Air brake for aircraft and preparation method of air brake

By using carbon fiber reinforced composite materials and high silicone oxide cloth reinforced phenolic resin materials in the aircraft speed reduction board, combined with titanium alloy joints, the problem of insufficient mechanical properties of titanium alloy is solved, high strength, lightweight and heat resistance are achieved, and the Materials and processing costs.

CN118907391AInactive Publication Date: 2024-11-08BEIJING COMPOSITE MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411200548.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The mechanical properties of titanium alloys are difficult to meet the needs of high strength and lightweight. Especially in the applications of hypersonic aircraft, the strength, stiffness and temperature resistance of existing speed reduction plates under force and heat load are insufficient.

Method used

The reduction plate for aircraft is prepared by using carbon fiber reinforced double horse resin-based composite material or carbon fiber reinforced polyimide resin-based composite material as structural layer, and with high silicone oxygen cloth reinforced phenolic resin-based composite material as heat protection layer. , titanium alloy can be used in metal joints, combined with high-temperature resistant adhesive to improve strength and lightweight.

Benefits of technology

A high-strength and lightweight reduction plate is realized, which reduces interface combination differences, saves raw materials and processing time, avoids fiber damage, and obtains the advantages of integrated structural functions and lightweight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118907391A_ABST
    Figure CN118907391A_ABST
Patent Text Reader

Abstract

The invention provides an air brake for an aircraft and a preparation method of the air brake, and the air brake for the aircraft comprises a metal joint, a structural layer and a heat-proof layer, the metal joint is arranged at one end of the structural layer, and the heat-proof layer is arranged on the structural layer; the structural layer is made of a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material; and the heat-proof layer is made of a high-silica cloth reinforced phenolic resin-based composite material. According to the air brake for the aircraft and the preparation method of the air brake, the heat-proof layer and the structural layer are integrally pressed and formed, so that the possibility of poor interface bonding caused by a post-bonding technology of the heat-proof layer and the structural layer is reduced, and the air brake has the advantages of structure and function integration, light weight and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of airbrakes for aircraft, and in particular relates to an airbrake for aircraft and a preparation method thereof. Background Art

[0002] As a typical load-bearing structural component of an aircraft, the speed brake is used to adjust the flight resistance of the aircraft, play a resistance role during the landing and deceleration of the aircraft, and assist in controlling the flight speed. When the aircraft is working at high speed, the speed brake is at a higher temperature, which puts forward higher requirements on the strength, stiffness, temperature resistance and lightness of the speed brake under the coupled environment of force and thermal load.

[0003] For example, the Chinese patent document with publication number CN112173074A discloses a reusable high-temperature speed brake mechanism, the skin of which is made of titanium alloy material to improve the strength of the speed brake. However, with the rapid development of hypersonic aircraft, the mechanical properties of titanium alloys are difficult to meet the requirements of high strength and light weight.

[0004] Based on the above difficulties, it is very necessary to propose a high-strength and lightweight deceleration plate preparation method while ensuring the load-bearing and temperature-resistant requirements. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a deceleration plate for aircraft and a preparation method thereof, aiming to solve the problem that the mechanical properties of titanium alloys are difficult to meet the requirements of high strength and light weight.

[0006] In order to solve the above problems, the first aspect of the present invention provides a speed brake for an aircraft, comprising:

[0007] A metal joint, a structural layer and a heat-proof layer; the metal joint is arranged at one end of the structural layer, and the heat-proof layer is arranged on the structural layer;

[0008] The structural layer is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0009] The heat protection layer is a high-silica cloth reinforced phenolic resin-based composite material.

[0010] Preferably, the metal joint is made of titanium alloy material; the raw material for preparing the structural layer is one of T800 reinforced bismaleimide resin unidirectional prepreg, T800 reinforced polyimide resin unidirectional prepreg, T1000 reinforced polyimide resin unidirectional prepreg and T1000 reinforced bismaleimide resin unidirectional prepreg.

[0011] A second aspect of the present invention provides a method for preparing the above-mentioned aircraft speed brake, comprising the following steps:

[0012] S1: laying the prepreg of the structural layer on the lower mold, pre-compacting it to a theoretical thickness, installing the female mold frame and the upper mold, closing the mold, and then pre-curing and molding to obtain a pre-cured structural layer;

[0013] S2: dismantle the upper mold, the female mold frame and the lower mold to install the metal joint, and install the metal joint at a selected position on the pre-cured structural layer;

[0014] S3: Laying the prepreg of the heat protection layer on the precured structural layer to a theoretical thickness, and co-curing to obtain the speed brake for the aircraft.

