High-strength, high-impact-resistance and high-barrier multilayer EVOH composite sheet as well as preparation method and application of high-strength, high-impact-resistance and high-barrier multilayer EVOH composite sheet

Through the multi-layer EVOH composite sheet structure and hot pressing preparation technology, the limitations of EVOH materials in the improvement of barrier properties and mechanical strength are solved, and the effects of high strength, high impact resistance and high barrier are achieved, suitable for packaging and mechanical parts and other fields.

CN118906595AActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310513102.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

Existing EVOH materials have limitations in improving barrier properties and mechanical strength, and the production process is complex and the improvement is limited.

Method used

Using a multi-layer EVOH composite sheet structure, including two outer layers and multiple core layers. The core layer improves the melting point gradient through tensile treatment, and the outer layer provides protection and enhances the material performance. It is prepared by hot pressing to achieve high strength and high strength. Impact resistance and high barrier effect.

Benefits of technology

The tensile strength, impact strength and peel strength of EVOH materials are significantly improved, while maintaining high gas barrier properties. The process is mature and can be produced in existing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004218496840000121
    Figure BDA0004218496840000121
  • Figure BDA0004218496840000131
    Figure BDA0004218496840000131
Patent Text Reader

Abstract

The invention relates to the field of polymer sheets, and discloses a high-strength, high-impact-resistance and high-barrier multilayer EVOH composite sheet as well as a preparation method and application thereof. The multilayer EVOH composite sheet comprises two outer layers A and a plurality of laminated core layers B located between the two outer layers A, and has a structure of AB1B2... BmA, m is an integer not less than 2; the two outer layers A are the same or different and respectively contain a polyolefin composition A; the core layers B respectively contain compositions B, and the compositions B are the same or different and respectively contain EVOH; the preparation process of the core layer B comprises a stretching step, and the stretching ratio is 1-15 times. According to the present invention, the multilayer EVOH composite sheet material has advantages of high gas barrier property, high tensile strength, high impact strength, and high peel strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer sheets, and more particularly to a high-strength, high-impact, high-barrier multi-layer EVOH composite sheet and a preparation method and application thereof. Background Art

[0002] Ethylene-vinyl alcohol copolymer (EVOH) is one of the synthetic resins with the best gas barrier properties so far. In addition to its excellent gas barrier properties, EVOH also has excellent oil resistance, organic solvent resistance and easy printability. Due to its thermal stability in combination with ethylene, multi-layer containers containing EVOH barrier layers are completely reusable. It is precisely these characteristics that plastic containers containing EVOH barrier layers can replace many glass and metal containers in food packaging.

[0003] With the implementation of plastic reduction policies at home and abroad in recent years, there is a need to further increase strength to reduce the thickness (weight) of packaging materials and improve barrier properties to extend the shelf life. Therefore, an EVOH material with higher strength and better barrier properties is needed. Patent document CN109705248A uses IIA group metal elements and EVOH to blend to obtain a composition with higher glass transition temperature, mechanical properties and barrier properties. Patent document CN113698695A discloses a composition composed of EVOH, manganese, boron, alkali metals, etc. By controlling the content of each component, the interaction between molecular hydrogen bonds, ionic bonds, etc. can be strengthened, and finally the gas barrier properties and gel behavior of the EVOH composition are enhanced. Patent document CN111993732A discloses a high-flatness, high-barrier, high-strength cooking-resistant stretch film, which comprises, from top to bottom, an outer layer, a first outer layer, a second outer layer, a first adhesive layer, a first PA layer, a high-barrier layer, a second PA layer, a second adhesive layer, a second heat-sealing layer, a first heat-sealing layer, and a heat-sealing layer. The outer layer, the first outer layer, and the second outer layer are all made of PP, the first adhesive layer and the second adhesive layer are made of polyethylene resin modified with maleic anhydride, the first PA layer and the second PA layer are made of PA, the high-barrier layer is made of EVOH, the second heat-sealing layer, the first heat-sealing layer, and the heat-sealing layer are all made of PE, and the product structure is PP / PP / PP / TIE / PA / EVOH / PA / TIE / PE / PE / PE, in which EVOH provides a high-barrier function and nylon provides a high-strength function.

[0004] From the perspective of existing technologies, most methods to improve the barrier properties of EVOH are blending and modification, and the method to improve the mechanical strength of EVOH is to introduce other materials such as nylon and polyamide for multi-layer composite. These methods have relatively complicated production processes and have limited effects on improving the strength, barrier properties and other properties of EVOH materials.

