Low-temperature high-impact-resistance high-strength polypropylene sheet and fabric thereof, polypropylene composite material and preparation method and application thereof
Patent Information
- Application Number
- CN202310506518.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-07
AI Technical Summary
Polypropylene materials are prone to brittleness in low temperature environments and have poor toughness, making it difficult to have high strength, interlayer peel strength and low temperature impact properties at the same time, which limits its application range, especially in high-end applications in special low temperature fields.
Using a multi-layer structure, impact-resistant polypropylene sheet and fabric, a high melting point spread is designed by hot-pressing the homopolymer and random copolymer polypropylene composition, combined with toughening agent and β-crystal nucleating agent. The layer structure improves the mechanical properties of the material and the interlayer peel strength, and maintains good impact resistance under low temperature conditions.
It realizes high strength, good interlayer peel strength and impact resistance of polypropylene materials under low temperature conditions, broadens its application areas, overcomes the fragility of polypropylene in low temperature environments, and is suitable for electrical component packaging and automobile manufacturing. and other fields.
Smart Images

Figure BDA0004216577600000221 
Figure BDA0004216577600000231
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polypropylene materials, and more particularly to a low-temperature, high-impact, high-strength polypropylene sheet and fabric thereof, a polypropylene composite material, and a preparation method and application thereof. Background Art
[0002] Polypropylene (PP) resin is the most widely used synthetic resin material at present. It has the advantages of low density and low cost and has good mechanical properties, processing performance and weldability.
[0003] Self-reinforced polymer composites can further improve the usability of high-performance materials. They are generally composed of a matrix and a reinforcing phase of the same polymer but different forms. The reinforcing phase is usually a highly oriented fiber or flat ribbon. Hot pressing is a common method for preparing self-reinforced polymer composites. Its working principle is that when the reinforcing phase is hot pressed at a certain temperature and pressure, the surface of the reinforcing phase fiber melts into a matrix melt. The matrix melt and the surface of the reinforcing phase co-crystallize when melted, thereby providing sufficient interfacial bonding strength. For example, the U.S. patent (US6312638B1) hot-presses melt-spun oriented polyolefin fibers, and prepares polyolefin sheets by partially melting and bonding the surface of the substrate at a specific temperature and pressure. However, this preparation method has defects such as high hot pressing temperature and sensitivity to hot pressing temperature, and the oriented fibers produce a large decomposition orientation after hot pressing, resulting in a significant decrease in the mechanical strength of the material.
[0004] Compared with the above method, the US patent (US8133537B2) obtains a polyolefin composite material by hot pressing three layers of polyolefin fibers with different melting points, wherein the melting temperatures of the first and second layers of polyolefin are lower than the core layer. This method broadens the hot pressing processing window, reduces the hot pressing pressure, and can complete the hot pressing molding of polyolefins with different melting points, but the impact strength and interlayer peeling strength of the prepared hot pressing composite material are relatively low.
[0005] As a crystalline material, polypropylene has certain impact resistance in the movement of its amorphous phase chain segments at room temperature (23°C), but in a low temperature environment, the movement of the molecular chain is limited, resulting in the inability to effectively release the impact energy. Therefore, polypropylene materials are constrained by their own structure-performance, and are very easy to become brittle and have poor toughness under low temperature conditions. These problems seriously limit the application of polypropylene materials, especially high-end applications in the field of special low temperatures. At present, existing technologies such as (CN114369315A, CN114409998A, CN 110698769 B, CN 114262486 A) mainly improve the low-temperature impact resistance of composite materials by melt blending and modification of PP and elastomer. This method is the most commonly used method to improve the low-temperature impact resistance of materials, but this method will significantly reduce the rigidity and modulus of the composite material, and cannot meet the use conditions required by high-performance materials such as "both rigid and tough" under low temperature conditions.
[0006] Therefore, how to overcome the application bottleneck of polypropylene itself, which is extremely brittle and has poor toughness under extreme conditions such as low temperature, and provide a polypropylene composite material with high strength, interlayer peel strength and low-temperature impact performance, is a technical problem that needs to be solved at present. Summary of the invention
[0007] The purpose of the present invention is to overcome the technical defect that the existing polypropylene composite material is difficult to have high strength, interlayer peeling strength and low-temperature impact performance at the same time, to further improve the comprehensive mechanical properties of polypropylene materials, achieve high performance, broaden its application field, and especially overcome the application bottleneck that polypropylene itself is extremely easy to become brittle and has poor toughness under extreme conditions such as low temperature. Provided are a low-temperature, high-impact, high-strength polypropylene sheet and its fabric, a polypropylene composite material, and a preparation method and application thereof. The high-strength, low-temperature, high-impact polypropylene sheet of the present invention is subjected to hot pressing to obtain a high-strength, low-temperature, high-impact polypropylene composite material. The high-strength, low-temperature, high-impact polypropylene composite material has excellent rigidity and low-temperature impact resistance. Even at a lower hot pressing temperature and within a wider hot pressing temperature range, the obtained high-strength, high-low-temperature, high-impact polypropylene composite material still has a high interlayer peeling strength.
[0008] The first aspect of the present invention is to provide an impact-resistant polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB';
[0009] Layer A contains a polypropylene composition A, which includes homopolymer polypropylene a and a toughening agent m; layer B is the same as or different from layer B', and each correspondingly contains a polypropylene composition B and a polypropylene composition B', and the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x and a toughening agent n; wherein the melting point of the polypropylene composition A is greater than the melting point of the polypropylene composition B and the polypropylene composition B'; the toughening agent m and the toughening agent n are the same as or different, and each is selected from an elastic material.
[0010] According to the present invention, the film layers B and B' on both sides of the film layer A are the same or different. In some preferred embodiments of the present invention, the film layers B and B' on both sides of the film layer A are the same.
[0011] In some preferred embodiments of the present invention, the melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10°C.
[0012] In a preferred embodiment of the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'; preferably, the melting point of the homopolypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees.
[0013] In some preferred embodiments of the present invention, the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C. In this preferred embodiment, the inventors of the present invention surprisingly found that the obtained polypropylene sheet is subjected to hot pressing to obtain a polypropylene composite material, which has more excellent mechanical properties and better interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained polypropylene composite material has a higher interlayer peeling strength. At the same time, it also has higher impact resistance at low temperatures (as low as -20°C), overcoming the technical defect that it is difficult for existing polypropylene composite materials to have high strength, interlayer peeling strength and low-temperature impact performance at the same time.
