Aluminum vacancy defect aluminum nitride as well as preparation method and application thereof

By preparing aluminum vacancy defective aluminum nitride in an inert gas environment, the fault problem caused by the decomposition of trifluoroacetonitrile in a gas insulated transformer is solved, efficient adsorption of trifluoroacetonitrile is achieved, and the safety and reliability of the equipment are improved.

CN118908156APending Publication Date: 2024-11-08LISHUI ZHENGYANG ELECTRIC POWER DESIGN INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410973878.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In gas insulated transformers, the decomposition and presence of trifluoroacetonitrile lead to failures, and the prior art is difficult to effectively adsorption, affecting the safety and reliability of the equipment.

Method used

By controlling the reaction temperature and the reaction of the Al2O3 sol solution with aluminum nitride in an inert gas environment, a material with aluminum vacancy defective is prepared, and a material with selective adsorption effect on trifluoroacetonitrile is used.

Benefits of technology

It realizes efficient adsorption of trifluoroacetonitrile, improves the safety and reliability of gas insulated transformers, avoids unnecessary failures, and does not adsorb other gases such as carbon tetrafluoride and perfluoroisobutyronitrile, maintains the equipment Excellent insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908156A_ABST
    Figure CN118908156A_ABST
Patent Text Reader

Abstract

The invention discloses aluminum vacancy defect aluminum nitride and a preparation method and application thereof.The preparation method of the aluminum vacancy defect aluminum nitride comprises the steps that in the inert gas environment and under the reaction temperature condition of 200-220 DEG C, aluminum nitride is washed with an Al2O3 sol solution for a reaction, then sintering is conducted, and the aluminum vacancy defect aluminum nitride is obtained; the solvent of the Al2O3 sol solution contains water. According to the preparation method disclosed by the invention, through protection of an inert gas environment and control of the reaction temperature, the Al2O3 sol solution and the aluminum nitride react to generate the aluminum vacancy defect aluminum nitride with an adsorption effect on trifluoroacetonitrile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inorganic materials, and more specifically, to aluminum vacancy defect aluminum nitride and a preparation method and application thereof. Background Art

[0002] With the development of urban construction, urban population is becoming more and more dense, and electricity consumption is also increasing sharply. High-voltage substations have been directly built in city centers and high-rise buildings. In order to ensure the safety of urban construction and residents, higher requirements are put forward for the safety, reliability, non-flammability and low noise of high-voltage substations, and special attention is paid to the fire prevention of high-voltage substations. In high-voltage substations, the traditional large-capacity oil-immersed transformers used have a large amount of oil. Once a fire occurs, it will bring unpredictable losses. Therefore, it is urgent to develop non-flammable transformers with good fire resistance.

[0003] Gas-Insulated Transformer (GIT) is a transformer that uses gas as the insulating medium. It is a non-flammable transformer that is widely favored due to its superior fireproof, explosion-proof and moisture-proof properties, as well as excellent electrical insulation properties and pollution-free. Gas-insulated transformers initially used SF6 gas as the insulating medium, but because it is a strong greenhouse gas and is not environmentally friendly, it was restricted, so the environmentally friendly gas perfluoroisobutyronitrile (C4F7N) was developed as the insulating medium of gas-insulated transformers.

[0004] Since latent faults such as insulation defects are inevitable inside gas-insulated transformers, local discharge is triggered, causing the gas insulating medium perfluoroisobutyronitrile (C4F7N) to decompose under the action of electric arc to produce a large number of low-insulation strength products, such as trifluoroacetonitrile (CF3CN), carbon tetrafluoride (CF4) and hexafluoroethane (C2F6), etc.; among them, trifluoroacetonitrile (CF3CN) is not only a highly toxic gas, but its presence can easily cause failure of gas-insulated transformers, so trifluoroacetonitrile (CF3CN) needs to be adsorbed in time.

[0005] Therefore, it is of great significance to develop a method for preparing aluminum vacancy defect aluminum nitride that has an adsorption effect on trifluoroacetonitrile. Summary of the invention

[0006] The purpose of the present invention is to provide an aluminum vacancy defect aluminum nitride having an adsorption effect on trifluoroacetonitrile, and a preparation method and application thereof.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] In a first aspect, the present invention provides a method for preparing aluminum nitride with aluminum vacancy defects, comprising:

[0009] In an inert gas environment, at a reaction temperature of 200-220°C, aluminum nitride (AlN) is washed with an Al2O3 sol solution for reaction, and then sintered to obtain aluminum vacancy defect aluminum nitride;

[0010] The solvent of the Al2O3 sol solution contains water.