[0015] Preferably, in step S1, the prepreg of the structural layer is laid in a symmetrical and alternating direction of ±45° and 0° / 90°; in step S3, the prepreg of the heat protection layer is laid in a symmetrical and alternating direction of ±45° and 0° / 90°.

[0016] Preferably, in step S1, after the first layer of the prepreg material of the structural layer is laid, vacuum pre-compacting is performed, and then vacuum pre-compacting is performed every 4-6 layers.

[0017] Preferably, the prepreg surface density of the structural layer is 100 to 300 g / m 2 , the volume content of the resin is 30-50%.

[0018] Preferably, the metal joint and the structural layer are fixed using a high temperature resistant adhesive.

[0019] Preferably, in step S1, the vacuuming time is 20 to 40 minutes, and the vacuum degree is ≤-0.08 MPa.

[0020] Preferably, in step S1, when the structural layer adopts carbon fiber reinforced bismaleimide resin prepreg, the precuring system is: room temperature rises to 150±15℃, keeps warm for 2~4h, and the pressure is 5~20MPa; from 150±15℃ to 200±15℃, keeps warm for 2~4h, and the pressure is 5~20MPa; from 200±15℃ to 250±15℃, keeps warm for 2~4h, and the pressure is 5~20MPa; when the structural layer adopts carbon fiber reinforced polyimide resin prepreg, the precuring system is: room temperature rises to 150±15℃, keeps warm for 2~4h, and the pressure is The pressure is 5-20MPa; from 150±15℃ to 200±15℃, keep warm for 2-4h, the pressure is 5-20MPa; from 200±15℃ to 250±15℃, keep warm for 2-4h, the pressure is 5-20MPa; from 250±15℃ to 300±15℃, keep warm for 2-4h, the pressure is 5-20MPa; from 300±15℃ to 350±15℃, keep warm for 2-4h, the pressure is 5-20MPa; from 350±15℃ to 400±15℃, keep warm for 2-4h, the pressure is 5-20MPa.

[0021] Preferably, in step S3, the curing system of the heat protection layer is: the room temperature is raised to 120±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 120±15°C to 140±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 140±15°C to 180±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 180±15°C to 220±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The aircraft speed brake of the present invention has a structural layer and a heat protection layer made of composite materials, which can meet the requirements of high strength and light weight. The preparation method of the aircraft speed brake of the present invention adopts the method of integrally pressing the heat protection layer and the structural layer to reduce the possibility of poor interface bonding caused by the post-bonding technology of the heat protection layer and the structural layer. At the same time, the net size molding technology is adopted to save the cost of raw materials and processing time and avoid fiber damage caused by processing. The obtained speed brake has the advantages of structural and functional integration and light weight. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a schematic diagram of a speed brake product for an aircraft according to an embodiment of the present invention;

[0025] Among them, 1-metal joint; 2-structural layer; 3-heat protection layer. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] A first aspect of an embodiment of the present invention provides a speed brake for an aircraft, comprising:

[0028] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0029] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0030] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0031] The aircraft speed brake of the embodiment of the present invention has a structural layer 2 and a heat protection layer 3 made of composite materials, which can meet the requirements of high strength and light weight. The preparation method of the aircraft speed brake of the embodiment of the present invention adopts a method of integrally pressing the heat protection layer 3 and the structural layer 2, which reduces the possibility of poor interface bonding caused by post-bonding technology between the heat protection layer and the structural layer. At the same time, the net size molding technology is adopted to save raw material costs and processing time and avoid fiber damage caused by processing. The obtained speed brake has the advantages of structural and functional integration and light weight.

[0032] In some embodiments, the metal joint 1 is made of titanium alloy material; the raw material for preparing the structural layer 2 is one of T800 reinforced bismaleimide resin unidirectional prepreg, T800 reinforced polyimide resin unidirectional prepreg, T1000 reinforced polyimide resin unidirectional prepreg and T1000 reinforced bismaleimide resin unidirectional prepreg.

[0033] A second aspect of an embodiment of the present invention provides a method for preparing the above-mentioned speed brake for an aircraft, comprising the following steps:

[0034] S1: laying the prepreg of the structural layer on the lower mold, and pre-compacting it to a theoretical thickness, installing the female mold frame and the upper mold, closing the mold, and then pre-curing and molding to obtain a pre-cured structural layer 2;

[0035] S2: dismantle the upper mold, the female mold frame and the lower mold to install the metal joint 1, and install the metal joint 1 at a selected position on the pre-cured structural layer 2;

[0036] S3: Laying the prepreg of the heat protection layer 3 on the precured structural layer 2 to the theoretical thickness, and co-curing to obtain the speed brake for the aircraft.