[0005] Therefore, how to provide an EVOH material with high strength, high impact resistance and high barrier properties is still a technical problem that needs to be solved in this field. Summary of the invention

[0006] In order to further solve the technical problems of barrier properties and mechanical strength of EVOH materials, the purpose of the present invention is to provide a high-strength, high-impact, high-barrier multilayer EVOH composite sheet and its preparation method and application. The multilayer EVOH composite sheet not only has high gas barrier properties, but also has high tensile strength and impact strength. In addition, the multilayer EVOH composite sheet also has high peel strength.

[0007] In a first aspect, the present invention provides a multilayer EVOH composite sheet, comprising two outer layers A and a plurality of laminated core layers B located between the two outer layers A, having AB1B2 ... B m A structure; m is an integer not less than 2; the two outer layers A are the same or different, and each contains a polyolefin composition A; the core layers B each contain a composition B, and the compositions B are the same or different, and each contains EVOH; the preparation process of the core layer B includes a stretching step, and the stretching ratio is 1-15 times.

[0008] According to the present invention, the melting point of the composition B can be selected within a wide range. In a preferred embodiment of the present invention, the melting point of the composition B is 150-210°C, preferably 160-200°C.

[0009] According to a preferred embodiment of the present invention, the core layer B contains only EVOH, that is, the composition B is EVOH.

[0010] According to the present invention, the material selection range of the EVOH is relatively wide. In a preferred embodiment of the present invention, the ethylene content in the EVOH is 15-50 mol%, preferably 21-49 mol%.

[0011] In a preferred embodiment of the present invention, the melt flow rate of the EVOH at 190° C. and a load of 2.16 kg is 1-50 g / 10 min, preferably 1-20 g / 10 min.

[0012] According to the present invention, the number m of the core layer B can be selected in a wide range. Preferably, m is 2-200, preferably 4-100.

[0013] In a preferred embodiment of the present invention, the multilayer EVOH composite sheet has AB1B2...B i …B n …B i…B2B1A lamellar structure, i and n are both integers not less than 2, and i≤n, n is 2-100, preferably 2-50.

[0014] According to the present invention, the multilayer EVOH composite sheet of the present invention has AB1B2...B m A structure, B1B2…B m The melting points can be the same or different, and the technical effects of the present invention can be achieved.

[0015] After research, the inventor of the present invention unexpectedly discovered that when B1B2…B m When the melting points are the same or arranged in a specific melting point gradient, the resulting multilayer EVOH composite sheet is better than B1B2…B m The case where the melting point is not arranged in a specific gradient manner has a better technical effect. Preferably, the composition B i Melting point ≥ composition B i+1 Melting point.

[0016] More preferably, composition B i Melting point > Composition B i+1 The melting point of B1B2...B m When the melting points are arranged according to a specific melting point gradient, compared to B1B2...B m The melting points are the same, and the technical effect is further improved. In particular, if the EVOH layer is subjected to the specific melting point gradient lamination hot pressing treatment of the present invention, the peel strength between the EVOH layers can be greatly improved. Further more preferably, the composition B i With composition B i+1 The melting point difference is 5-15°C.

[0017] According to the present invention, the stretching ratio can be selected within a wide range. In a preferred embodiment of the present invention, the stretching ratio is 2-15 times.

[0018] According to the present invention, preferably, the stretching method is a combination of one or more of free stretching, solid phase stretching and multi-stage stretching.

[0019] In a more preferred embodiment of the present invention, the stretching conditions in the preparation step of the core layer B include: the core layer B is prepared by extrusion molding, casting or calendering, and stretching of EVOH.

[0020] More preferably, the stretching conditions include: the stretching temperature is 140-185° C., preferably 150-175° C.; and the stretching ratio is 2-15 times.

[0021] The present invention does not limit the thickness of the high-strength, high-impact, high-barrier composite sheet, and can be selected in a wide range according to its actual application field. In a preferred embodiment of the present invention, the thickness of the multilayer EVOH composite sheet is 5-1000 μm, preferably 5-500 μm, and more preferably 5-300 μm.

[0022] According to the present invention, the total thickness of all core layers B in the thickness of the multi-layer EVOH composite sheet can be selected within a wide range. In a preferred embodiment of the present invention, taking the total thickness of the multi-layer EVOH composite sheet as 100%, the total thickness of all core layers B accounts for 10%-90% of the total thickness of the multi-layer EVOH composite sheet.

[0023] The thickness of the outer layer A on both sides of the core layer B may be the same or different, preferably the same.