[0011] The preparation method of the invention uses the protection of an inert gas environment and controls the reaction temperature to react Al2O3 sol solution with aluminum nitride to generate aluminum vacancy defect aluminum nitride having an adsorption effect on trifluoroacetonitrile.

[0012] Specifically, the present invention protects the inert gas environment and controls the reaction temperature, so that oxygen (O) in water in the Al2O3 sol solution enters the lattice of aluminum nitride (AlN) and combines with Al to form aluminum oxide (Al2O3) and dissolves into the Al2O3 sol solution, so that aluminum vacancies appear in the aluminum nitride (AlN), and aluminum vacancy defective aluminum nitride is obtained; at the same time, since the Al2O3 sol solution contains a large amount of Al2O3, it can inhibit a large amount of Al in the aluminum nitride (AlN) from combining with O and dissolving into the Al2O3 sol solution, thereby preventing a large amount of Al from being lost in the aluminum nitride (AlN).

[0013] In the present invention, the aluminum vacancy defective aluminum nitride containing aluminum vacancies can adsorb trifluoroacetonitrile (CF3CN) with a small molecular diameter by combining with a cyano group (-CN), and the aluminum vacancy defective aluminum nitride will not adsorb carbon tetrafluoride (CF4) and hexafluoroethane (C2F6) containing only CF bonds, nor will it adsorb perfluoroisobutyronitrile (C4F7N) containing a cyano group (-CN) and a large molecular diameter.

[0014] In the present invention, when the reaction temperature is lower than 200°C, it is not conducive to the formation of aluminum vacancies, which will affect the synthesis of aluminum vacancy defective aluminum nitride; when the reaction temperature is higher than 220°C, it is easy to cause the formation of larger pores in the aluminum nitride, which is not conducive to the adsorption of trifluoroacetonitrile (CF3CN) by aluminum vacancy defective aluminum nitride; and when the temperature is higher than 220°C or lower than 200°C, aluminum vacancy defective aluminum nitride adsorbs perfluoroisobutyronitrile (C4F7N), reducing its selective adsorption capacity for trifluoroacetonitrile (CF3CN).

[0015] Preferably, the inert gas is at least one of nitrogen, argon and helium.

[0016] Preferably, the solid content of the Al2O3 sol solution is 20%-25%.

[0017] Preferably, the ratio of the flushing speed of the Al2O3 sol solution to the mass of aluminum nitride is (80-100) mL / min:1 g.

[0018] Preferably, the pH of the Al2O3 sol solution is 2-5.

[0019] In the present invention, the Al2O3 sol solution with a pH of 2-5 can provide acidic conditions for the reaction, further promoting the synthesis of aluminum nitride with aluminum vacancy defects.

[0020] In the present invention, the Al2O3 sol solution can be purchased from the market or prepared by conventional methods in the art, such as: preparing the Al2O3 sol solution by hydrolyzing alcohol aluminum using a hydrothermal method, and the alcohol aluminum can be aluminum isopropoxide, aluminum sec-butoxide, aluminum isobutoxide, and the like.

[0021] Preferably, the flushing is performed 4-6 times, the duration of each flushing is 20-25 seconds, and the time interval between each flushing is 3-5 minutes.

[0022] The present invention controls the reaction rate and reaction degree between the Al2O3 sol solution and the aluminum nitride by controlling the number of flushing, the time of each flushing, and the time interval between each flushing, thereby obtaining aluminum vacancy defect aluminum nitride with a large number of aluminum vacancies, and further improving the adsorption effect or adsorption rate of aluminum vacancy defect aluminum nitride on trifluoroacetonitrile. In particular, when the time of each flushing is too long, aluminum nitride is easily further decomposed by the acidic Al2O3 sol solution after aluminum vacancies are formed, thereby affecting the number of aluminum vacancies in the aluminum vacancy defect aluminum nitride, which is not conducive to improving the adsorption effect or adsorption rate of aluminum vacancy defect aluminum nitride on trifluoroacetonitrile (CF3CN); when the time of each flushing is too short, fewer aluminum vacancies are formed, which is also not conducive to the adsorption effect or adsorption rate of high aluminum vacancy defect aluminum nitride on trifluoroacetonitrile (CF3CN).

