Gold stamping material, preparation method thereof and application of gold stamping material to electronic product shell
Through the technology of mica powder and nanotitanium dioxide composite and nanosilicon dioxide filling pores, the problem of poor corrosion resistance of gold stamping patterns in electronic products shells is solved, and the long-term stable existence and high durability of the patterns are achieved.
Patent Information
- Application Number
- CN202410973643.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The gold stamping pattern on the shell of electronic products has poor corrosion resistance, and the high frequency of use leads to a decrease in the pattern quality.
Mica powder is combined with nanotitanium dioxide, and a layered arrangement structure is formed through the cross-linking process, and the pores are filled with nanosilica, which enhances the corrosion resistance and density of the coating film to form a new hot stamping material.
It significantly improves the corrosion resistance and aging resistance of hot stamping patterns, so that the pattern exists stably on the substrate for a long time and extends its service life.
Smart Images

Figure BDA0004953929680000161 
Figure BDA0004953929680000171
Abstract
Description
Technical Field
[0001] The present application relates to the field of hot stamping technology, and in particular to a hot stamping material and a preparation method thereof, and an application thereof in electronic product housings. Background Art
[0002] The hot stamping process uses the principle of heat transfer to transfer the metal layer to the surface of the substrate to form a special metal effect. The hot stamping paper used in the hot stamping process is composed of polyester film and multiple chemical coatings coated on its surface. Hot stamping paper generally includes polyester film, release layer, imaging layer, metal layer and adhesive layer. The release layer isolates the metal layer from the polyester film and is easy to separate during hot stamping. The imaging layer mainly displays the color of the hot stamping paper. After hot stamping, it is covered on the surface of the hot stamping pattern to play a protective role. The adhesive layer acts as a binder to connect the hot stamping paper and the substrate.
[0003] With the rapid development of electronic products, people are paying more and more attention to the appearance of electronic products. It is a common method for people to use hot stamping to form unique patterns or logos on the shell of electronic products. However, due to the increasing frequency of daily use of electronic products, the patterns on the shell of electronic products have gradually shown problems of general quality and poor corrosion resistance. Summary of the invention
[0004] In order to improve the corrosion resistance of the pattern after hot stamping, the present application provides a hot stamping material and a preparation method thereof and an application thereof in the housing of an electronic product.
[0005] In the first aspect, the present application provides a hot stamping material, which adopts the following technical solution:
[0006] A hot stamping material, comprising a base film, a release layer, an imaging layer, a metal layer and an adhesive layer;
[0007] The coating used for the imaging layer includes the following components by weight: 20-25 parts of acrylic resin, 5-10 parts of amino resin, 75-85 parts of organic solvent, 3-5 parts of nano silicon dioxide and 3-5 parts of mica powder composite nano titanium dioxide.
[0008] By adopting the above technical scheme, acrylic resin and amino resin are cross-linked, and mica powder composite nano titanium dioxide is dispersed in the coating during the curing process. When the coating is cured, the mica powder is affected by the surface tension and forms a layered arrangement structure parallel to each other and the surface of the coating on the coating. This layered arrangement structure can fully block water, oxygen and other corrosive substances, thereby improving the corrosion resistance of the coating. In addition, titanium dioxide can improve the UV resistance, aging resistance and scrub resistance of the coating. Titanium dioxide is compounded with mica powder, and titanium dioxide is evenly distributed in the layered arrangement structure formed by mica powder, thereby greatly improving the corrosion resistance and aging resistance of the coating. In addition, nano silicon dioxide further fills the pores in the coating, thereby further improving the compactness of the coating, blocking the erosion of water, oxygen, etc. to the coating, and can further improve the comprehensive performance of the coating. Therefore, the imaging layer covers the surface of the metal layer, which effectively protects the metal layer, so that the pattern after hot stamping can exist stably on the surface of the substrate for a long time, showing a longer service life.
[0009] In a specific embodiment, the mica powder composite nano-titanium dioxide is prepared as follows:
[0010] The nano-titanium dioxide and silane coupling agent solution are mixed, heated for reaction, and then chitosan-coated mica powder is added, and the reaction is continued. After the reaction, the mixture is centrifuged to obtain mica powder composite nano-titanium dioxide.