[0024] According to the present invention, the thickness of layer A and layer B can be controlled by the melt pump of the extruder during the processing.

[0025] According to the present invention, the placement angle of the core layer B can be selected within a wide range. In a preferred embodiment of the present invention, the core layers B are stacked from top to bottom with an angle of 0-90° between the warp and the warp.

[0026] The outer layer A mainly plays the role of protecting the core layer BB. Because EVOH is relatively easy to absorb moisture, the outer composite layer A can effectively improve the service life. The material selection of layer A of the present invention is not strictly limited. According to the present invention, the two outer layers A are the same or different, and each contains a polyolefin composition A. In a preferred embodiment of the present invention, the polyolefin composition A contains polyolefin a and a thermal bonding enhancer b.

[0027] According to the present invention, the contents of polyolefin a and thermal adhesion enhancer b can be selected within a wide range. In a preferred embodiment of the present invention, taking the total weight of the polyolefin composition A as 100wt%, the polyolefin composition A contains 70-99wt% of polyolefin a and 1-30wt% of thermal adhesion enhancer b; preferably, the polyolefin composition A includes 80-99wt% of polyolefin a and 1-20wt% of thermal adhesion enhancer b.

[0028] According to the present invention, the polyolefin a can be selected from a wide range. In a preferred embodiment of the present invention, the polyolefin a is selected from one or more of polypropylene, polyethylene, and ethylene-vinyl acetate.

[0029] According to the present invention, the thermal adhesion enhancer b can be selected from a wide range. In a preferred embodiment of the present invention, the thermal adhesion enhancer b is selected from one or more of anhydride-modified polypropylene, anhydride-modified polyethylene, anhydride-modified ethylene-vinyl acetate, glycidyl methacrylate (GMA)-modified polypropylene, glycidyl methacrylate-modified polyethylene (i.e., GMA-modified polyethylene), glycidyl methacrylate-modified ethylene-vinyl acetate (i.e., GMA-modified ethylene-vinyl acetate), and maleic anhydride copolymers.

[0030] According to the present invention, the high-strength, high-impact and high-barrier multilayer EVOH composite sheet of the present invention can be prepared by a variety of methods. In a preferred embodiment of the present invention, the multilayer EVOH composite sheet is prepared by sequentially stacking an outer layer A, multiple core layers B and an outer layer A, and then laminating them.

[0031] In a more preferred embodiment of the present invention, the lamination method is first hot pressing and then cooling and shaping; further preferably, the multi-layer EVOH composite sheet is prepared by respectively extruding, casting or calendering, stretching and slitting the raw materials for forming the outer layer A and the raw materials for forming the core layer B to obtain corresponding sheets, and then stacking, hot pressing and cooling and shaping the corresponding sheets in a corresponding structural order.

[0032] The multilayer EVOH composite sheet of the present invention has at least one of the following characteristics:

[0033] The tensile strength of the multilayer EVOH composite sheet is 50-350 MPa, preferably 150-350 MPa;

[0034] The drop weight impact strength of the multi-layer EVOH composite sheet is 50-200 J, preferably 100-200 J;

[0035] The interlayer peel strength of the multilayer EVOH composite sheet is 1-2N / mm, preferably 1.2-2N / mm;

[0036] The oxygen permeability of the multilayer EVOH composite sheet is 0.1-20*10 -3 cm 3 / m 2 24h, preferably 0.1-10*10 -3 cm 3 / m 2 ·24h.

[0037] All parameters are obtained by directly testing the composite sheets in the corresponding embodiments and comparative examples according to the corresponding standards.

[0038] The detection methods of the above parameters include but are not limited to the methods described in the specific implementation methods of the present invention.

[0039] The second aspect of the present invention is to provide a method for preparing the multilayer EVOH composite sheet described in the first aspect, comprising respectively making the raw material for forming the outer layer A and the raw material for forming the core layer B into corresponding sheets A and B, and then stacking, hot pressing, and cooling the corresponding sheets according to the corresponding structural sequence; wherein the preparation process of the sheet B includes a stretching step, and the stretching ratio is 1-15 times.

[0040] In a preferred embodiment of the present invention, the step of preparing sheet A includes: melt blending the raw materials forming the outer layer A and preferably extruding them, and then casting or calendering, stretching, and slitting to obtain sheet A; the conditions and equipment for melt blending the raw materials forming the outer layer A adopt the conditions and equipment for melt blending of polyolefins in the prior art, and preferably, the equipment adopts a twin-screw extruder.