[0023] Preferably, the average particle size of the aluminum nitride is 20-50 nm.

[0024] Preferably, the sintering temperature is 400-450° C. and the sintering time is 1-3 hours.

[0025] In the present invention, the Al2O3 sol solution and aluminum nitride (AlN) are reacted and then sintered, which is beneficial to remove oxygen-containing impurities in aluminum nitride (AlN), prevent aluminum nitride with aluminum vacancy defects from reacting with perfluoroisobutyronitrile (C4F7N), causing perfluoroisobutyronitrile loss inside the gas-insulated transformer, and affecting the adsorption effect or adsorption rate of aluminum nitride with aluminum vacancy defects on trifluoroacetonitrile (CF3CN). When the sintering temperature is too high, the amount of the second phase at the AlN crystal interface is too high, affecting the adsorption effect or adsorption rate of aluminum nitride with aluminum vacancy defects on trifluoroacetonitrile (CF3CN).

[0026] Preferably, after the sintering, washing and drying are also included.

[0027] More preferably, the washing solvent is an organic solvent; the organic solvent is at least one of acetone, ethanol and isobutanol.

[0028] More preferably, the drying is performed in an inert gas environment.

[0029] In a second aspect, the present invention provides an aluminum vacancy defect aluminum nitride prepared by the above preparation method.

[0030] In a third aspect, the present invention provides an application of aluminum nitride with aluminum vacancy defects in adsorption materials.

[0031] In a fourth aspect, the present invention provides a method for preparing an aluminum vacancy defect aluminum nitride adsorption film, comprising:

[0032] S1. mixing aluminum vacancy defect aluminum nitride and a polymer solution to obtain a precursor solution;

[0033] S2. The precursor solution is made into a membrane by electrospinning to obtain an aluminum vacancy defect aluminum nitride adsorption membrane (AlNNS adsorption membrane).

[0034] Preferably, in step S1, the polymer is at least one of polyamic acid (PAA), polyvinyl alcohol (PVA), polypropylene (PP), polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), polylactic acid (PLA), polyacrylonitrile, chitosan and its derivatives, and cellulose and its derivatives.

[0035] Preferably, in step S1, the mass fraction of aluminum nitride with aluminum vacancy defects in the precursor solution is 0.8%-1.2%.

[0036] In the present invention, when the mass fraction of aluminum vacancy defect aluminum nitride in the precursor solution is too high, it is not conducive to the adhesion of aluminum vacancy defect aluminum nitride to the aluminum vacancy defect aluminum nitride adsorption film, and the aluminum vacancy defect aluminum nitride is easily caused to fall off from the aluminum vacancy defect aluminum nitride adsorption film, thereby causing the aluminum vacancy defect aluminum nitride adsorption film to form insulation defects in the gas-insulated transformer, affecting the proof work of the gas-insulated transformer.

[0037] Preferably, in step S1, the solid content of the polymer solution is 15%-25%.

[0038] Preferably, in step S1, the mixing temperature is 50-60°C.

[0039] Preferably, in step S1, the mixing method is stirring, and the stirring time is 10-12 hours.

[0040] Preferably, in step S2, the electrospinning conditions are: the pressure of the syringe needle is set to 23-27 kV, the receiving wheel speed is set to 180-200 r / min, the spinning distance is set to 14-18 cm, the syringe injection speed is set to 0.6-1.0 mL / h, and the parallel movement speed relative to the receiving wheel is set to 8-10 cm / min.

[0041] Preferably, in step S2, the film made of the polymer mixed solution is vacuum dried.

[0042] More preferably, the vacuum drying is carried out at a temperature of 140-160° C. and for a time of 10-12 h.

[0043] In a fifth aspect, the present invention provides an aluminum vacancy defect aluminum nitride adsorption film prepared by the above-mentioned preparation method.

[0044] In a sixth aspect, the present invention provides an application of an aluminum vacancy defect aluminum nitride adsorption film in the adsorption of trifluoroacetonitrile (CF3CN).