[0014] In some preferred embodiments of the present invention, based on the total thickness of the impact-resistant polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%. The thicknesses of film layers B and B' on both sides of film layer A can be the same or different, preferably the same.
[0015] The present invention does not limit the thickness of the polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.
[0016] According to the present invention, the thickness of the film layers A, B, B' can be controlled by the melt pump of the extruder during the processing.
[0017] In some preferred embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-98wt% of homopolypropylene a and 2-50wt% of toughening agent m; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of toughening agent m.
[0018] In some preferred embodiments of the present invention, based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each comprise 70-98 wt% of random copolymerized polypropylene x and 2-50 wt% of toughening agent n; preferably, the polypropylene composition B and the polypropylene composition B' each comprise 70-90 wt% of random copolymerized polypropylene x and 10-30 wt% of toughening agent n.
[0019] In some preferred embodiments of the present invention, the homopolypropylene a has: a melting point of 150-170°C, preferably 160-170°C; and / or a melt flow rate at 230°C and 2.16 kg load of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, further preferably 2.5-18 g / 10 min; and / or an isotacticity (mm) of not less than 96%.
[0020] According to the present invention, the toughening agent m and the toughening agent n are the same or different, and are each selected from elastic materials; preferably, the toughening agent m and the toughening agent n are each selected from elastomers and / or soft biodegradable materials. According to the present invention, further preferably, the toughening agent m and the toughening agent n are each selected from at least one of the following substances and / or modified substances of at least one of the following substances: polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, biodegradable polyester, natural rubber, bio-based elastomer, special rubber; further preferably, the toughening agent m and the toughening agent n are each selected from at least one of the following substances and / or modified substances of at least one of the following substances: polybutylene adipate terephthalate, polybutylene terephthalate succinate, polybutylene succinate and copolymers thereof, polycaprolactone, natural rubber, hydrogenated nitrile rubber, polyolefin elastomer; more preferably, the toughening agent m and the toughening agent n are each selected from at least one of the following substances and / or modified substances of at least one of the following substances: polyolefin elastomer, hydrogenated nitrile rubber.
[0021] The above-mentioned bio-based elastomer can be, by way of example, at least one of a bio-based polyurethane elastomer, a bio-based polyamide elastomer, and a bio-based polyester elastomer.
[0022] According to the present invention, when the toughening agent m and the toughening agent n each contain a rubber material, both are vulcanized rubber materials.
[0023] In some further preferred embodiments of the present invention, the toughening agent m and the toughening agent n are each selected from polyolefin elastomer maleic anhydride modified product and hydrogenated nitrile rubber; preferably, the weight ratio of the polyolefin elastomer maleic anhydride modified product to the hydrogenated nitrile rubber is 0.2 to 5 (i.e. (0.2 to 5): 1); more preferably,
[0024] The polyolefin elastomer is a copolymer elastomer of ethylene and the following olefins: propylene and / or α-olefin; more preferably, the α-olefin is a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene.
[0025] According to the present invention, the maleic anhydride modified polyolefin elastomer can be prepared by existing technology, or a commercial product can be used. According to the present invention, further more preferably, the toughener m and the toughener n are each obtained by the following method: the maleic anhydride modified polyolefin elastomer and hydrogenated nitrile rubber are mixed to obtain a modified hydrogenated nitrile masterbatch, and then the modified hydrogenated nitrile masterbatch is vulcanized to obtain a vulcanized rubber, and the vulcanized rubber is crushed to obtain a toughener m and a toughener n. The specific processing conditions can adopt the existing processing conditions in this field, and the present invention is not particularly limited, including but not limited to the method described in the specific embodiment of the present invention.
[0026] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the toughening component m in the composition can better absorb impact energy, meet the impact performance, especially the impact performance requirements under low temperature environment, so that the sheet has better low temperature impact resistance. At the same time, since the macromolecular chain segments in the homopolymerized polypropylene a are relatively regular, crystallization occurs during the preparation of the sheet, so the sheet also has better tensile properties.
[0027] In some preferred embodiments of the present invention, the random copolymer polypropylene x has:
[0028] The melting point is 110-150°C, preferably 120-140°C; and / or, the melt flow rate at 230°C and 2.16kg load is 0.5-50g / 10min, preferably 1-20g / 10min, and further preferably 3-18g / 10min; and / or, the molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, it is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
[0029] According to the research conducted by the inventors, when the polypropylene composition B 、 When the melt mass flow rate and polymer composition ratio of B' are within the preferred range, the low melting point random copolymer polypropylene x and toughening agent n in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the toughening agent n is a single-component multifunctional auxiliary agent, which can provide good adhesion properties for the sheet, further improve the interlayer peeling strength, and significantly improve the low-temperature impact resistance of the sheet.
[0030] In some preferred embodiments of the present invention, the layer A further contains a β-crystalline nucleating agent; preferably,
[0031] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.
[0032] The content of the β-crystal nucleating agent has a wide selection range. Preferably, relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.
[0033] According to the research of the present inventors, when the melting point difference, polymer composition ratio and thickness distribution of film layer A of polypropylene composition A, polypropylene combination B and polypropylene combination B' are within the preferred range, the sheet preparation process can be smoother, thereby making the sheet have better uniformity, tensile strength, impact resistance and interlayer peeling strength.
[0034] In some preferred embodiments of the present invention, the BAB' layer structure of the polypropylene sheet can be prepared by a variety of methods. In a preferred embodiment of the present invention, the BAB' layer structure of the impact-resistant polypropylene sheet is obtained by co-extruding a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B'.
[0035] The second aspect of the present invention is to provide a method for preparing the impact-resistant polypropylene sheet described in the first aspect, comprising co-extruding, casting or calendering, and stretching a layer A raw material containing a polypropylene composition A, a layer B raw material containing a polypropylene composition B, and a layer B' raw material containing a polypropylene composition B' according to a BAB' structure to obtain the impact-resistant polypropylene sheet.
[0036] In some preferred embodiments of the present invention, the preparation of the raw material of layer A includes melt blending the components including the homopolypropylene a and the toughening agent m. The conditions and equipment for melt blending the polypropylene composition A are the conditions and equipment for melt blending of polyolefins in the prior art. For example, the melting temperature can be 130-168° C., and the equipment is preferably a twin-screw extruder.
[0037] In some preferred embodiments of the present invention, the preparation of the raw materials for layers B and B' comprises melt blending the components including the random copolymer polypropylene x and the toughening agent n. The conditions and equipment for melt blending the raw materials for layers B and B' are the conditions and equipment for melt blending of polyolefins in the prior art. For example, the melting temperature can be 100-148°C, and the equipment is preferably a twin-screw extruder.