[0041] The extrusion molding and casting temperature selection range of the outer layer A of the present invention is relatively wide. In a preferred embodiment of the present invention, the co-extrusion molding and casting temperatures are independently selected from 200-250°C; the calendering temperature is 50-70°C.

[0042] The stretching conditions of the outer layer A have a wide selection range. In a preferred embodiment of the present invention, the stretching conditions include: the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching, preferably solid phase stretching, and / or multi-stage stretching, more preferably multi-stage stretching; the stretching temperature is 90-165°C, preferably 90-140°C; the stretching ratio is preferably 1-20 times, preferably 2-15 times.

[0043] In a preferred embodiment of the present invention, the step of preparing the core layer B comprises: extruding the raw material for forming the core layer B, and then casting or calendering, stretching, and slitting to obtain the sheet B.

[0044] In a more preferred embodiment of the present invention, the preparation conditions of the sheet B include: the temperatures of extrusion molding and casting are independently selected from 200-260°C; and the calendering temperature is 50-90°C.

[0045] According to the present invention, the preparation process of the core layer B includes a stretching step, and the stretching ratio is 1-15 times. For the stretching method, it can be selected from a variety of methods. Preferably, the stretching method of the sheet B is a combination of one or more of free stretching, solid phase stretching, and multi-stage stretching; more preferably, the stretching method is a combination of one or two of solid phase stretching and multi-stage stretching. Among them, the inventors found that solid phase stretching not only further improves the mechanical strength, but also helps to further improve the barrier properties.

[0046] The stretching conditions of the sheet B can be selected within a wide range. Preferably, the stretching temperature is 140-185°C, preferably 150-175°C; the stretching ratio is 1-15 times, preferably 2-15 times.

[0047] In a preferred embodiment of the present invention, the stacking method includes: from top to bottom, the sheets A and B are stacked in sequence with an angle of 0-90 degrees between the warp directions.

[0048] The inventors have found that after EVOH is stretched and strengthened, its mechanical strength and barrier properties will be significantly improved. After the multi-layer EVOH film is stacked, the directions perpendicular to the film can maintain their respective barrier properties. In the direction parallel to the film, since the multi-layer EVOH film is stacked at 0-90° between the warp and the warp, and the melting point of the EVOH film is arranged in a gradient, it can be easily bonded by hot pressing, so that the tensile strength, impact strength, peel strength and other mechanical properties of the multi-layer EVOH are greatly improved.

[0049] In a preferred embodiment of the present invention, the hot pressing temperature is 135-190°C, preferably 150-190°C.

[0050] In a preferred embodiment of the present invention, the hot pressing pressure is 2-10 MPa.

[0051] In a preferred embodiment of the present invention, the preheating time is 5-600 s, and / or the hot pressing time is 1-600 s, preferably 10-500 s.

[0052] In a preferred embodiment of the present invention, the cooling and shaping conditions include: a cooling pressure of 2-8 MPa, and / or a cooling time of 30-700 s.

[0053] In a more preferred embodiment of the present invention, the hot pressing conditions include: the hot pressing temperature is 135-190°C, preferably 150-190°C; and / or, the hot pressing pressure is 2-10MPa; and / or, the preheating time is 5-600s, and / or, the hot pressing time is 1-600s, preferably 10-500s; and / or, the cooling and shaping conditions include: the cooling pressure is 2-8MPa, and / or, the cooling time is 30-700s.

[0054] In a third aspect, the purpose of the present invention is to provide an application of the multilayer EVOH composite sheet described in the first aspect or the multilayer EVOH composite sheet obtained by the preparation method described in the second aspect in the fields of packaging, mechanical parts, and industrial and agricultural films.

[0055] When the composite sheet of the present invention is used for film packaging, it can also be further processed, such as stamping molding, blister molding, etc. The composite sheet of the present invention can be subjected to secondary molding processing according to application requirements.

[0056] As mentioned above, although the gas barrier properties and material strength of EVOH itself can meet the current use requirements, as people's living standards improve, these basic properties of EVOH need to be further improved. In the conventional understanding, although increasing the thickness of EVOH can improve the gas barrier properties, its tensile strength and impact strength are improved less. In particular, the existing packaging field generally requires packaging materials to have a lower thickness. Increasing the thickness of EVOH materials to increase their gas barrier properties is contrary to reducing the thickness. At the same time, in the conventional understanding, when EVOH is multi-layered, the multi-layered materials are often easy to peel off, which will cause the composite material to have new defects.