[0037] In some embodiments, in step S1, the prepreg of the structural layer 2 is laid in a symmetrical direction of alternating ±45° and 0° / 90°; in step S3, the prepreg of the heat protection layer 3 is laid in a symmetrical direction of alternating ±45° and 0° / 90°.

[0038] In some embodiments, in step S1, after the first layer of prepreg of the structural layer 2 is laid, vacuum pre-compacting is performed, and then vacuum pre-compacting is performed every 4-6 layers.

[0039] In some embodiments, the prepreg surface density of the structural layer 2 is 100 to 300 g / m 2 , the volume content of the resin is 30-50%.

[0040] In some embodiments, the metal joint 1 and the structural layer 2 are fixed using a high temperature resistant adhesive.

[0041] In some embodiments, in step S1, the vacuuming time is 20 to 40 minutes, and the vacuum degree is ≤-0.08 MPa.

[0042] In some embodiments, in step S1, when the structural layer 2 adopts carbon fiber reinforced bismaleimide resin prepreg, the precuring system is: the room temperature is raised to 150±15℃, kept warm for 2 to 4 hours, and the pressure is 5 to 20MPa; from 150±15℃ to 200±15℃, kept warm for 2 to 4 hours, and the pressure is 5 to 20MPa; from 200±15℃ to 250±15℃, kept warm for 2 to 4 hours, and the pressure is 5 to 20MPa; when the structural layer 2 adopts carbon fiber reinforced polyimide resin prepreg, the precuring system is: the room temperature is raised to 150±15℃, kept warm for 2 to 4 hours , pressure is 5~20MPa; from 150±15℃ to 200±15℃, keep warm for 2~4h, pressure is 5~20MPa; from 200±15℃ to 250±15℃, keep warm for 2~4h, pressure is 5~20MPa; from 250±15℃ to 300±15℃, keep warm for 2~4h, pressure is 5~20MPa; from 300±15℃ to 350±15℃, keep warm for 2~4h, pressure is 5~20MPa; from 350±15℃ to 400±15℃, keep warm for 2~4h, pressure is 5~20MPa.

[0043] In some embodiments, in step S3, the curing system of the heat protection layer 3 is as follows: the room temperature is raised to 120±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 120±15°C to 140±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 140±15°C to 180±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 180±15°C to 220±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa.

[0044] Example 1

[0045] The aircraft speed brake of this embodiment includes:

[0046] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0047] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0048] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0049] The method for preparing the aircraft speed brake of this embodiment comprises the following steps:

[0050] S1. Coat the release agent on the steel upper mold and lower mold respectively, and lay a certain number of layers of T800 reinforced bismuth resin unidirectional prepreg on the lower mold to prepare the structural layer 2 of the speed brake. The structural layer 2 includes the skin part and the reinforcement part. The laying direction of the skin part is [0° / 0° / 45° / 90° / -45° / 0° / 0°] s Alternate cyclic laying; the laying of reinforcement parts includes transverse reinforcement laying and longitudinal reinforcement laying. The transverse reinforcement is laid with 4-6 layers of continuous prepreg, the longitudinal reinforcement is laid with 4-6 layers of prepreg that are disconnected at the intersection, the longitudinal reinforcement is laid with 4-6 layers of continuous prepreg, the transverse reinforcement is laid with 4-6 layers of prepreg that are disconnected at the intersection, and so on. Alternate cyclic laying; after the first layer is laid, vacuum pre-compact it, and then vacuum every 4-6 layers to ensure that the cloth layer is flat, spread and compacted. After laying to the theoretical thickness, install the female mold frame and the upper mold, close the mold, and use a press to pre-cure and shape the structural layer according to a certain curing system; the curing system is: heating from room temperature to 165℃, keeping warm for 2h, pressurizing at 5MPa; heating from 165℃ to 205℃, keeping warm for 2h; pressurizing at 10MPa. Among them, the surface density of T800 reinforced bismuth prepreg is 250g / m 2 , the volume content of the resin is 40%.

[0051] S2. After the pre-pressing of the fiber-reinforced resin-based composite material is completed, the structural layer 2-metal joint 1 part is assembled: the upper mold and the female mold frame in the mold are disassembled, the metal part installation position of the lower mold is disassembled, the metal part bonding tool and the metal joint 1 are installed, and the bonding tool is positioned with the lower mold mouth and the metal part pin. Use high-temperature resistant adhesive to fix the metal joint 1 and the composite material, and after curing, punch holes and screw them.