[0011] In a specific embodiment, the chitosan-coated mica powder is prepared by spraying a chitosan dilute acid solution of a certain concentration on the surface of the mica powder to obtain the chitosan-coated mica powder after film formation.
[0012] In a specific embodiment, the chitosan dilute acid solution has a mass concentration of 2-3%.
[0013] By adopting the above technical scheme, on the one hand, nano titanium dioxide and mica powder are effectively compounded through the connection between chitosan and silane coupling agent; on the other hand, the interaction between chitosan and acrylic resin can make mica powder exist stably in the coating film, which helps to form a dense network structure in the coating film.
[0014] In a specific embodiment, the mass ratio of the mica powder to nano-titanium dioxide is 1:(2-3).
[0015] In a specific embodiment, the mica powder has a size of 100-200 mesh, and the nano titanium dioxide has a size of 30-50 nm.
[0016] By adopting the above technical solution, suitable proportions and suitable specifications, mica powder and nano-titanium dioxide can form an effective composite.
[0017] In a specific embodiment, the particle size of the nano-silicon dioxide is 80-100 nm.
[0018] By adopting the above technical solution, the appropriate particle size can reduce the possibility of nano-silicon dioxide agglomeration in the system, which helps the nano-silicon dioxide to disperse in the system and fill in the pores, so that the coating forms a dense structure.
[0019] In a specific embodiment, the nano-silica is pre-treated with silane polyethylene glycol amino groups.
[0020] By adopting the above technical scheme, when the nano-silica is treated with silane polyethylene glycol amino groups, the groups generated by silane hydrolysis react with the nano-silica, and the polyethylene glycol segments stretch in the coating and participate in the cross-linking and curing of the coating, thereby increasing the density of the coating. At the same time, the amino groups can form hydrogen bonds with the chitosan on the surface of the mica powder, thereby connecting the nano-silica and the mica powder, ensuring the stability of the nano-silica and the mica powder in the coating, thereby effectively ensuring that the coating has high corrosion resistance.
[0021] In a specific embodiment, the amino resin is selected from melamine formaldehyde resin, methyl etherified melamine resin, and n-butyl etherified melamine resin.
[0022] In a specific embodiment, the organic solvent is selected from toluene, butanone, and cyclohexanone.
[0023] In a second aspect, the present application provides a method for preparing a hot stamping material, using the following technical solution:
[0024] A method for preparing a hot stamping material comprises the following steps: coating a release layer on a base film and drying; coating an imaging layer on the release layer and drying; plating a metal layer on the imaging layer; and coating an adhesive layer on the metal layer to obtain hot stamping paper.
[0025] In a third aspect, the present application provides an application of a hot stamping material, using the following technical solution:
[0026] The invention discloses an application of hot stamping material, which is applied to the housing of electronic products.
[0027] In summary, the present application includes at least one of the following beneficial technical effects:
[0028] 1. The present application combines mica powder and nano-titanium dioxide so that the nano-titanium dioxide is evenly distributed in the coating film by virtue of the layered arrangement of the mica powder in the coating film. The combination of the two greatly improves the corrosion resistance of the imaging layer, so that the hot stamping pattern can be permanently and stably present on the surface of the substrate;
[0029] 2. The present application utilizes the function of nano-silicon dioxide in filling gaps in the coating film, so that the density of the coating film is further improved, thereby further improving the corrosion resistance of the imaging layer. DETAILED DESCRIPTION
[0030] The present application is further described in detail below with reference to the embodiments.
[0031] In the present application, the acrylic resin model is HK75010; the amino resin is specifically melamine formaldehyde resin, model HA9161; aminopolyethylene glycol silane is purchased from Pengshuo Biotechnology; other raw materials such as the coating used for the release layer and the adhesive used for the adhesive layer can be obtained commercially.
[0032] Preparation Example 1
[0033] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 2%. The chitosan dilute acid solution was sprayed on the surface of 100-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 30nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:2, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 1:2 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, the mica powder was centrifuged to obtain mica powder composite nano-titanium dioxide.