[0057] The multilayer EVOH composite sheet of the present invention changes the molding processing conditions by physical methods (the preparation process of the core layer B includes a stretching step with a stretching ratio of 1-15 times) to control the aggregate structure of the material, so that the multilayer EVOH composite sheet obtains an intrinsic reinforcement effect, that is, the mechanical properties of the material are greatly improved. The multilayer EVOH composite sheet of the present invention is prepared by a hot pressing method. During hot pressing, the surface of the multilayer sheet softens and the sheets are bonded to each other by intermolecular forces to provide interfacial adhesion. The inventor of the present invention surprisingly found through research that the multilayer EVOH composite sheet of the present invention has AB1B2…B i …B n …B i ...B2B1 sheet structure, preferably in the film layer B i Melting point of B ≥ B i+1 The melting point of the multi-layer EVOH composite sheet laminated and hot-pressed with the above structure not only has high gas barrier properties, but also has high tensile strength and impact strength. In addition, the multi-layer EVOH composite sheet also has high peel strength.

[0058] In summary, compared with the prior art, the present invention has the following beneficial effects:

[0059] (1) Compared with conventional single-layer or EVOH composite materials of the same thickness, the composite sheet prepared by the present invention has higher mechanical strength and gas barrier properties (the smaller the oxygen permeability value, the better).

[0060] (2) The composite sheet of the present invention can change the number of stacking layers according to application requirements. Through the preferred unique melting point gradient setting, the hot pressing temperature selection of the composite sheet can be wider, the adhesion between different EVOH layers is strong, and the outer layer polyolefin can maintain the water resistance and boiling resistance of the composite sheet.

[0061] (3) The high-strength, high-impact, and high-barrier composite sheet of the present invention can be produced with the aid of existing equipment, has a mature process, and has important application value. DETAILED DESCRIPTION

[0062] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0063] In the following examples and comparative examples:

[0064] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.

[0065] The composite sheet performance is tested according to the following method:

[0066] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, where the test temperature is 230°C and the load is 2.16 kg;

[0067] (2) Tensile strength: measured according to the method specified in GB / T1040.1-2018;

[0068] (3) Hammer impact strength: measured according to the method specified in GB / T14153-1993;

[0069] (4) Oxygen permeability: measured according to the method specified in GB / T19789-2005;

[0070] (5) Interlayer peel strength: measured according to the method specified in QB / T2358-1998.

[0071] The parameters in Table 1 are obtained by directly testing the composite sheets in the corresponding embodiments and comparative examples.

[0072] In the following examples, the sources of some raw materials are described in the examples, and the remaining raw materials are commercially available unless otherwise specified.

[0073] Example 1

[0074] The following steps are used to prepare a multi-layer EVOH composite sheet with high strength, high impact resistance and high barrier properties:

[0075] (1) Preparation of polyolefin composition film layer A:

[0076] Polyolefin a is Shanghai Petrochemical low-density polyethylene Q281D, melt index: 2.8g / 10min, density: 0.925g / cm 3 ; Thermal bonding enhancer b is Japan Mitsui ADMER NF528;

[0077] The components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. The mixture is added to a high-speed stirrer and mixed evenly. The mixed material is then added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 180-210°C. The screw is melt-mixed evenly, extruded, granulated and dried to obtain polyethylene composition pellets.

[0078] The polyethylene composition pellets are fed into an extrusion casting machine and then flow out, and then pass through a calendering roller and a traction roller in sequence, and then undergo solid phase stretching, edge cutting and winding, so as to obtain the polyolefin composition film layer A.

[0079] The temperature of the extrusion casting was 215° C., and the temperature of the calender roll was 55° C. The temperature during the solid phase stretching was 120° C., the stretching rate was 2 m / min, and the stretching ratio was 7 times.

[0080] (2) Preparation of EVOH film layer B:

[0081] EVOH (F171B from Kuraray Co., Ltd., Japan, ethylene content 32%, melting point 183°C, melt index 1.6g / 10min at 190°C / 2.16kg) is added to an extrusion casting machine and then passes through a calendering roller, a pulling roller, and then solid phase stretching, trimming and winding to obtain the EVOH film layer B.

[0082] The temperature of the extrusion casting was 220° C., and the temperature of the calender roll was 55° C. The temperature during the solid phase stretching was 170° C., the stretching rate was 2 m / min, and the stretching ratio was 7 times.

[0083] (3) Preparation of multilayer EVOH composite sheets:

[0084] Four layers of EVOH film layers B are stacked at 90° between the warp and the warp, and a layer of polyolefin film layer A is placed on the outermost layer of EVOH (i.e., the structure is ABBBBA), and the composite sheet S1 is obtained after hot pressing and cooling. The hot pressing conditions used are: temperature 170°C, hot pressing pressure 5MPa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the obtained composite sheet S1 is 100μm, of which the thickness of the EVOH film layer B accounts for 80% of the total thickness of the sheet.