[0052] S3. Remove the metal parts bonding tooling and lay a certain number of layers of high-silicon-reinforced phenolic prepreg on the precured product to prepare the heat protection layer 3 of the speed brake. The laying direction is [0° / 45° / 90° / -45°] s Alternate cycle paving, after paving to the theoretical thickness, co-curing is carried out; the curing system is: heating from room temperature to 120℃, keeping warm for 2h, pressurizing 5MPa; heating from 120℃ to 140℃, keeping warm for 2h; pressurizing 10MPa; heating from 140℃ to 180℃, keeping warm for 2h; pressure 10MPa; heating from 180℃ to 235℃, keeping warm for 2h; pressure 10MPa. After curing, demoulding is carried out to obtain the final product.

[0053] Example 2

[0054] The aircraft speed brake of this embodiment includes:

[0055] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0056] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0057] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0058] The method for preparing the aircraft speed brake of this embodiment comprises the following steps:

[0059] S1. Coat the release agent on the steel upper mold and lower mold respectively, and lay a certain number of layers of T800 reinforced bismuth resin unidirectional prepreg on the lower mold to prepare the structural layer 2 of the speed brake. The structural layer 2 includes the skin part and the reinforcement part. The laying direction of the skin part is [0° / 0° / 45° / 90° / -45° / 0° / 0°] s Alternate cyclic laying; the laying of reinforcement parts includes transverse reinforcement laying and longitudinal reinforcement laying. The transverse reinforcement is laid with 4-6 layers of continuous prepreg, the longitudinal reinforcement is laid with 4-6 layers of prepreg that are disconnected at the intersection, the longitudinal reinforcement is laid with 4-6 layers of continuous prepreg, the transverse reinforcement is laid with 4-6 layers of prepreg that are disconnected at the intersection, and so on. Alternate cyclic laying; after the first layer is laid, vacuum is drawn for pre-compaction, and then vacuum is drawn every 4-6 layers to ensure that the cloth layer is flattened, spread and compacted. After laying to the theoretical thickness, the female mold frame and the upper mold are installed, and the mold is closed. The press is used to pre-cure and shape the structural layer 2 according to a certain curing system; the curing system is: heating from room temperature to 165℃, keeping warm for 2h, and pressurizing at 5MPa; heating from 165℃ to 205℃, keeping warm for 2h; pressurizing at 10MPa. Among them, the surface density of T800 reinforced bismuth prepreg is 150g / m 2 , the volume content of the resin is 40%.

[0060] S2. After the pre-pressing of the fiber-reinforced resin-based composite material is completed, the structural layer 2-metal joint 1 part is assembled: the upper mold and the female mold frame in the mold are disassembled, the metal part installation position of the lower mold is disassembled, the metal part bonding tool and the metal joint 1 are installed, and the bonding tool is positioned with the lower mold mouth and the metal part pin. Use high-temperature resistant adhesive to fix the metal joint 1 and the composite material, and after curing, punch holes and screw them.

[0061] S3. Remove the metal parts bonding tooling and lay a certain number of layers of high-silicon-reinforced phenolic prepreg on the precured product to prepare the heat protection layer 3 of the speed brake. The laying direction is [0° / 45° / 90° / -45°] s Alternate cycle paving, after paving to the theoretical thickness, co-curing is carried out; the curing system is: heating from room temperature to 120℃, keeping warm for 2h, pressurizing 5MPa; heating from 120℃ to 140℃, keeping warm for 2h; pressurizing 10MPa; heating from 140℃ to 180℃, keeping warm for 2h; pressure 10MPa; heating from 180℃ to 235℃, keeping warm for 2h; pressure 10MPa. After curing, demoulding is carried out to obtain the final product.