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] The preparation method of the invention uses the protection of an inert gas environment and controls the reaction temperature to react Al2O3 sol solution with aluminum nitride to generate aluminum vacancy defect aluminum nitride having an adsorption effect on trifluoroacetonitrile.

[0047] The present invention controls the reaction rate and reaction degree between the Al2O3 sol solution and aluminum nitride by controlling the number of flushings, the time of each flushing and the time interval between each flushing, thereby obtaining aluminum vacancy defect aluminum nitride with a large number of aluminum vacancies, and further improving the adsorption effect or adsorption rate of aluminum vacancy defect aluminum nitride on trifluoroacetonitrile.

[0048] In the present invention, sintering after the Al2O3 sol solution reacts with aluminum nitride (AlN) is beneficial to remove oxygen-containing impurities in aluminum nitride (AlN), prevent aluminum nitride with aluminum vacancy defects from reacting with perfluoroisobutyronitrile (C4F7N), causing perfluoroisobutyronitrile loss inside the gas-insulated transformer, and affecting the adsorption effect or adsorption rate of aluminum nitride with aluminum vacancy defects on trifluoroacetonitrile (CF3CN). When the sintering temperature is too high, the amount of the second phase at the AlN crystal interface is too high, affecting the adsorption effect or adsorption rate of aluminum nitride with aluminum vacancy defects on trifluoroacetonitrile (CF3CN). BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a graph showing the adsorption rate of CF3CN over time on the aluminum vacancy defect-treated aluminum nitride adsorption film in Application Example 1.

[0050] Figure 2This is a graph showing the adsorption rate of C4F7N on the aluminum vacancy defect aluminum nitride adsorption film of Application Example 1 over time.

[0051] Figure 3 This is a graph showing the adsorption rate of CF3CN over time for aluminum vacancy defect-treated aluminum nitride adsorption film after recovery in Application Example 1. DETAILED DESCRIPTION

[0052] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0053] In each embodiment and comparative example of the present invention, the use of reagents is as follows:

[0054] The solid content of Al2O3 sol solution is 20%, pH=2-5, the manufacturer of Al2O3 sol solution is Hangzhou Hengna New Materials Co., Ltd., and the product model is HN-JR14W;

[0055] The manufacturer of polyamic acid (PAA) is Hubei Langbowan, and the product brand is LBW-0114.

[0056] The manufacturer of aluminum nitride (AlN) is Shanghai Xiaohuang Nanotechnology, and the product model is XH-AlN-30.

[0057] Example 1

[0058] This embodiment provides an aluminum vacancy defect aluminum nitride, and a preparation method thereof includes:

[0059] In a dry argon environment, at a reaction temperature of 210°C, 4g of aluminum nitride (AlN) with an average particle size of 30nm was rinsed with Al2O3 sol solution for 5 times for reaction, each rinsing time was 25s, and the time interval between each rinsing was 4min, and then sintered at 425°C for 2h, washed with acetone for many times, and dried at 100°C in a dry argon environment to obtain aluminum vacancy defect aluminum nitride;

[0060] The solvent of the Al2O3 sol solution contains water; the ratio of the flushing speed of the Al2O3 sol solution to the mass of aluminum nitride is 90mL / min:1g.

[0061] Example 2-11 and Comparative Example 1-2

[0062] Examples 2-11 and Comparative Examples 1-2 provide different aluminum vacancy defect aluminum nitrides and preparation methods thereof, which differ from Example 1 in that the reaction temperature, the time of each flushing, and the sintering temperature are different, and the rest are consistent with Example 1, as shown in the following table:

[0063] Table 1 Experimental conditions of Examples 1-11 and Comparative Examples 1-2

[0064] Reaction temperature / ℃ Time of each flushing / s Sintering temperature / ℃ Example 1 210 25 425 Example 2 200 25 425 Example 3 220 25 425 Comparative Example 1 140 25 425 Comparative Example 2 350 25 425 Example 4 210 20 425 Example 5 210 30 425 Example 6 210 5 425 Example 7 210 60 425 Example 8 210 25 400 Example 9 210 25 450 Example 10 210 25 300 Embodiment 11 210 25 550

[0065] Application Examples

[0066] Application Example 1

[0067] This application example provides an aluminum vacancy defect aluminum nitride adsorption film, and a preparation method thereof includes:

[0068] S1. Stirring the aluminum vacancy defect aluminum nitride and polyamic acid (PAA) solution prepared in Example 1 with a magnetic stirrer at 55° C. for 12 h to uniformly disperse the aluminum vacancy defect aluminum nitride prepared in Example 1 in the solution to obtain a precursor solution;

[0069] S2. The precursor solution was loaded into a 10 mL syringe, which was installed on an electrospinning instrument. The electrospinning conditions were controlled as follows: the pressure of the syringe needle was set to 25 kV, the receiving wheel speed was set to 190 r / min, the spinning distance was set to 16 cm, the syringe injection speed was set to 0.8 mL / h, and the parallel movement speed relative to the receiving wheel was set to 9 cm / min. The membrane was electrospun to form a film, and the membrane was placed in a vacuum drying oven. After vacuuming, it was dried at 150 ° C for 12 h to obtain an aluminum vacancy defect aluminum nitride adsorption film (AlNNS adsorption film);

[0070] The polyamic acid (PAA) solution is prepared by dissolving polyamic acid in deionized water solvent, and its solid content is 20%. The mass fraction of the aluminum nitride with aluminum vacancy defects prepared in Example 1 in the precursor solution is 1.0%.

[0071] Application Example 2-11 and Comparative Application Example 1-2

[0072] Application Examples 2-11 and Comparative Application Examples 1-2 provide different aluminum vacancy defect aluminum nitride adsorption films and preparation methods thereof. The difference between them and Application Example 1 is that Application Examples 2-11 respectively use the aluminum vacancy defect aluminum nitride prepared by Examples 2-11, and Comparative Application Examples 1-2 respectively use the aluminum vacancy defect aluminum nitride prepared by Comparative Examples 1-2. The rest are consistent with Application Example 1.

[0073] Comparative Application Example 3

[0074] This comparative application example provides an aluminum nitride adsorption film, which differs from Application Example 1 in that aluminum nitride (AlN) with an average particle size of 30 nm is used instead of the aluminum vacancy defect aluminum nitride prepared in Example 1, and the rest is consistent with Application Example 1.

[0075] Performance Testing

[0076] The following performance tests were performed on the aluminum vacancy defect aluminum nitride adsorption films of each application example and comparative application example:

[0077] (1) Gas adsorption test

[0078] The aluminum vacancy defect aluminum nitride adsorption film (AlNNS adsorption film) of each application example or comparative application example was cut into a circular film with a diameter of 8 cm, and the circular film was placed in a sealed can with a volume of 5 L at room temperature, and 100 ppm (volume fraction) of the test gas was filled in the sealed can, and then carbon dioxide was filled to make the relative air pressure of the sealed can be 0.14 MPa, and static adsorption was performed for 20 days. The concentration of the test gas in the sealed can was tested every day by a gas chromatography-mass spectrometer, and the adsorption rate of the circular film to the test gas was calculated by the following formula:

[0079] Adsorption rate on the nth day (%) = (100ppm-concentration of the gas to be tested after adsorption for n days) / 100ppm×100%;

[0080] Wherein, the gas to be tested is one of perfluoroisobutyronitrile (C4F7N), trifluoroacetonitrile (CF3CN), carbon tetrafluoride (CF4), and hexafluoroethane (C2F6); since the test period is 20 days, the value range of n is 0-20;

[0081] The experimental results are shown in the following table:

[0082] Table 2 Gas adsorption test results of circular membranes of various application examples and comparative application examples

[0083]

[0084] Figure 1 This is a graph showing the adsorption rate of CF3CN over time on the aluminum vacancy defect-treated aluminum nitride adsorption film in Application Example 1. Figure 2 This is a graph showing the adsorption rate of C4F7N on the aluminum vacancy defect aluminum nitride adsorption film of Application Example 1 over time.

[0085] from Figure 1-2 As shown in Table 2, the aluminum vacancy defect aluminum nitride of the present invention has a good adsorption effect on trifluoroacetonitrile, and the aluminum vacancy defect aluminum nitride will not adsorb carbon tetrafluoride (CF4) and hexafluoroethane (C2F6) containing only CF bonds, nor will it adsorb perfluoroisobutyronitrile (C4F7N) containing cyano (-CN) but with a large molecular diameter.