[0085] Comparative Example 1

[0086] The multilayer EVOH composite sheet was prepared as follows:

[0087] (1) Same as step (1) of Example 1;

[0088] (2) EVOH was not subjected to solid phase stretching, but the die of the casting machine and the distance between the calendering rollers were controlled to make the obtained EVOH film layer B have the same thickness as that of Example 1;

[0089] (3) The same as step (3) of Example 1, the obtained composite sheet is D1.

[0090] The thickness of the obtained composite sheet is 100 μm, wherein the thickness of the EVOH film layer Bi accounts for 80% of the total thickness of the sheet.

[0091] Example 2

[0092] The multilayer EVOH composite sheet was prepared as follows:

[0093] Step (1) and step (2) are the same as steps (1) and (2) of Example 1;

[0094] Except for step (3) in which the four EVOH film layers B are stacked at an angle of 0° between the warp directions, the rest of the process is the same as step (3) of Example 1, and the resulting composite sheet is S2.

[0095] Example 3

[0096] The multilayer EVOH composite sheet was prepared as follows:

[0097] Step (1) is the same as step (1) of Example 1;

[0098] The material selection in step (2) is the same as that in step (2) of Example 1, except that after the EVOH is solid-phase stretched (stretching rate is 2 m / min, stretching ratio is 7 times), a second stage free stretching is performed, with a stretching rate of 0.5 m / min and a stretching ratio of 2 times.

[0099] Step (3) is the same as step (3) of Example 1. The resulting composite sheet is S3 with a thickness of 62 μm, wherein the thickness of the EVOH film layer Bi accounts for 52% of the total thickness of the sheet.

[0100] Example 4

[0101] The multilayer EVOH composite sheet was prepared as follows:

[0102] Steps (1) and (2) are the same as steps (1) and (2) of Example 1;

[0103] In step (3), except that the number of EVOH film layer B is changed to 7 layers, the rest is the same as step (3) of Example 1. The resulting composite sheet is S4 with a thickness of 160 μm, wherein the thickness of EVOH film layer B accounts for 87% of the total thickness of the sheet.

[0104] Example 5

[0105] The multilayer EVOH composite sheet was prepared as follows:

[0106] Step (1) is the same as step (1) of Example 1;

[0107] Step (2) Preparation of EVOH film layer B:

[0108] EVOH (respectively: Japan Kuraray Company, M100B, ethylene content 25%, melting point 195 ° C, corresponding to B1;

[0109] L171B, ethylene content 27%, melting point 190°C, corresponding to B2;

[0110] F171B, ethylene content 32%, melting point 183°C, corresponding to B3;

[0111] H171B, ethylene content 38%, melting point 172°C, corresponding to B4) is added to the extrusion casting machine and then passes through the calendering roller and the pulling roller in sequence, and then undergoes solid phase stretching, trimming and winding to obtain the EVOH film layers B1, B2, B3, and B4.

[0112] The temperature of the extrusion casting was 220° C., and the temperature of the calendering roller was 55° C. The temperature during the solid phase stretching was 170° C., the stretching rate was 2 m / min, the stretching ratio was 7 times, and the thickness of each film layer Bi was the same as that of the film layer B in Example 1.

[0113] (3) Preparation of composite sheets:

[0114] 7 layers of EVOH film layer B i The layers are stacked at 90° between the warp directions, and the stacking method from top to bottom is: B1 / B2 / B3 / B4 / B3 / B2 / B1. A layer of polyolefin film layer A is placed on the outermost layer of EVOH, that is, the structure is AB1 / B2 / B3 / B4 / B3 / B2 / B1A. The hot pressing conditions are the same as in Example 1, and a composite sheet S5 with a thickness of 160μm is obtained, wherein the thickness of the EVOH film layer Bi accounts for 87% of the total thickness of the sheet.

[0115] Example 6

[0116] The multilayer EVOH composite sheet was prepared as follows:

[0117] Step (1) and step (2) are the same as step (1) of Example 1;

[0118] In step (3), the stacking pattern of Bi from top to bottom is: B4 / B3 / B2 / B1 / B2 / B3 / B4, and the rest is the same as Example 5, to obtain a composite sheet S6 with a thickness of 160 μm, wherein the thickness of the EVOH film layer Bi accounts for 87% of the total thickness of the sheet.