[0062] Example 3

[0063] The aircraft speed brake of this embodiment includes:

[0064] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0065] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0066] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0067] The method for preparing the aircraft speed brake of this embodiment comprises the following steps:

[0068] S1. Coat the release agent on the steel upper mold and lower mold respectively, and lay a certain number of layers of T1000 reinforced bismaleimide resin composite material on the lower mold to prepare the structural layer 2 of the speed brake. The structural layer 2 includes the skin part and the reinforcement part. The ply direction of the skin part is [0° / 0° / 45° / 90° / -45° / 0° / 0°] s Alternate cyclic laying; the laying of reinforcement parts includes transverse reinforcement laying and longitudinal reinforcement laying. The transverse reinforcement is laid with 4-6 layers of continuous prepreg cloth, the longitudinal reinforcement is laid with 4-6 layers of prepreg cloth that are disconnected at the intersection, the longitudinal reinforcement is laid with 4-6 layers of continuous prepreg cloth, the transverse reinforcement is laid with 4-6 layers of prepreg cloth that are disconnected at the intersection, and so on. Alternate cyclic laying; after the first layer is laid, vacuum pre-compact it, and then vacuum every 4-6 layers to ensure that the cloth layer is flat, spread and compacted. After laying to the theoretical thickness, install the female mold frame and the upper mold, close the mold, and use a press to pre-cure and shape the structural layer 2 according to a certain curing system; the curing system is: heating from room temperature to 165℃, keeping warm for 2h, pressurizing at 5MPa; heating from 165℃ to 205℃, keeping warm for 2h; pressurizing at 10MPa. Among them, the surface density of T1000 reinforced bismaleimide resin composite material is 250g / m 2 , the volume content of the resin is 40%.

[0069] S2. After the pre-pressing of the fiber-reinforced resin-based composite material is completed, the structural layer 2-metal joint 1 part is assembled: the upper mold and the female mold frame in the mold are disassembled, the metal part installation position of the lower mold is disassembled, the metal part bonding tool and the metal joint 1 are installed, and the bonding tool is positioned with the lower mold mouth and the metal part pin. Use high-temperature resistant adhesive to fix the metal joint 1 and the composite material, and after curing, punch holes and screw them.

[0070] S3. Remove the metal parts bonding tooling and lay a certain number of layers of high-silicon-reinforced phenolic prepreg on the precured product to prepare the heat protection layer 3 of the speed brake. The laying direction is [0° / 45° / 90° / -45°] s Alternate cycle paving, after paving to the theoretical thickness, co-curing is carried out; the curing system is: heating from room temperature to 120℃, keeping warm for 2h, pressurizing 5MPa; heating from 120℃ to 140℃, keeping warm for 2h; pressurizing 10MPa; heating from 140℃ to 180℃, keeping warm for 2h; pressure 10MPa; heating from 180℃ to 235℃, keeping warm for 2h; pressure 10MPa. After curing, demoulding is carried out to obtain the final product.

[0071] Example 4

[0072] The aircraft speed brake of this embodiment includes:

[0073] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0074] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0075] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0076] The method for preparing the aircraft speed brake of this embodiment comprises the following steps:

[0077] S1. Coat the release agent on the steel upper mold and lower mold respectively, and lay a certain number of layers of T800 reinforced polyimide resin composite material on the lower mold to prepare the structural layer 2 of the speed brake. The structural layer 2 includes a skin part and a reinforcement part. The ply direction of the skin part is [0° / 0° / 45° / 90° / -45° / 0° / 0°] s Alternate cyclic laying; the laying of reinforcement parts includes transverse reinforcement laying and longitudinal reinforcement laying. The transverse reinforcement is laid with 4-6 layers of continuous prepreg, and the longitudinal reinforcement is laid with 4-6 layers of prepreg that are disconnected at the intersection. The longitudinal reinforcement is laid with 4-6 layers of continuous prepreg, and the transverse reinforcement is laid with 4-6 layers of prepreg that are disconnected at the intersection, and so on. Alternate cyclic laying; after the first layer is laid, vacuum pre-compact it, and then vacuum every 4-6 layers to ensure that the cloth layer is flat, spread and compacted. After laying to the theoretical thickness, install the female mold frame and the upper mold, close the mold, and use a press to pre-cure and shape the structural layer 2 according to a certain curing system; the curing system is: heating from room temperature to 165℃, keeping warm for 2h, pressurizing at 5MPa; heating from 165℃ to 205℃, keeping warm for 2h; pressurizing at 5MPa. Among them, the surface density of T800 reinforced polyimide resin prepreg is 200g / m 2 , the volume content of the resin is 40%.

[0078] S2. After the pre-pressing of the fiber-reinforced resin-based composite material is completed, the structural layer 2-metal joint 1 part is assembled: the upper mold and the female mold frame in the mold are disassembled, the metal part installation position of the lower mold is disassembled, the metal part bonding tool and the metal joint 1 are installed, and the bonding tool is positioned with the lower mold mouth and the metal part pin. Use high-temperature resistant adhesive to fix the metal joint 1 and the composite material, and after curing, punch holes and screw them.