[0038] In some preferred embodiments of the present invention, the co-extrusion and casting temperatures are independently selected from 200-240°C.
[0039] In some preferred embodiments of the present invention, the calendering temperature is 50-70°C.
[0040] The selection range of stretching conditions is relatively wide. In a preferred embodiment of the present invention, the stretching conditions include: the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is 90-165°C, preferably 90-140°C, and further preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0041] The specific process of preparing the film by the extrusion calendering method is a common choice in the art and will not be described in detail here.
[0042] The third aspect of the present invention is to provide an impact-resistant polypropylene fabric, which is a three-dimensional polypropylene fabric obtained by weaving the impact-resistant polypropylene sheet described in the first aspect; preferably, the impact-resistant polypropylene fabric is obtained by slitting and weaving the impact-resistant polypropylene sheet; and / or, the impact-resistant polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
[0043] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then woven to obtain the polypropylene fabric.
[0044] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain, twill, satin or three-dimensional polypropylene fabric obtained by weaving three-layer co-extruded polypropylene stretch flat tape, and the three-layer co-extruded polypropylene stretch flat tape includes at least one film layer A formed by a high-melting point polypropylene combination A and at least one film layer B formed by a low-melting point polypropylene composition B, wherein the polypropylene composition A includes homopolymer polypropylene a and a toughening agent m; the polypropylene composition B includes a random copolymer polypropylene x and a toughening agent n, and the polymer film B layer is located on both sides of the A layer and is the same or different.
[0045] The fourth aspect of the present invention provides an impact-resistant polypropylene composite material, which is prepared by thermally pressing multiple layers of the impact-resistant polypropylene sheets described in the first aspect and / or the impact-resistant polypropylene fabric described in the third aspect.
[0046] Preferably, the impact-resistant polypropylene composite material is prepared by thermally pressing multiple layers of the impact-resistant polypropylene sheets or the impact-resistant polypropylene fabrics.
[0047] Preferably, the multi-layer impact-resistant polypropylene sheets are stacked from top to bottom in the angle of 0-90° along the respective machine directions.
[0048] Preferably, the multi-layer impact-resistant polypropylene fabric is stacked from top to bottom with the warp direction and the warp direction being 0-90 degrees.
[0049] Preferably, the number of layers of the multi-layer impact-resistant polypropylene sheet and / or the multi-layer impact-resistant polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers, and most preferably 4-100 layers.
[0050] In some preferred embodiments of the present invention, the impact-resistant polypropylene composite material comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B iA i B' i The structure of the impact-resistant polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;
[0051] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i ,
[0052] The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group.
[0053] According to the present invention, in the structure of the polypropylene composite material, the upper i-th group and the lower i-th group may be the same or different.
[0054] In a preferred embodiment of the present invention, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is 5°C or more, preferably 10°C or more, and more preferably 20°C or more.
[0055] According to the present invention, the core layers in each polypropylene sheet unit can be made of the same material or different materials. There is no particular limitation on this. As long as A i The melting point is greater than that of the polypropylene composition B i , polypropylene composition B' i The melting point can achieve better technical effects.
[0056] In a preferred embodiment of the present invention, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is each 1-40°C, preferably 1-10°C, and more preferably 1-5°C.
[0057] According to the present invention, the total number of stacked groups of the polypropylene sheet unit group is 2n-1. The present invention has a wide selection range for the total number of stacked groups of the polypropylene sheet unit group. In a preferred embodiment of the present invention, 2≤n≤100 is selected, more preferably, 2≤n≤50, and further preferably, 2≤n≤30.
[0058] According to the present invention, the selection range of the number of polypropylene sheet units included in each polypropylene sheet unit group is relatively wide. In a preferred embodiment of the present invention, each polypropylene sheet unit group independently includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.
[0059] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.
[0060] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.
[0061] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B'n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.
[0062] In a preferred embodiment of the present invention, the polypropylene composite material has at least one of the following characteristics:
[0063] Longitudinal tensile strength ≥130MPa, preferably ≥160MPa;
[0064] Interlayer peel strength ≥1N / mm, preferably ≥1.2N / mm;
[0065] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.
[0066] When the polypropylene composite material is obtained by hot pressing 24 layers of polypropylene fabrics and has a thickness of about 1.6 mm, the -20°C drop hammer impact strength is ≥160 J, preferably ≥180 J.
[0067] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.
[0068] The fifth aspect of the present invention is to provide a method for preparing the impact-resistant polypropylene composite material described in the fourth aspect, the method comprising laminating and hot-pressing the impact-resistant polypropylene sheets and / or the impact-resistant polypropylene fabrics, and then cooling and shaping them to form the impact-resistant polypropylene composite material.
[0069] Preferably, the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.
[0070] Preferably, the pressure of the hot pressing fusion is 2-10 MPa.
[0071] Preferably, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s.
[0072] Preferably, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s.
[0073] Preferably, the number of layers of the impact-resistant polypropylene sheet and / or the impact-resistant polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers.
[0074] Preferably, adjacent layers of the impact resistant polypropylene fabric laminate are placed at an angle of 0-90° between the warp directions.
[0075] Preferably, adjacent layers of the impact resistant polypropylene sheet laminate are placed at 0-90° along their respective machine directions.
[0076] In a more preferred embodiment of the present invention, the method for preparing the high-strength and high-impact polypropylene composite material comprises the following steps:
[0077] Step a: co-extrude the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure and cast or calender to obtain a polypropylene co-extruded sheet; preferably, the extrusion casting or calendering temperature is 200-240° C., and the temperature of the calendering roller is 50-70° C.;
[0078] Step b: stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is preferably 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0079] Step c: cutting the polypropylene stretched sheet to prepare polypropylene flat strips, and weaving the flat strips to prepare polypropylene fabrics; preferably, the width of the polypropylene flat strips is 2-5 mm, and the polypropylene fabrics include plain weave, twill, satin weave or other three-dimensional polypropylene fabrics;
[0080] Step d: laminating the polypropylene fabrics in sequence, hot pressing and fusing them, and then cooling and shaping them to form a polypropylene composite material; preferably, in the step d, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10MPa, preheating time 5-600s, hot pressing time 1-600s, preferably 10-500s, cooling pressure 2-8MPa, cooling time 30-700s; preferably, adjacent polypropylene fabrics in the polypropylene composite material can be placed at 0-90° between the warp and the warp.