[0034] Preparation Example 2
[0035] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 3%. The chitosan dilute acid solution was sprayed on the surface of 100-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 30nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:2, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 1:2 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, centrifugation was performed to obtain mica powder composite nano-titanium dioxide.
[0036] Preparation Example 3
[0037] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 2%. The chitosan dilute acid solution was sprayed on the surface of 100-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 30nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:3, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 1:2 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, centrifugation was performed to obtain mica powder composite nano-titanium dioxide.
[0038] Preparation Example 4
[0039] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 2%. The chitosan dilute acid solution was sprayed on the surface of 200-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 50nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:2, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 1:2 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, centrifugation was performed to obtain mica powder composite nano-titanium dioxide.
[0040] Preparation Example 5
[0041] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 2%. The chitosan dilute acid solution was sprayed on the surface of 500-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 30nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:2, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 1:2 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, the mica powder was centrifuged to obtain mica powder composite nano-titanium dioxide.
[0042] Preparation Example 6
[0043] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 2%. The chitosan dilute acid solution was sprayed on the surface of 100-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 100nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:2, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 1:2 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, centrifugation was performed to obtain mica powder composite nano-titanium dioxide.
[0044] Preparation Example 7
[0045] Chitosan was dissolved in a dilute acetic acid solution with a mass concentration of 1% to prepare a chitosan dilute acid solution with a mass concentration of 2%. The chitosan dilute acid solution was sprayed on the surface of 100-mesh mica powder to obtain chitosan-coated mica powder after film formation, wherein the mass ratio of the chitosan dilute acid solution to the mica powder was 1:1. 30nm nano-titanium dioxide and a 3% γ-(2,3-epoxypropoxy)propyltrimethoxysilane aqueous solution were mixed in a mass ratio of 1:2, heated to 75°C for reaction, and then chitosan-coated mica powder was added in a mass ratio of 2:1 to the mica powder and nano-titanium dioxide to continue the reaction. After the reaction was completed, the mica powder was centrifuged to obtain mica powder composite nano-titanium dioxide.
[0046] Example 1
[0047] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 1. wherein the specification of the nano-silicon dioxide is 80nm.
[0048] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0049] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0050] An adhesive is coated on the metal layer to form an adhesive layer.
[0051] Example 2
[0052] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 230g of acrylic resin, 50g of amino resin, 850g of toluene, 30g of nano-silicon dioxide and 40g of mica powder composite nano-titanium dioxide prepared in Preparation Example 1. wherein the specification of the nano-silicon dioxide is 80nm.
[0053] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0054] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0055] An adhesive is coated on the metal layer to form an adhesive layer.
[0056] Example 3
[0057] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 250g of acrylic resin, 100g of amino resin, 830g of toluene, 40g of nano-silicon dioxide and 50g of mica powder composite nano-titanium dioxide prepared in Preparation Example 1. wherein the specification of the nano-silicon dioxide is 80nm.
[0058] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0059] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0060] An adhesive is coated on the metal layer to form an adhesive layer.
[0061] Example 4
[0062] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 2. wherein the specification of the nano-silicon dioxide is 80nm.
[0063] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0064] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0065] An adhesive is coated on the metal layer to form an adhesive layer.
[0066] Example 5
[0067] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 3. wherein the specification of the nano-silicon dioxide is 80nm.
[0068] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0069] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0070] An adhesive is coated on the metal layer to form an adhesive layer.
[0071] Example 6
[0072] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 4. wherein the specification of the nano-silicon dioxide is 80nm.
[0073] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0074] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0075] An adhesive is coated on the metal layer to form an adhesive layer.
[0076] Example 7
[0077] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 5. wherein the specification of the nano-silicon dioxide is 80nm.
[0078] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0079] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0080] An adhesive is coated on the metal layer to form an adhesive layer.
[0081] Example 8
[0082] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 6. wherein the specification of the nano-silicon dioxide is 80nm.
[0083] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0084] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0085] An adhesive is coated on the metal layer to form an adhesive layer.
[0086] Example 9
[0087] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 7. wherein the specification of the nano-silicon dioxide is 80nm.
[0088] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0089] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0090] An adhesive is coated on the metal layer to form an adhesive layer.
[0091] Example 10
[0092] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 1. The specification of the nano-silicon dioxide is 100nm.