[0086] In addition, from Figure 1 It can be seen that the adsorption of trifluoroacetonitrile by the aluminum vacancy defect aluminum nitride adsorption film of Application Example 1 of the present invention reaches a saturated state on the 14th day, and the adsorption rate reaches 92.35%.

[0087] (2) Repeatability test

[0088] The aluminum vacancy defect aluminum nitride adsorption film of Application Example 1 after the (1) gas adsorption test is taken out, washed with acetone for multiple times in a dry argon environment, and dried in a dry argon environment at 300°C for 10 hours, and then taken out to complete the recovery of the aluminum vacancy defect aluminum nitride adsorption film of the corresponding Example 1; then, the trifluoroacetonitrile (CF3CN) adsorption test is continued according to the experimental steps of the (1) gas adsorption test.

[0089] Figure 3 This is a graph showing the adsorption rate of CF3CN over time for aluminum vacancy defect-treated aluminum nitride adsorption film after recovery in Application Example 1.

[0090] from Figure 3 It can be seen that the adsorption of trifluoroacetonitrile by the aluminum vacancy defect aluminum nitride adsorption membrane of Application Example 1 used for the second time after recovery reached a saturated state on the 17th day, and the adsorption rate reached 86.23%, which was only slightly lower than the 92.35% when it was used for the first time. This shows that the aluminum vacancy defect aluminum nitride adsorption membrane of the present invention can be reused and has good reusability.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing aluminum nitride with aluminum vacancy defects, characterized in that: include: In an inert gas environment, at a reaction temperature of 200-220°C, aluminum nitride is washed with an Al2O3 sol solution to react, and then sintered to obtain aluminum vacancy defect aluminum nitride; The solvent of the Al2O3 sol solution contains water.

2. The method for preparing aluminum nitride with aluminum vacancy defects according to claim 1, characterized in that: The sintering temperature is 400-450°C.

3. The method for preparing aluminum nitride with aluminum vacancy defects according to claim 1, characterized in that: The number of flushing is 4-6 times, the duration of each flushing is 20-25 seconds, and the time interval between each flushing is 3-5 minutes.

4. The method for preparing aluminum nitride with aluminum vacancy defects according to claim 1, characterized in that: The solid content of the Al2O3 sol solution is 20%-25%; the ratio of the flushing speed of the Al2O3 sol solution to the mass of aluminum nitride is (80-100) mL / min:1g.

5. An aluminum vacancy defect aluminum nitride, characterized in that: Prepared by the preparation method described in any one of claims 1 to 4.

6. Use of the aluminum vacancy defect-treated aluminum nitride according to claim 5 in adsorption materials.

7. A method for preparing an aluminum vacancy defect aluminum nitride adsorption film, characterized in that: include: S1. mixing the aluminum vacancy defect aluminum nitride according to claim 5 and a polymer solution to obtain a precursor solution; S2. The precursor solution is made into a membrane by electrospinning to obtain an aluminum vacancy defect aluminum nitride adsorption membrane.

8. The method for preparing the aluminum vacancy defect aluminum nitride adsorption film according to claim 7, characterized in that: At least one of the following: (1) In step S1, the polymer is at least one of polyamic acid, polyvinyl alcohol, polypropylene, polyvinyl pyrrolidone, polyethylene glycol, polylactic acid, polyacrylonitrile, chitosan and its derivatives, cellulose and its derivatives; (2) In step S1, the mass fraction of aluminum nitride with aluminum vacancy defects in the precursor solution is 0.8%-1.2%; (3) In step S1, the solid content of the polymer solution is 15%-25%; (4) In step S1, the mixing temperature is 50-60°C; (5) In step S2, the electrospinning conditions are as follows: the pressure of the syringe needle is set to 23-27 kV, the receiving wheel speed is set to 180-200 r / min, the spinning distance is set to 14-18 cm, the syringe injection speed is set to 0.6-1.0 mL / h, and the parallel movement speed relative to the receiving wheel is set to 8-10 cm / min.

9. An aluminum vacancy defect-free aluminum nitride adsorption film prepared by the preparation method according to any one of claims 7-8.

10. Use of the aluminum vacancy defect aluminum nitride adsorption film according to claim 9 in the adsorption of trifluoroacetonitrile.