[0079] S3. Remove the metal parts bonding tooling and lay a certain number of layers of high-silicon-reinforced phenolic prepreg on the precured product to prepare the heat protection layer 3 of the speed brake. The laying direction is [0° / 45° / 90° / -45°] s Alternate cycle paving, after paving to the theoretical thickness, co-curing is carried out; the curing system is: heating from room temperature to 120℃, keeping warm for 2h, pressurizing 5MPa; heating from 120℃ to 140℃, keeping warm for 2h; pressurizing 10MPa; heating from 140℃ to 180℃, keeping warm for 2h; pressure 10MPa; heating from 180℃ to 235℃, keeping warm for 2h; pressure 10MPa. After curing, demoulding is carried out to obtain the final product.

[0080] Example 5

[0081] The aircraft speed brake of this embodiment includes:

[0082] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0083] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0084] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0085] The method for preparing the aircraft speed brake of this embodiment comprises the following steps:

[0086] S1. Coat the release agent on the steel upper mold and lower mold respectively, and lay a certain number of layers of T800 reinforced polyimide resin composite material on the lower mold to prepare the structural layer 2 of the speed brake. The structural layer 2 includes a skin part and a reinforcement part. The ply direction of the skin part is [0° / 0° / 45° / 90° / -45° / 0° / 0°] sAlternate cyclic laying; the laying of reinforcement parts includes transverse reinforcement laying and longitudinal reinforcement laying. The transverse reinforcement is laid with 4-6 layers of continuous prepreg cloth, the longitudinal reinforcement is laid with 4-6 layers of prepreg cloth that are disconnected at the intersection, the longitudinal reinforcement is laid with 4-6 layers of continuous prepreg cloth, the transverse reinforcement is laid with 4-6 layers of prepreg cloth that are disconnected at the intersection, and so on. Alternate cyclic laying; after the first layer is laid, vacuum is drawn for pre-compaction, and then vacuum is drawn every 4-6 layers to ensure that the cloth layer is flattened, spread and compacted. After laying to the theoretical thickness, the female mold frame and the upper mold are installed, and the mold is closed. The press is used to pre-cure and mold the structural layer 2 according to a certain curing system; the curing system is: heating from room temperature to 165℃, keeping warm for 2h, and pressurizing at 5MPa; heating from 165℃ to 205℃, keeping warm for 2h; pressurizing at 5MPa. Among them, the surface density of T800 reinforced polyimide resin prepreg is 250g / m 2 , the volume content of the resin is 35%.

[0087] S2. After the pre-pressing of the fiber-reinforced resin-based composite material is completed, the structural layer 2-metal joint 1 part is assembled: the upper mold and the female mold frame in the mold are disassembled, the metal part installation position of the lower mold is disassembled, the metal part bonding tool and the metal joint 1 are installed, and the bonding tool is positioned with the lower mold mouth and the metal part pin. Use high-temperature resistant adhesive to fix the metal joint 1 and the composite material, and after curing, punch holes and screw them.

[0088] S3. Remove the metal parts bonding tooling and lay a certain number of layers of high-silicon-reinforced phenolic prepreg on the precured product to prepare the heat protection layer 3 of the speed brake. The laying direction is [0° / 45° / 90° / -45°] s Alternate cycle paving, after paving to the theoretical thickness, co-curing is carried out; the curing system is: heating from room temperature to 120℃, keeping warm for 2h, pressurizing 5MPa; heating from 120℃ to 140℃, keeping warm for 2h; pressurizing 10MPa; heating from 140℃ to 180℃, keeping warm for 2h; pressure 10MPa; heating from 180℃ to 235℃, keeping warm for 2h; pressure 10MPa. After curing, demoulding is carried out to obtain the final product.

[0089] Example 6

[0090] The aircraft speed brake of this embodiment includes:

[0091] A metal joint 1, a structural layer 2 and a heat-proof layer 3; the metal joint 1 is arranged at one end of the structural layer 2, and the heat-proof layer 3 is arranged on the structural layer 2;

[0092] The structural layer 2 is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material;

[0093] The heat protection layer 3 is a high-silica cloth reinforced phenolic resin-based composite material.