[0093] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0094] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0095] An adhesive is coated on the metal layer to form an adhesive layer.
[0096] Embodiment 11
[0097] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 1. wherein the specification of the nano-silicon dioxide is 30nm.
[0098] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0099] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0100] An adhesive is coated on the metal layer to form an adhesive layer.
[0101] Example 12
[0102] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder composite nano-titanium dioxide prepared in Preparation Example 1. wherein the specification of the nano-silicon dioxide is 80nm; the nano-silicon dioxide is treated with aminopolyethylene glycol silane in advance, specifically, the aminopolyethylene glycol silane is dissolved in water to prepare an aqueous solution with a mass concentration of 3%, and then the nano-silicon dioxide is added to the aqueous solution, the mass ratio of the two is 1:2, and the reaction is carried out at 70°C, and the obtained material is obtained after the reaction is completed.
[0103] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0104] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0105] An adhesive is coated on the metal layer to form an adhesive layer.
[0106] Application Example 1
[0107] A hot stamping material is applied to the shells of electronic products such as mobile phones, computers, etc. The hot stamping material is prepared by Example 1.
[0108] Application Example 2
[0109] A hot stamping material is applied to the shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 2.
[0110] Application Example 3
[0111] A hot stamping material is applied to the shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 3.
[0112] Application Example 4
[0113] A hot stamping material is applied to the shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 4.
[0114] Application Example 5
[0115] A hot stamping material is applied to the shells of electronic products such as mobile phones and computers. The hot stamping material is prepared according to Example 5.
[0116] Application Example 6
[0117] A hot stamping material is used for the outer shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 6.
[0118] Application Example 7
[0119] A hot stamping material is used for the outer shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 7.
[0120] Application Example 8
[0121] A hot stamping material is used for the outer shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 8.
[0122] Application Example 9
[0123] A hot stamping material is used for the outer shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 9.
[0124] Application Example 10
[0125] A hot stamping material is used for the outer shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 10.
[0126] Application Example 11
[0127] A hot stamping material is used for the outer shells of electronic products such as mobile phones and computers. The hot stamping material is prepared by Example 11.
[0128] Comparative Example 1
[0129] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used in the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of mica powder. wherein the mica powder has a specification of 100 mesh and the nano-silicon dioxide has a specification of 80nm.
[0130] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0131] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0132] An adhesive is coated on the metal layer to form an adhesive layer.
[0133] Comparative Example 2
[0134] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used in the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide and 30g of nano-titanium dioxide. The specification of the nano-titanium dioxide is 30nm, and the specification of the nano-silicon dioxide is 80nm.
[0135] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0136] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0137] An adhesive is coated on the metal layer to form an adhesive layer.
[0138] Comparative Example 3
[0139] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used in the imaging layer comprises 200g of acrylic resin, 70g of amino resin, 750g of toluene, 50g of nano-silicon dioxide, 10g of mica powder and 20g of nano-titanium dioxide. wherein the mica powder has a size of 100 mesh, the nano-titanium dioxide has a size of 30nm, and the nano-silicon dioxide has a size of 80nm.
[0140] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0141] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0142] An adhesive is coated on the metal layer to form an adhesive layer.
[0143] Comparative Example 4
[0144] A hot stamping material comprises a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; wherein the coating used for the imaging layer comprises 250g of acrylic resin, 70g of amino resin, 750g of toluene and 30g of mica powder composite nano titanium dioxide prepared in Preparation Example 1.
[0145] During the preparation, a base film coated with a release layer is taken, and the imaging layer coating is coated on the release layer, and cured at 160° C. to form an imaging layer;
[0146] Vacuum aluminum is deposited on the imaging layer to form a metal layer;
[0147] An adhesive is coated on the metal layer to form an adhesive layer.
[0148] Performance Testing
[0149] The hot stamping materials in each embodiment and each comparative example were respectively hot stamped on the detection panel under the same hot stamping conditions to form hot stamping patterns, and then the following tests were performed:
[0150] (1) The test panel was immersed in sodium hydroxide solutions of different concentrations, and the corrosion of the hot stamping pattern on the test panel was observed every 30 minutes. The time when the hot stamping pattern changed due to corrosion was recorded, as shown in Table 1.