[0081] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented polypropylene flat ribbon with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat ribbon according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional polypropylene fabrics.
[0082] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.
[0083] During the preparation, the polypropylene sheet and / or the polypropylene fabric are stacked in sequence and then preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polypropylene composite material, i.e., a stacked hot-pressed product. Afterwards, the sheets are sliced by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressurizing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within a preferred range, preferably when the preparation equipment is used to prepare the polymer composite material, the polymer composite material has better tensile strength, impact resistance, and interlayer peeling strength.
[0084] The sixth aspect of the present invention provides an application of the impact-resistant polypropylene sheet described in the first aspect, the impact-resistant polypropylene fabric described in the third aspect, the impact-resistant polypropylene composite material described in the fourth aspect, and the impact-resistant polypropylene composite material prepared by the preparation method described in the fifth aspect in the fields of electrical component packaging, automobile manufacturing, military materials, and consumer products;
[0085] According to a specific embodiment of the present invention, the material fields include electrical and electronics industry, luggage and transportation industry, shoemaking industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.
[0086] Compared with the prior art, the present invention has the following beneficial effects:
[0087] (1) The high-strength and high-low-temperature impact-resistant polypropylene composite material of the present invention has excellent rigidity, low-temperature impact resistance and interlayer peeling performance. The high performance of the material is achieved through component design, especially the temperature difference of the melting point of the composition in the sheet, which broadens the application field of polypropylene, especially overcomes the application bottleneck of polypropylene itself, which is that it is very easy to become brittle and has poor toughness under extreme conditions such as low temperature.
[0088] The polypropylene composite material has the following characteristics:
[0089] The longitudinal (MD) tensile strength is ≥130MPa, preferably ≥160MPa; the interlayer peel strength is ≥1N / mm, preferably ≥1.2N / mm; when the composite material is only composed of 24 layers of polypropylene fabrics hot pressed together and the thickness is about 1.6mm, the -20°C drop hammer impact strength is ≥160J, preferably ≥180J.
[0090] (2) The polypropylene composite material of the present invention can be prepared at a relatively low hot pressing temperature and within a relatively wide hot pressing temperature range, which effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high-temperature operation. At the same time, when prepared at a relatively low hot pressing temperature, it still has good interlayer peeling strength.
[0091] (3) The preparation method can reduce the hot pressing operation time, while improving production efficiency and reducing production energy consumption.
[0092] (4) The present invention reduces the hot pressing temperature and expands the hot pressing temperature range to 50°C; it effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high temperature operation. DETAILED DESCRIPTION
[0093] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0094] In the following examples and comparative examples:
[0095] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.
[0096] The properties of the polypropylene composition and sheet were tested according to the following methods, and the film test results are shown in Table 1:
[0097] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, where the test temperature is 230°C and the load is 2.16 kg;
[0098] (2) Melting point: measured according to the method specified in GB / T 28724-2012;
[0099] (3) Tensile strength: measured according to the method specified in GB / T1040.1-2018;
[0100] (4) Low temperature (-20°C) drop hammer impact strength: measured according to the method specified in GB / T14153-1993;
[0101] (5) Interlayer peel strength: measured according to the method specified in QB / T2358-98;
[0102] (6) Maleic anhydride grafted ethylene-octene copolymer (POE-g-MAH): CMG5805-L, manufactured by Jiayirong Company.
[0103] (7) Hydrogenated nitrile rubber (HNBR): saturation 99%, acrylonitrile content 36%, Mooney viscosity 65, Japan Zeon Co., Ltd.
[0104] (8) Mixed toughening agent 1#: hydrogenated nitrile rubber: POE-g-MAH = 80:20 (weight ratio). The preparation method is as follows:
[0105] a. 20 parts by weight of POE-g-MAH were added to a mixer and melted at 180°C, and then 80 parts by weight of hydrogenated nitrile rubber and 0.1 parts by weight of antioxidant RD (Ningkang Chemical) were added, the stirring speed was 50r / min, and the mixture was mixed for 5 minutes to obtain a modified hydrogenated nitrile masterbatch.
[0106] b. The modified hydrogenated nitrile masterbatch was prepared into vulcanized rubber according to the common rubber processing technology: 100 parts by weight of modified hydrogenated nitrile masterbatch, 5 parts by weight of zinc oxide (Beijing Inokai), 1 part by weight of stearic acid (Beijing Inokai), 40 parts by weight of N-220 carbon black (Tianjin Baochi Chemical), 1 part by weight of antioxidant RD (Ningkang Chemical), 8 parts by weight of peroxide vulcanizing agent F-40 (Beijing Inokai) and 2 parts by weight of triallyl isocyanurate (vulcanizing agent, Beijing Inokai) were mixed in an internal mixer, and then vulcanized in an ordinary flat vulcanizing press at 180°C for 10 minutes.
[0107] c. The vulcanized rubber is physically crushed to obtain mixed toughening agent 1#.
[0108] (9) Mixed toughening agent 2#: hydrogenated nitrile rubber: POE-g-MAH = 50:50 (weight ratio). The preparation method is as follows:
[0109] a. 50 parts by weight of POE-g-MAH were added to a mixer and melted at 180°C, and then 50 parts by weight of hydrogenated nitrile rubber and 0.1 parts by weight of antioxidant RD (Ningkang Chemical) were added, the stirring speed was 50r / min, and the mixture was mixed for 5 minutes to obtain a modified hydrogenated nitrile masterbatch.
[0110] b. The modified hydrogenated nitrile masterbatch was prepared into vulcanized rubber according to the common rubber processing technology: 100 parts by weight of modified hydrogenated nitrile masterbatch, 2.5 parts by weight of zinc oxide (Beijing Inokai), 1 part by weight of stearic acid (Beijing Inokai), 25 parts by weight of N-220 carbon black (Tianjin Baochi Chemical), 1 part by weight of antioxidant RD (Ningkang Chemical), 5 parts by weight of peroxide vulcanizing agent F-40 (Beijing Inokai) and 1.25 parts by weight of triallyl isocyanurate (vulcanizing agent, Beijing Inokai) were mixed in an internal mixer, and then vulcanized in an ordinary flat vulcanizing press at 180°C for 10 minutes.
[0111] c. The vulcanized rubber is physically crushed to obtain mixed toughening agent 2#.
[0112] (10) Mixed toughening agent 3#: hydrogenated nitrile rubber: POE-g-MAH = 20:80 (weight ratio). The preparation method is as follows:
[0113] a. 80 parts by weight of POE-g-MAH were added to a mixer and melted at 180°C, and then 20 parts by weight of hydrogenated nitrile rubber and 0.1 parts by weight of antioxidant RD (Ningkang Chemical) were added, the stirring speed was 50r / min, and the mixture was mixed for 5 minutes to obtain a modified hydrogenated nitrile masterbatch.