[0094] The method for preparing the aircraft speed brake of this embodiment comprises the following steps:

[0095] S1. Coat the release agent on the steel upper mold and lower mold respectively, and lay a certain number of layers of T1000 reinforced polyimide resin composite material on the lower mold to prepare the structural layer 2 of the speed reducer. The structural layer 2 includes a skin part and a reinforcement part. The laying direction of the skin part is [0° / 0° / 45° / 90° / -45° / 0° / 0°] s Alternate cyclic laying; the reinforcement part of the laying includes transverse reinforcement laying and longitudinal reinforcement laying. The transverse reinforcement is laid with 4-6 layers of continuous prepreg cloth, the longitudinal reinforcement is laid with 4-6 layers of prepreg cloth that are disconnected at the intersection, the longitudinal reinforcement is laid with 4-6 layers of continuous prepreg cloth, the transverse reinforcement is laid with 4-6 layers of prepreg cloth that are disconnected at the intersection, and so on. Alternate cyclic laying; after the first layer is laid, vacuum pre-compact it, and then vacuum every 4-6 layers to ensure that the cloth layer is flat, spread and compacted. After laying to the theoretical thickness, install the female mold frame and the upper mold, close the mold, and use a press to pre-cure and shape the structural layer 2 according to a certain curing system; the curing system is: heating from room temperature to 165℃, keeping warm for 2h, pressurizing at 5MPa; heating from 165℃ to 205℃, keeping warm for 2h; pressurizing at 5MPa. Among them, the surface density of T1000 reinforced polyimide resin composite material is 250g / m 2 , the volume content of the resin is 40%.

[0096] S2. After the pre-pressing of the fiber-reinforced resin-based composite material is completed, the structural layer 2-metal joint 1 part is assembled: the upper mold and the female mold frame in the mold are disassembled, the metal part installation position of the lower mold is disassembled, the metal part bonding tool and the metal joint 1 are installed, and the bonding tool is positioned with the lower mold mouth and the metal part pin. Use high-temperature resistant adhesive to fix the metal joint 1 and the composite material, and after curing, punch holes and screw them.

[0097] S3. Remove the metal parts bonding tooling and lay a certain number of layers of high-silicon-reinforced phenolic prepreg on the precured product to prepare the heat protection layer 3 of the speed brake. The laying direction is [0° / 45° / 90° / -45°] s Alternate cycle paving, after paving to the theoretical thickness, co-curing is carried out; the curing system is: heating from room temperature to 120℃, keeping warm for 2h, pressurizing 5MPa; heating from 120℃ to 140℃, keeping warm for 2h; pressurizing 10MPa; heating from 140℃ to 180℃, keeping warm for 2h; pressure 10MPa; heating from 180℃ to 235℃, keeping warm for 2h; pressure 10MPa. After curing, demoulding is carried out to obtain the final product.

[0098] Comparative Example 1

[0099] The speed reducer body of this comparative example is made of traditional titanium alloy material, and the preparation method is to use the superplastic forming method of titanium alloy, and utilize the ultra-high elongation and superplasticity of titanium alloy material under specific temperature and strain rate conditions, and use the superplastic metal sheet as the formed blank to realize forming processing in the mold cavity, so as to obtain the forming process of various required shape parts. The theoretical unfolded size of the speed reducer is calculated according to the outer dimensions, the part contour is processed according to the size requirements, the solder stop is applied in the superplastic forming area, the mold is coated with a release agent, the part is installed in the mold, the mold is placed in the superplastic equipment, diffusion bonding and superplastic forming are carried out, the part and the mold are cooled, and the furnace is processed to obtain the final product.

[0100] The aircraft speed reducer of the present invention adopts a compression molding process, and the mold is used to ensure that the product maintains its original shape and size, thereby achieving net size molding of the product. Traditional metal molding methods include casting, plastic processing, cutting, welding and powder metallurgy, some of which can achieve net size molding, while others require secondary processing and are different from composite material molding processes.

[0101] The performance of the speed reducer assembly of the above-mentioned embodiments and comparative examples was tested, and the results are shown in Table 1. It can be seen from the results in Table 1 that, compared with the traditional titanium alloy used in the comparative example, the tensile strength of the present invention is significantly improved, the density is significantly reduced, and the weight of the bottom shield assembly is reduced.

[0102] Table 1 Speed ​​brake assembly performance test

[0103] Group Tensile strength(MPa) <![CDATA[Density (g / cm 3 )]]> Example 1 2784 1.65 Example 2 2406 1.65 Example 3 2960 1.65 Example 4 2726 1.67 Example 5 2318 1.67 Example 6 2926 1.67 Comparative Example 1 895 4.50

[0104] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A speed brake for an aircraft, It is characterized in that include: A metal joint, a structural layer and a heat-proof layer; the metal joint is arranged at one end of the structural layer, and the heat-proof layer is arranged on the structural layer; The structural layer is a carbon fiber reinforced bismaleimide resin-based composite material or a carbon fiber reinforced polyimide resin-based composite material; The heat protection layer is a high-silica cloth reinforced phenolic resin-based composite material.