[0119] The properties of the composite sheets prepared in the above embodiments and comparative examples are shown in Table 1.

[0120] Table 1

[0121]

[0122]

[0123] From the comparison between Examples 1-6 of the present invention and Comparative Example 1, it can be seen that after solid phase stretching, the tensile strength, impact strength and oxygen barrier performance of EVOH are significantly improved.

[0124] It can be seen from Example 1 and Comparative Example 1 that the tensile strength, impact strength and oxygen barrier rate of the laminated composite sheet are increased exponentially. This is because EVOH is placed at 90° between the warp and the warp directions, and the composite sheet is reinforced in both the transverse and longitudinal directions after being subjected to external force.

[0125] The multilayer EVOH composite sheet of the present invention has AB1B2...B m A structure, B1B2...B m The melting points can be the same or different, and the technical effects of the present invention can be achieved.

[0126] After research, the inventor of the present invention unexpectedly discovered that when B1B2…B m When the melting points are the same or arranged in a specific melting point gradient, the resulting multilayer EVOH composite sheet is better than B1B2…B m The case where the melting points are not arranged in a specific melting point gradient manner has a better technical effect, specifically, see Examples 4, 5 and 6.

[0127] And when B1B2…B m When the melting points are arranged according to a specific melting point gradient, compared to B1B2…B m The melting points are the same, and the technical effect is further improved. For details, see the comparison between Example 4 and Example 5. In particular, if the EVOH layer is subjected to the specific melting point gradient lamination hot pressing treatment of the present invention, the peeling strength between the EVOH layers can be greatly improved.

[0128] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

[0129] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0130] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0131] The endpoints and any values ​​of the scope disclosed in the present application document are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, between the endpoint values ​​of each scope, between the endpoint values ​​of each scope and a separate point value, and between separate point values, one or more new numerical ranges can be combined with each other, and these numerical ranges should be considered as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be considered as specifically disclosed in this article.

[0132] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

[0133] Moreover, any embodiment described in this document may be freely combined with one or more other embodiments described in this document, and the technical solutions or technical ideas formed thereby are deemed to be part of the original disclosure or original record of the present invention, and should not be regarded as new content that has not been disclosed or anticipated in this document, unless a person skilled in the art considers that the combination is obviously unreasonable.

Claims

1. A multi-layer EVOH composite sheet, comprising two outer layers A and a plurality of laminated core layers B located between the two outer layers A, having AB1B2…B m A structure; m is an integer not less than 2; The two outer layers A are the same or different, and each contains a polyolefin composition A; the core layers B each contain a composition B, and the composition B is the same or different, and each contains EVOH; The preparation process of the core layer B includes a stretching step, and the stretching ratio is 1-15 times.

2. The multilayer EVOH composite sheet according to claim 1, characterized in that: The melting point of the composition B is 150-210°C, preferably 160-200°C; and / or, The composition B is EVOH; and / or, The ethylene content of the EVOH is 15-50 mol%, preferably 21-49 mol%; and / or, The m is 2-200, preferably 4-100.

3. The multilayer EVOH composite sheet according to claim 1, characterized in that: The multi-layer EVOH composite sheet has AB1B2...B i …B n …B i …B2B1A lamellar structure, i and n are both integers not less than 2, and i≤n, n is 2-100, preferably 2-50; and / or, The composition B i Melting point ≥ composition B i+1 The melting point of the composition B is preferably i Melting point > Composition B i+1 The melting point of composition B is preferably i With composition B i+1 The melting point difference is 5-15°C.

4. The multilayer EVOH composite sheet according to claim 1, characterized in that: The stretching ratio is 2-15 times; and / or the stretching method is a combination of one or more of free stretching, solid phase stretching, and multi-stage stretching; preferably, The stretching conditions in the step of preparing the core layer B include: the core layer B is prepared by extrusion molding, casting or calendering, and stretching EVOH; Further preferably, the stretching conditions include: The stretching temperature is 140-185°C, preferably 150-175°C; the stretching ratio is 2-15 times.

5. The multi-layer EVOH composite sheet according to claim 1, characterized in that: The thickness of the multi-layer EVOH composite sheet is 5-1000 μm, preferably 5-500 μm, and more preferably 5-300 μm; and / or, Taking the total thickness of the multi-layer EVOH composite sheet as 100%, the total thickness of all core layers B accounts for 10%-90% of the total thickness of the multi-layer EVOH composite sheet; and / or, The core layers B are stacked from top to bottom in a warp direction at an angle of 0-90 degrees.