[0114] b. The modified hydrogenated nitrile masterbatch was prepared into vulcanized rubber according to the common rubber processing technology: 100 parts by weight of modified hydrogenated nitrile masterbatch, 1 part by weight of zinc oxide (Beijing Inokai), 0.5 parts by weight of stearic acid (Beijing Inokai), 10 parts by weight of N-220 carbon black (Tianjin Baochi Chemical), 0.5 parts by weight of antioxidant RD (Ningkang Chemical), 2 parts by weight of peroxide vulcanizing agent F-40 (Beijing Inokai) and 0.5 parts by weight of triallyl isocyanurate (vulcanizing agent, Beijing Inokai) were mixed in an internal mixer, and then vulcanized in an ordinary flat vulcanizing press at 180°C for 10 minutes.
[0115] c. The vulcanized rubber is physically crushed to obtain mixed toughening agent 3#.
[0116] (11) Sulfurized hydrogenated nitrile rubber, the preparation method is as follows:
[0117] The hydrogenated nitrile rubber is prepared into a vulcanized hydrogenated nitrile rubber according to a common rubber processing technology: 100 parts by weight of hydrogenated nitrile masterbatch (saturation of 99%, acrylonitrile content of 36%, Mooney viscosity of 65, Japan Zeon Co., Ltd.), 5 parts by weight of zinc oxide (Beijing Inokai), 1 part by weight of stearic acid (Beijing Inokai), 50 parts by weight of N-220 carbon black (Tianjin Baochi Chemical), 2 parts by weight of antioxidant RD (Ningkang Chemical), 8 parts by weight of peroxide vulcanizing agent F-40 (Beijing Inokai) and 2 parts by weight of triallyl isocyanurate (vulcanizing agent, Beijing Inokai) are mixed in an internal mixer, and then vulcanized in a common flat vulcanizing press at 180°C for 10 minutes, and then the vulcanized hydrogenated nitrile rubber is obtained after physical crushing.
[0118] (12) In the following examples, the β-crystal nucleating agent with the brand name VP101B was sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation. The sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.
[0119] Example 1
[0120] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0121] (1) Preparation of polypropylene composition A:
[0122] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component m is the above-mentioned mixed toughening agent 1#;
[0123] The components prepared above were weighed and mixed according to the proportions, wherein the mass fraction Wa of component a was 80 parts by weight, and the mass fraction Wm of component m was 20 parts by weight.
[0124] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230° C. The screw was melt-mixed uniformly, extruded, granulated and dried to obtain polypropylene composition pellets. The melting point of the polypropylene composition A was tested to be 156° C.
[0125] (2) Preparation of polypropylene composition B:
[0126] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component n is the above-mentioned mixed toughening agent 1#;
[0127] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wn of component n is 15 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and the melting point thereof is detected to be 137° C.;
[0128] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0129] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering machine, and the polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion casting machine.
[0130] After the pellets are co-extruded and compounded out from the die of the extruder, they are sequentially passed through a calendering roller and a traction roller, and then subjected to solid phase stretching, edge cutting and winding, thereby obtaining the sheet.
[0131] The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 55°C. The temperature during the solid phase stretching was 135°C, the stretching rate was 2m / min, and the stretching ratio was 6 times. After stretching, the film was rolled up to form a polypropylene sheet (composite film), which consisted of an upper surface layer (film layer A), a core layer (film layer A), and a lower surface layer (film layer B).
[0132] The thickness of the polypropylene sheet (composite film) is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.
[0133] (4) Preparation of polypropylene fabric:
[0134] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain a plain weave polypropylene fabric.
[0135] (5) Preparation of polypropylene composite materials:
[0136] The polypropylene fabrics obtained in the above step (4) are laminated and hot pressed in sequence to form a laminated polypropylene sheet. The laminated polypropylene sheet includes 24 layers of polypropylene fabrics, and the polypropylene fabrics are placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5Mpa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.67mm.
[0137] Example 2
[0138] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0139] (1) Preparation of polypropylene composition A:
[0140] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1 g / 10 min, and an isotacticity of 97%; component m is SEBS (Kraton 1652, USA);
[0141] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wm of component m is 30 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B is added. Then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melted and mixed uniformly, extruded, granulated and dried, polypropylene composition pellets are obtained. The melting point of the polypropylene composition A is tested to be 160°C.
[0142] (2) Preparation of polypropylene composition B:
[0143] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 134°C, an ethylene-propylene-butene terpolymer, and a melt flow rate of 5.2 g / 10 min; component n is SEBS (Kraton 1652, USA);
[0144] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 80 parts by weight, the mass fraction Wn of component n is 20 parts by weight, and the other steps are the same as step (1), and finally polypropylene composition B pellets are obtained. The melting point of the polypropylene composition B is 129°C after testing.
[0145] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0146] The preparation process is the same as step (3) of Example 1.
[0147] (4) Preparation of polypropylene fabric:
[0148] The preparation process is the same as step (4) of Example 1.
[0149] (5) Preparation of polypropylene composite materials:
[0150] The preparation process is the same as step (5) of Example 1.
[0151] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0152] Example 3
[0153] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0154] (1) Preparation of polypropylene composition A:
[0155] Same as Example 1, wherein component m is a propylene-based elastomer (Mobil VISTAMAXX 6102); the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wm of component m is 10 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with a grade of VP101B is added. Polypropylene composition A pellets are obtained, and the melting point of the polypropylene composition A is 158°C after testing.
[0156] (2) Preparation of polypropylene composition B:
[0157] The same as Example 1, wherein component n is a propylene-based elastomer (Mobil VISTAMAXX 6102); the mass fraction Wx of component x is 90 parts by weight, and the mass fraction Wn of component n is 10 parts by weight, and finally a polypropylene composition B pellet is obtained. The melting point of the polypropylene composition B is 138°C after testing.
[0158] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0159] The preparation process is the same as step (3) of Example 1.
[0160] (4) Preparation of polypropylene fabric:
[0161] The preparation process is the same as step (4) of Example 1.
[0162] (5) Preparation of polypropylene composite materials:
[0163] The preparation process is the same as step (5) of Example 1.
[0164] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0165] Example 4
[0166] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0167] (1) Preparation of polypropylene composition A:
[0168] Same as Example 1, wherein component m is the mixed toughening agent 2# mentioned above; polypropylene composition A pellets are obtained, and the melting point of the polypropylene composition A is 155°C after testing.
