the base material according to claim 2, Features: The raw materials for preparing the maleopimaric anhydride include rosin and maleic anhydride.
4. The headphone cover and substrate laminated composite fabric according to claim 1, Features: The raw materials for preparing the fluorosilicone modified chain extender include nano filler, perfluorosilane and long-chain diamine.
5. The composite fabric of the earphone cover and the base material according to claim 2, Features: The mass ratio of the nanofiller, perfluorosilane and long-chain diamine is (2-3):1:1.
5.
6. The composite fabric of the earphone cover and the base material according to claim 1, Features: The raw materials for preparing the modified cellulose nanocrystals include esterified cellulose nanocrystals and phenolamines.
7. The composite fabric of the earphone cover and the base material according to claim 6, Features: The raw materials for preparing the esterified cellulose nanocrystals include cellulose nanocrystal bodies and long-chain alkyl acids.
8. The composite fabric of the earphone cover and the base material according to claim 7, Features: The raw materials for preparing the phenolamine include catechol and triethylenediamine.
9. The composite fabric of the earphone cover and the base material according to claim 8, Features: The mass ratio of the esterified cellulose nanocrystals, catechol and triethylenediamine is (6-10):1:1.
2.
10. A processing technology for bonding a composite fabric of an earphone cover and a substrate as claimed in claim 1, Features: Use the following steps: The modified imide alcohol and the polyether polyol are heated for decompression dehydration, and after cooling, anhydrous modified imide alcohol and anhydrous polyether polyol are obtained; the anhydrous modified imide alcohol, anhydrous polyether polyol, a solvent, a fluorosilicone modified chain extender and an auxiliary agent are heated, mixed and stirred to obtain a monomer mixture, isocyanate is added to the monomer mixture, the temperature is increased to react to obtain a prepolymer, a catalyst and modified cellulose nanocrystals are added to the prepolymer to react, and an adhesive is obtained after decompression degassing; the adhesive is coated on the surface of the substrate fabric to obtain an adhesive layer, and after the earphone cover fabric is bonded to the adhesive layer, it is pressed to obtain a composite fabric bonded with the earphone cover and the substrate.
Citation Information
Patent Citations
Super-soft protein synthetic leather elastique in four sides and resistant hydrolysis
CN108867085A
Cellulose nanocrystal reinforced self-repairing water-based polyurethane material and preparation method thereof
CN110028686A
Catecholamine-modified cellulose material as well as preparation method and application thereof in filter membrane
CN113045678A
Modified TPU, modified TPU synthetic leather and preparation method of modified TPU synthetic leather