6. The multilayer EVOH composite sheet according to any one of claims 1 to 5, characterized in that: The polyolefin composition A contains polyolefin a and thermal adhesion enhancer b; preferably, Taking the total weight of the polyolefin composition A as 100wt%, the polyolefin composition A contains 70-99wt% of polyolefin a and 1-30wt% of thermal adhesion enhancer b; preferably, the polyolefin composition A comprises 80-99wt% of polyolefin a and 1-20wt% of thermal adhesion enhancer b; and / or, The polyolefin a is selected from one or more of polypropylene, polyethylene, and ethylene-vinyl acetate; and / or, The thermal adhesion enhancer b is selected from one or more of anhydride modified polypropylene, anhydride modified polyethylene, anhydride modified ethylene-vinyl acetate, glycidyl methacrylate modified polypropylene, glycidyl methacrylate modified polyethylene, glycidyl methacrylate modified ethylene-vinyl acetate, and maleic anhydride copolymer.

7. The multilayer EVOH composite sheet according to any one of claims 1 to 5, characterized in that: The multi-layer EVOH composite sheet is prepared by sequentially stacking an outer layer A, a plurality of core layers B, and an outer layer A, and then laminating them; preferably, The lamination method is to first heat press and then cool and shape; further preferably, The multi-layer EVOH composite sheet is prepared by extruding, casting or calendering, stretching and slitting the raw materials for forming the outer layer A and the raw materials for forming the core layer B to obtain corresponding sheets, and then stacking, hot pressing and cooling the corresponding sheets in a corresponding structural order.

8. A method for preparing a multilayer EVOH composite sheet according to any one of claims 1 to 7, comprising respectively preparing a raw material for forming an outer layer A and a raw material for forming a core layer B into corresponding sheets A and B, and then stacking, hot pressing, and cooling the corresponding sheets in a corresponding structural order; wherein, The preparation process of the sheet B includes a stretching step, and the stretching ratio is 1-15 times.

9. The preparation method according to claim 8, characterized in that: The step of preparing the sheet A comprises: melt-blending the raw materials forming the outer layer A, preferably extruding, and then casting or calendering, stretching, and slitting to obtain the sheet A; preferably, The preparation conditions of sheet A include: The temperatures for extrusion molding and casting are independently selected from 200-250°C; the calendering temperature is 50-70°C; and / or, The stretching method is a combination of one or more of free stretching, solid phase stretching and multi-stage stretching; preferably, the stretching temperature is 90-165° C., preferably 90-140° C.; and the stretching ratio is 1-20 times.

10. The preparation method according to claim 8, characterized in that: The step of preparing the core layer B comprises: extruding the raw material for forming the core layer B, and then casting or calendering, stretching, and slitting to obtain a sheet B; preferably, The preparation conditions of sheet B include: The temperatures for extrusion molding and casting are independently selected from 200-260°C; the calendering temperature is 50-90°C; and / or, The stretching method is a combination of one or more of free stretching, solid phase stretching, and multi-stage stretching; preferably, the stretching temperature is 140-185°C, preferably 150-175°C; the stretching ratio is 1-15 times, preferably 2-15 times; more preferably, The stretching method is one of solid phase stretching and multi-stage stretching or a combination of the two methods.

11. The preparation method according to any one of claims 8 to 10, characterized in that: The stacking method includes: from top to bottom, the sheets A and B are stacked in order with an angle of 0-90 degrees between the warp and the warp; and / or, The hot pressing conditions include: the hot pressing temperature is 135-190°C, preferably 150-190°C; and / or, the hot pressing pressure is 2-10MPa; and / or, the preheating time is 5-600s, and / or, the hot pressing time is 1-600s, preferably 10-500s; And / or, the cooling and shaping conditions include: a cooling pressure of 2-8 MPa, and / or a cooling time of 30-700 s.

12. Use of the multilayer EVOH composite sheet according to any one of claims 1 to 7 or the multilayer EVOH composite sheet obtained by the preparation method according to any one of claims 8 to 11 in the fields of packaging, mechanical parts, and industrial and agricultural films.

Citation Information

Patent Citations

  • Ethylene-vinyl alcohol copolymer composition, and shaped product and application thereof

    CN109705248A

  • High-flatness, high-barrier, high-strength and cooking-resistant stretch film and production method thereof

    CN111993732A

  • Ethylene-vinyl alcohol copolymer composition with good oxygen barrier properties

    CN113698695A

  • Heat sealable multilayer film and its method of preparation

    CA2205393A1

  • Multi-layer heat sealable co-extrusion and biaxial tension composite thin film

    CN110303740A