[0169] (2) Preparation of polypropylene composition B:
[0170] Same as Example 1, wherein component n is the mixed toughening agent 2# mentioned above; finally, pellets of polypropylene composition B are obtained. The melting point of polypropylene composition B is found to be 136°C.
[0171] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0172] The preparation process is the same as step (3) of Example 1.
[0173] (4) Preparation of polypropylene fabric:
[0174] The preparation process is the same as step (4) of Example 1.
[0175] (5) Preparation of polypropylene composite materials:
[0176] The preparation process is the same as step (5) of Example 1.
[0177] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0178] Example 5
[0179] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0180] (1) Preparation of polypropylene composition A:
[0181] The same as Example 1, wherein component m is the mixed toughening agent 3# mentioned above; a pellet of polypropylene composition A is obtained, and the melting point of the polypropylene composition A is 153°C after testing.
[0182] (2) Preparation of polypropylene composition B:
[0183] Same as Example 1, wherein component n is the mixed toughening agent 3# mentioned above; finally, pellets of polypropylene composition B are obtained. The melting point of polypropylene composition B is found to be 135°C.
[0184] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0185] The preparation process is the same as step (3) of Example 1.
[0186] (4) Preparation of polypropylene fabric:
[0187] The preparation process is the same as step (4) of Example 1.
[0188] (5) Preparation of polypropylene composite materials:
[0189] The preparation process is the same as step (5) of Example 1.
[0190] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0191] Example 6
[0192] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0193] (1) Preparation of polypropylene composition A:
[0194] Same as Example 1, wherein component m is the above-mentioned sulfide hydrogenated nitrile rubber, namely raw material (11); polypropylene composition A pellets are obtained, and the melting point of the polypropylene composition A is 156°C after testing.
[0195] (2) Preparation of polypropylene composition B:
[0196] Same as Example 1, wherein component n is the above-mentioned sulfide hydrogenated nitrile rubber, namely raw material (11); finally, pellets of polypropylene composition B are obtained. The melting point of polypropylene composition B is 138°C after testing.
[0197] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0198] The preparation process is the same as step (3) of Example 1.
[0199] (4) Preparation of polypropylene fabric:
[0200] The preparation process is the same as step (4) of Example 1.
[0201] (5) Preparation of polypropylene composite materials:
[0202] The preparation process is the same as step (5) of Example 1.
[0203] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0204] Example 7
[0205] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0206] (1) Preparation of polypropylene composition A:
[0207] The same as Example 1, wherein component m is POE-g-MAH; polypropylene composition A pellets are obtained, and the melting point of the polypropylene composition A is 152°C after testing.
[0208] (2) Preparation of polypropylene composition B:
[0209] Same as Example 1, wherein component n is POE-g-MAH; finally, pellets of polypropylene composition B are obtained. The melting point of polypropylene composition B is 133°C after testing.
[0210] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0211] The preparation process is the same as step (3) of Example 1.
[0212] (4) Preparation of polypropylene fabric:
[0213] The preparation process is the same as step (4) of Example 1.
[0214] (5) Preparation of polypropylene composite materials:
[0215] The preparation process is the same as step (5) of Example 1.
[0216] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0217] Example 8
[0218] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0219] (1) Preparation of polypropylene composition A:
[0220] The preparation process is the same as step (1) of Example 1.
[0221] (2) Polypropylene composition B i Preparation:
[0222] The main preparation process is the same as step (2) of Example 1. The difference is that component B i Medium i The materials selected are as follows:
[0223] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min, and a melting point of 130°C;
[0224] Component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min, and a melting point of 135°C;
[0225] Component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.3, a melt flow rate of 6.6 g / 10 min, and a melting point of 140°C;
[0226] Component n is still the above mixed toughening agent 1#;
[0227] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +n=B i , i=1, 2, 3), after testing, the melting point of B1 is 128°C, the melting point of B2 is 133°C, and the melting point of B3 is 138°C.
[0228] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0229] The preparation process is the same as step (3) of Example 1. Sheets B1AB1, B2AB2, and B3AB3 are obtained respectively.
[0230] (4) Preparation of polypropylene fabric:
[0231] The preparation process is the same as step (4) of Example 1. Plain woven polypropylene fabrics B1AB1, B2AB2, and B3AB3 are obtained.
[0232] (5) Preparation of polypropylene composite materials:
[0233] The polypropylene fabrics obtained in the above step (4) are stacked in order, from bottom to top, B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 90s, hot pressing time 90s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 412μm.
[0234] Example 9
[0235] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0236] (1) Preparation of polypropylene composition A:
[0237] The preparation process is the same as step (1) of Example 1.
[0238] (2) Polypropylene composition B i Preparation:
[0239] The main preparation process is the same as step (2) of Example 1. The difference is that component B i Medium i The materials selected are as follows:
[0240] Components x1-x4 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 128°C; components x5-x8 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 135°C; components x9-x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 142°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.
[0241] Component n is still the above mixed toughening agent 1#;
[0242] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +n=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12). After testing, the melting points of B1-B4 are 127°C, the melting points of B5-B8 are 135°C, and the melting points of B9-B 12 The melting point is 141°C.
[0243] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0244] The preparation process is the same as step (3) of Example 1.
[0245] (4) Preparation of polypropylene fabric:
[0246] The preparation process is the same as step (4) of Example 1.
[0247] (5) Preparation of polypropylene composite materials:
[0248] The polypropylene fabrics obtained in step (4) are stacked in order, from bottom to top: B 12 AB 12 …B3AB3, B2AB2, B1AB1, B1AB1, B2AB2, B3AB3, …B 12 AB 12 The total number of stacked layers is 24, and the laminated polypropylene fabric is hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed in a direction of 90 degrees between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 160s, hot pressing time 160s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.66mm.
[0249] Comparative Example 1
[0250] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0251] (1) Preparation of polypropylene composition A:
[0252] Same as Example 1, but without adding component m;
[0253] (2) Preparation of polypropylene composition B:
[0254] Same as Example 1, but without adding component n;
[0255] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0256] The preparation process is the same as step (3) of Example 1.
[0257] (4) Preparation of polypropylene fabric:
[0258] The preparation process is the same as step (4) of Example 1.
[0259] (5) Preparation of polypropylene composite materials:
[0260] The preparation process is the same as step (5) of Example 1.
[0261] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0262] Comparative Example 2
[0263] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0264] (1) Preparation of polypropylene composition A:
[0265] Same as Example 1.