[0151] (2) The water resistance of the hot stamping pattern on each test panel was tested with reference to GB / T 25264-2010 “Solvent-based acrylic resin coatings”.
[0152] (3) Referring to method B in GB / T 16422.3-2022, irradiate the hot stamping pattern on the test panel with ultraviolet light for 24 hours, and then repeat tests (1) and (2).
[0153] Table 1 Performance test results
[0154]
[0155]
[0156] It can be seen from Table 1 that compared with comparative examples 1-3, the hot stamping patterns in Examples 1-4 exhibit better corrosion resistance, indicating that the composite of mica powder and nano-titanium dioxide in the present application can effectively improve the corrosion resistance and aging resistance of the imaging layer, and greatly improve the stability of the hot stamping pattern on the substrate.
[0157] It can be seen from Example 1 and Comparative Example 4 that the addition of a certain amount of nano-silicon dioxide in the present application can better improve the corrosion resistance of the hot stamping pattern.
[0158] In combination with Example 1, Example 5 and Example 9, it can be seen that the ratio of mica powder and nano-titanium dioxide will affect the performance of mica powder composite nano-titanium dioxide on the coating. Preparing mica powder composite nano-titanium dioxide with reference to the ratio disclosed in this application can ensure that the imaging layer can exist stably and has better corrosion resistance.
[0159] It can be seen from Example 1 and Example 6 to Example 8 that by limiting the specifications of mica powder and nano-titanium dioxide, the mica powder and nano-titanium dioxide can be better compounded, so that the imaging layer exhibits better corrosion resistance.
[0160] It can be seen from Example 1, Example 10 and Example 11 that the appropriate particle size of nano-silicon dioxide helps it to disperse in the coating film, so that it can be better filled into the gaps in the coating film, improve the density of the coating film, and further improve the corrosion resistance of the imaging layer.
[0161] In combination with Example 1 and Example 12, the corrosion resistance of the imaging layer can be further improved after the nano-silicon dioxide is treated with.
[0162] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A hot stamping material, characterized in that: It includes a base film, a release layer, an imaging layer, a metal layer and an adhesive layer; The coating used for the imaging layer includes the following components by weight: 20-25 parts of acrylic resin, 5-10 parts of amino resin, 75-85 parts of organic solvent, 3-5 parts of nano silicon dioxide and 3-5 parts of mica powder composite nano titanium dioxide.
2. The hot stamping material according to claim 1, characterized in that: The preparation of the mica powder composite nano titanium dioxide is as follows: The nano-titanium dioxide and silane coupling agent solution are mixed, heated for reaction, and then chitosan-coated mica powder is added, and the reaction is continued. After the reaction, the mixture is centrifuged to obtain mica powder composite nano-titanium dioxide.
3. The hot stamping material according to claim 2, characterized in that: The chitosan-coated mica powder is prepared by spraying a chitosan dilute acid solution of a certain concentration on the surface of the mica powder to obtain the chitosan-coated mica powder after film formation.
4. The hot stamping material according to claim 3, characterized in that: The mass concentration of the chitosan dilute acid solution is 2-3%.
5. The hot stamping material according to claim 2, characterized in that: The mass ratio of the mica powder to nano titanium dioxide is 1:(2-3).
6. The hot stamping material according to claim 2, characterized in that: The specification of the mica powder is 100-200 meshes, and the specification of the nano titanium dioxide is 30-50nm.
7. The hot stamping material according to claim 1, characterized in that: The particle size of nano-silicon dioxide is 80-100nm.
8. The hot stamping material according to claim 1, characterized in that: The amino resin is selected from melamine formaldehyde resin, methyl etherified melamine resin, and n-butyl etherified melamine resin.
9. A method for preparing a hot stamping material according to any one of claims 1 to 8, characterized in that: The following steps are involved: The release layer is coated on the base film and dried; the imaging layer is coated on the release layer and dried; the imaging layer is plated with a metal layer; and the adhesive layer is coated on the metal layer to obtain the hot stamping paper.
10. Application of a hot stamping material according to any one of claims 1 to 8, characterized in that: Used in electronic product housings.