2. The aircraft speed brake according to claim 1, Features: The metal joint is made of titanium alloy; The raw material for preparing the structural layer is one of T800 reinforced bismaleimide resin unidirectional prepreg, T800 reinforced polyimide resin unidirectional prepreg, T1000 reinforced polyimide resin unidirectional prepreg and T1000 reinforced bismaleimide resin unidirectional prepreg.

3. A method for preparing the aircraft speed brake according to claim 1 or 2, It is characterized in that The following steps are involved: S1: laying the prepreg of the structural layer on the lower mold, pre-compacting it to a theoretical thickness, installing the female mold frame and the upper mold, closing the mold, and then pre-curing and molding to obtain a pre-cured structural layer; S2: dismantle the upper mold, the female mold frame and the lower mold to install the metal joint, and install the metal joint at a selected position on the pre-cured structural layer; S3: Laying the prepreg of the heat protection layer on the precured structural layer to a theoretical thickness, and co-curing to obtain the speed brake for the aircraft.

4. The method for preparing the speed brake for an aircraft according to claim 3, It is characterized in that The specific steps include: In step S1, the prepreg material of the structural layer is laid in a symmetrical and alternating direction of ±45° and 0° / 90°; in step S3, the prepreg material of the heat protection layer is laid in a symmetrical and alternating direction of ±45° and 0° / 90°.

5. The method for preparing the speed brake for an aircraft according to claim 3, Features: In step S1, after the first layer of the prepreg material of the structural layer is laid, vacuum pre-compacting is performed, and then vacuum pre-compacting is performed every 4-6 layers.

6. The method for preparing the speed brake for an aircraft according to claim 3, Features: The prepreg surface density of the structural layer is 100-300 g / m 2 , the volume content of the resin is 30 to 50%.

7. The method for preparing the speed brake for an aircraft according to claim 3, Features: The metal joint and the structural layer are fixed with high temperature resistant adhesive.

8. The method for preparing the speed brake for an aircraft according to claim 3, Features: In step S1, the vacuuming time is 20 to 40 minutes, and the vacuum degree is ≤-0.08 MPa.

9. The method for preparing the speed brake for an aircraft according to claim 3, Features: In step S1, when the structural layer adopts carbon fiber reinforced bismaleimide resin prepreg, the precuring system is: room temperature rises to 150±15℃, keeps warm for 2~4h, and the pressure is 5~20MPa; from 150±15℃ to 200±15℃, keeps warm for 2~4h, and the pressure is 5~20MPa; from 200±15℃ to 250±15℃, keeps warm for 2~4h, and the pressure is 5~20MPa; when the structural layer adopts carbon fiber reinforced polyimide resin prepreg, the precuring system is: room temperature rises to 150±15℃, keeps warm for 2~4h, and the pressure is The temperature is increased from 150±15℃ to 200±15℃, keep warm for 2~4h, and the pressure is 5~20MPa; from 200±15℃ to 250±15℃, keep warm for 2~4h, and the pressure is 5~20MPa; from 250±15℃ to 300±15℃, keep warm for 2~4h, and the pressure is 5~20MPa; from 300±15℃ to 350±15℃, keep warm for 2~4h, and the pressure is 5~20MPa; from 350±15℃ to 400±15℃, keep warm for 2~4h, and the pressure is 5~20MPa.

10. The method for preparing the speed brake for aircraft according to claim 3, Features: In step S3, the curing system of the heat-proof layer is: the room temperature is raised to 120±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; the temperature is raised from 120±15°C to 140±15°C, kept warm for 2 to 4 hours, and the pressure is 5 to 20 MPa; Raise the temperature from 140±15℃ to 180±15℃, keep warm for 2~4h, and the pressure is 5~20MPa; raise the temperature from 180±15℃ to 220±15℃, keep warm for 2~4h, and the pressure is 5~20MPa.

Citation Information

Patent Citations

  • Preparation method of spaceflight projectile body heat shielding structure

    CN107328316A

  • Carrying aircraft and load delivery method

    CN111017193A

  • Reusable high-temperature speed reducing plate mechanism

    CN112173074A

  • Bottom curtain board assembly for aircraft and preparation method of bottom curtain board assembly

    CN116495162A

  • High-pressure composite material spray pipe and integrated forming method thereof

    CN117662330A