[0266] (2) Preparation of polypropylene composition B:
[0267] Same as Example 1, but without adding component n;
[0268] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0269] The preparation process is the same as step (3) of Example 1.
[0270] (4) Preparation of polypropylene fabric:
[0271] The preparation process is the same as step (4) of Example 1.
[0272] (5) Preparation of polypropylene composite materials:
[0273] The preparation process is the same as step (5) of Example 1.
[0274] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0275] Comparative Example 3
[0276] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0277] (1) Preparation of polypropylene composition A:
[0278] Same as Example 1, but without adding component n;
[0279] (2) Preparation of polypropylene composition B:
[0280] Same as Example 1.
[0281] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0282] The preparation process is the same as step (3) of Example 1.
[0283] (4) Preparation of polypropylene fabric:
[0284] The preparation process is the same as step (4) of Example 1.
[0285] (5) Preparation of polypropylene composite materials:
[0286] The preparation process is the same as step (5) of Example 1.
[0287] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0288] Comparative Example 4
[0289] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0290] (1) Preparation of polypropylene composition A:
[0291] Same as Example 1. However, m is a polypropylene impact copolymer prepared by Sinopec Beijing Research Institute of Chemical Industry (under the test condition of 23°C, the impact strength is 23KJ / m 2 ), ethylene content of 11%wt, melt flow rate of 2.0g / 10min, melting point of 155°C. The melting point of the polypropylene composition A was found to be 157°C.
[0292] (2) Preparation of polypropylene composition B:
[0293] Same as Example 1;
[0294] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0295] The preparation process is the same as step (3) of Example 1.
[0296] (4) Preparation of polypropylene fabric:
[0297] The preparation process is the same as step (4) of Example 1.
[0298] (5) Preparation of polypropylene composite materials:
[0299] The preparation process is the same as step (5) of Example 1.
[0300] Comparative Example 5
[0301] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0302] (1) Preparation of polypropylene composition A:
[0303] Same as Example 1.
[0304] (2) Preparation of polypropylene composition B:
[0305] Same as Example 1, but component n is petroleum resin (C5 Lanzhou Petrochemical), and finally polypropylene composition B pellets are obtained, and the melting point thereof is 135°C after detection;
[0306] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0307] The preparation process is the same as step (3) of Example 1.
[0308] (4) Preparation of polypropylene fabric:
[0309] The preparation process is the same as step (4) of Example 1.
[0310] (5) Preparation of polypropylene composite materials:
[0311] The preparation process is the same as step (5) of Example 1.
[0312] Comparative Example 6
[0313] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0314] (1) Preparation of polypropylene composition A:
[0315] Same as Example 1. However, m is a polypropylene impact copolymer prepared by Sinopec Beijing Research Institute of Chemical Industry (under the test condition of 23°C, the impact strength is 23KJ / m 2 ), ethylene content of 11%wt, melt flow rate of 2.0g / 10min, melting point of 155°C. The melting point of polypropylene composition A was found to be 157°C.
[0316] (2) Preparation of polypropylene composition B:
[0317] Same as Example 1, but component n is petroleum resin (C5 Lanzhou Petrochemical), and finally polypropylene composition B pellets are obtained, and the melting point thereof is 135°C after detection;
[0318] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0319] The preparation process is the same as step (3) of Example 1.
[0320] (4) Preparation of polypropylene fabric:
[0321] The preparation process is the same as step (4) of Example 1.
[0322] (5) Preparation of polypropylene composite materials:
[0323] The preparation process is the same as step (5) of Example 1.
[0324] Comparative Example 7
[0325] According to the method of Example 8, a three-layer coextruded polypropylene sheet and a polypropylene fabric were prepared.
[0326] The difference lies in the preparation of the polypropylene composite material. The prepared polypropylene fabrics are stacked in sequence, from bottom to top, B1A1B1, B2A2B2, B3A3B3, B2A2B2, B1A1B1, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 110s, hot pressing time 110s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 416μm.
[0327] Comparative Example 8
[0328] According to the method of Example 9, a three-layer coextruded polypropylene sheet and a polypropylene fabric were prepared.
[0329] The difference lies in the preparation of the polypropylene composite material. The prepared polypropylene fabrics are stacked in sequence, from bottom to top, B1AB 1… B 10 AB 10 , B 11 AB 11 , B 12 AB 12 , B 12 AB 12 , B 11 AB 11 , B 10 AB 10 , ...B1AB1 The total number of stacked layers is 24, and the laminated polypropylene fabric is hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed in a direction of 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 160s, hot pressing time 160s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.60mm.
[0330] Experimental example
[0331] The polypropylene composite materials obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.
[0332] (1) Tensile strength: Sample preparation and determination shall be carried out in accordance with the method specified in GB / T1040.1-2018.
[0333] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.
[0334] (3) Low temperature (-20°C) drop hammer impact strength: measured according to the method specified in GB / T14153-1993. The thicknesses of the polypropylene composite materials obtained in Examples 1-5 and Comparative Examples 1-5 are similar, about 1.6 mm, and are all within the range of 1.6 mm ± 1 mm.
[0335] Table 1
[0336]
[0337]
[0338] The examples and test results in Table 1 show that the polypropylene composite material prepared according to the present invention has good tensile properties and low-temperature impact properties, and has good interlayer peel strength at a relatively low hot pressing temperature. When the polypropylene composite material of the present invention is hot-pressed with 24 layers of polypropylene fabric and has a thickness of about 1.6 mm, the low-temperature drop hammer impact strength at -20°C is ≥160J.
[0339] It can be seen from Comparative Examples 1-8 that, compared with Example 1 of the present invention, a series of comparative examples that do not use the toughening component m / n or use conventional impact copolymer polypropylene as the m component and use conventional binder C5 petroleum resin as the n component show that the low-temperature impact performance and interlayer peel strength of the obtained polypropylene composite material cannot be achieved at the same time, and both are reduced, among which the low-temperature impact performance is significantly reduced.
[0340] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0341] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. An impact-resistant polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB'; Wherein layer A contains polypropylene composition A, and the polypropylene composition A includes homopolymer polypropylene a and toughening agent m; layer B and layer B' are the same or different, and each correspondingly contains polypropylene composition B and polypropylene composition B', and the polypropylene composition B and the polypropylene composition B' each include random copolymer polypropylene x and toughening agent n; in, The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'; The toughening agent m and the toughening agent n are the same or different, and are each selected from an elastic material.
2. The impact-resistant polypropylene sheet according to claim 1, Features: The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10° C.; and / or, The difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C; and / or, based on the total thickness of the impact-resistant polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.
3. The impact-resistant polypropylene sheet according to claim 1, Features: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-98 wt% of homopolypropylene a and 2-50 wt% of toughening agent m; preferably, the polypropylene composition A comprises 70-90 wt% of homopolypropylene a and 10-30 wt% of toughening agent m; and / or, Based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 70-98wt% of random copolymer polypropylene x and 2-50wt% of toughening agent n; preferably, the polypropylene composition B and the polypropylene composition B' each include 70-90wt% of random copolymer polypropylene x and 10-30wt% of toughening agent n.
4. The impact-resistant polypropylene sheet according to any one of claims 1 to 3, Features: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.
5. The impact-resistant polypropylene sheet according to any one of claims 1 to 3, Features: The toughening agent m and the toughening agent n are each selected from elastomers and / or soft biodegradable materials; preferably, The toughening agent m and the toughening agent n are each selected from at least one of the following substances and / or at least one modified substance of the following substances: polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, biodegradable polyester, natural rubber, bio-based elastomer, special rubber; more preferably, The toughening agent m and the toughening agent n are each selected from at least one of the following substances and / or at least one modified substance of the following substances: polybutylene adipate terephthalate, polybutylene terephthalate succinate, polybutylene succinate and copolymers thereof, polycaprolactone, natural rubber, hydrogenated nitrile rubber, polyolefin elastomer; more preferably, The toughening agent m and the toughening agent n are each selected from at least one of the following substances and / or at least one modified substance of the following substances: polyolefin elastomer, hydrogenated nitrile rubber.
6. The impact-resistant polypropylene sheet according to any one of claims 1 to 3, Features: The toughening agent m and the toughening agent n are each selected from polyolefin elastomer maleic anhydride modified product and hydrogenated nitrile rubber; preferably, The weight ratio of the maleic anhydride modified polyolefin elastomer to the hydrogenated nitrile rubber is 0.2 to 5; more preferably, The polyolefin elastomer is a copolymer elastomer of ethylene and the following olefins: propylene and / or α-olefin; more preferably, the α-olefin is a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene.
7. The impact-resistant polypropylene sheet according to any one of claims 1 to 3, Features: The random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
8. The impact-resistant polypropylene sheet according to any one of claims 1 to 3, Features: The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.
9. The impact-resistant polypropylene sheet according to any one of claims 1 to 3, Features: The BAB' sheet structure of the impact-resistant polypropylene sheet is obtained by co-extruding a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B'.
10. The method for preparing the impact-resistant polypropylene sheet according to any one of claims 1 to 9, comprising co-extruding, casting or calendering, and stretching a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B' according to a BAB' structure to obtain the impact-resistant polypropylene sheet.
11. The method for preparing the impact-resistant polypropylene sheet according to claim 10, It is characterized in that The preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a and the toughening agent m; and / or, The preparation of the raw materials for the layers B and B' comprises melt blending the components including the random copolymer polypropylene x and the toughening agent n; and / or, The co-extrusion and casting temperatures are independently selected from 200-240° C.; and / or, The calendering temperature is 50-70°C; and / or, The stretching conditions include: the stretching temperature is 90-165° C., preferably 90-140° C., and more preferably 90-119° C.; and the stretching ratio is 1-20 times.
12. An impact-resistant polypropylene fabric, a three-dimensional polypropylene fabric obtained by weaving the impact-resistant polypropylene sheet according to any one of claims 1 to 9; Preferably, the impact-resistant polypropylene fabric is obtained by slitting and weaving the impact-resistant polypropylene sheet; and / or the impact-resistant polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
13. An impact-resistant polypropylene composite material, wherein the impact-resistant polypropylene composite material is prepared by hot pressing multiple layers of the impact-resistant polypropylene sheet according to any one of claims 1 to 9 and / or the impact-resistant polypropylene fabric according to claim 12; preferably, The impact-resistant polypropylene composite material is prepared by thermally pressing multiple layers of the impact-resistant polypropylene sheets or the impact-resistant polypropylene fabric; and / or, The multi-layer impact-resistant polypropylene sheets are stacked from top to bottom in the direction of 0-90° along their respective machine directions; and / or, The multi-layer impact-resistant polypropylene fabric is stacked from top to bottom with the warp direction and the warp direction being 0-90 degrees apart; and / or, The number of layers of the multi-layer impact-resistant polypropylene sheet and / or the multi-layer impact-resistant polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers, and most preferably 4-100 layers.
14. The impact-resistant polypropylene composite material according to claim 13, Features: The impact-resistant polypropylene composite material comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the impact-resistant polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group.
15. The impact-resistant polypropylene composite material according to claim 14, Features: Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 2≤n≤100, preferably, 2≤n≤50; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.
16. A method for preparing the impact-resistant polypropylene composite material according to any one of claims 13 to 15, the method comprising laminating and hot-pressing the impact-resistant polypropylene sheet and / or the impact-resistant polypropylene fabric, and then cooling and shaping to prepare the impact-resistant polypropylene composite material; preferably, The temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, The pressure of the hot pressing fusion is 2-10 MPa; and / or, The preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, The cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s; and / or, the number of layers of the impact-resistant polypropylene sheet and / or the impact-resistant polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers; and / or, Adjacent layers of the impact-resistant polypropylene fabric laminate are placed at an angle of 0-90° between the warp direction and the warp direction; and / or, Adjacent layers of the impact resistant polypropylene sheet laminate are placed at 0-90 degrees along their respective machine directions.
17. Use of the impact-resistant polypropylene sheet according to any one of claims 1 to 9, the impact-resistant polypropylene fabric according to claim 12, the impact-resistant polypropylene composite material according to any one of claims 13 to 15, and the impact-resistant polypropylene composite material prepared by the preparation method according to claim 16 in the fields of electrical component packaging, automobile manufacturing, military materials, and consumer products.
Citation Information
Patent Citations
High-adhesiveness and high-impact polypropylene composite film as well as preparation method and application thereof
CN115991033A
Low-haze high-impact heat-sealing polypropylene composite film as well as preparation method and application thereof
CN115991039A
Low-haze high-impact-resistance coloring heat-sealing polypropylene composite film as well as preparation method and application thereof
CN115991040A
High-adhesiveness and high-impact polypropylene composite film as well as preparation method and application thereof
CN115991042A
Low-haze high-impact heat-sealing polypropylene composite film as well as preparation method and application thereof
CN115991907A