Preparation method for catalyzing surface carbon graphitization of lithium iron phosphate material

By adding ferrocene catalyst to the surface of lithium iron phosphate material and using reducing gas to coordinate catalysis, the problem of insufficient graphitization at low temperatures is solved, and the graphitization and electrochemical performance of lithium iron phosphate material is significantly improved, achieving high Conductivity and good rate performance.

CN118908169APending Publication Date: 2024-11-08YIBIN TIANYUAN NEW LITHIUM BATTERY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410942940.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high graphitization of lithium iron phosphate positive electrode materials at lower temperatures, resulting in insufficient conductivity and affecting electrochemical performance.

Method used

By adding a ferrocene catalyst to the surface of lithium iron phosphate material and using hydrogen or ammonia as a reducing gas during high-temperature sintering, the graphitization reaction is synergistically catalyzed to improve the catalyst activity and graphitization degree.

Benefits of technology

It significantly improves the graphitization degree and electrochemical properties of lithium iron phosphate materials, improves the conductivity and rate performance, and has a simple process and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908169A_ABST
    Figure CN118908169A_ABST
Patent Text Reader

Abstract

According to the preparation method for catalyzing the surface carbon graphitization of the lithium iron phosphate material, the catalytic graphitization reaction effect of the catalyst is promoted by utilizing the promoting effect of the reducing gas on the catalytic activity of the catalyst, and the graphitization degree is improved through the synergistic effect of the catalyst and the reducing gas; the carbon-coated lithium iron phosphate positive electrode material with higher graphitization degree is obtained and has higher conductivity, selectivity is achieved between the catalyst and the reducing gas, and the higher graphitization degree can be obtained under the condition that ferrocene is used as the catalyst and hydrogen is used as the reducing gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of lithium iron phosphate positive electrode materials, and more specifically, to a preparation method for graphitizing the surface carbon of lithium iron phosphate materials. Background Art

[0002] At present, the wide application of lithium-ion secondary batteries in 3C electronics, energy storage, new energy vehicles and other industries has brought great convenience to people's daily life. LiFePO4 has been widely used in recent years due to its many advantages such as high safety and long cycle life, but it also has its own inherent disadvantages, such as poor conductivity, slow lithium ion diffusion, low tap density, poor processing performance, etc., which seriously restrict the practical application of LiFePO4. In order to improve the conductivity of the material, conductive materials are usually coated on the surface of lithium iron phosphate particles to improve the conductivity between particles, impurity ions are doped at the lattice position to improve the internal conductivity of the material, and nano-sizing is used to reduce the ion diffusion path to improve the ion conductivity. The above methods can effectively improve the conductivity of lithium iron phosphate positive electrode materials and improve their rate performance. The most common method is to increase the conductivity of lithium iron phosphate positive electrode materials by coating lithium iron phosphate positive electrode materials with carbon and increasing the graphitization degree of carbon. However, a higher degree of graphitization is limited by the reaction temperature and requires >1800°C. However, too high a temperature will lead to excessive grain growth and the generation of impurities. Therefore, studying how to obtain a high degree of graphitization of carbon sources at a lower temperature is a technical problem that needs to be solved. At present, studies have used catalysts to enable carbon sources to obtain a higher degree of graphitization at a lower temperature, improve product purity and conductivity, and thereby improve the electrochemical properties of lithium iron phosphate positive electrode materials.

[0003] For example, Chinese patent CN102347476A discloses a lithium iron phosphate / carbon composite positive electrode material prepared by a catalytic graphitization method and a preparation method thereof. The invention is prepared by a lithium iron phosphate precursor, a carbon source and a catalyst that can promote the graphitization of carbon materials. The catalyst is a transition metal and alloy including one or more of nickel, iron, cobalt, titanium and vanadium, or a metal salt including one or more of cobalt chloride, nickel chloride, chromium acetate, ferrocene, titanium bromide and iodine chloride, and the lithium source, iron source, phosphorus source, carbon source, catalyst or catalyst precursor are sintered in two stages of heat treatment under a non-oxidizing protective atmosphere to obtain a lithium iron phosphate / carbon composite positive electrode material, wherein the amount of the catalyst is 0.1% to 10% of the mass of the lithium iron phosphate, and the carbon content is 1 to 10% of the mass of the final product. Although the addition of a catalyst in the patent effectively improves the graphitization degree of carbon, the specific implementation is carried out under an inert gas, and no reducing gas is used, and there is no mention of the improvement of the catalytic activity of the gas, thereby further promoting the improvement of the graphitization degree.

[0004] For example, Chinese patent CN101572305A discloses a method for preparing a LiFePO4 / C positive electrode material with high rate performance, which comprises weighing raw materials LiFePO4 and a lithium source compound according to a molar ratio of Li to Fe of 1 to 1.05:1, adding a carbon source and a ferrocene catalyst, and ball milling for 8 to 12 hours with anhydrous ethanol as a ball milling medium to obtain a slurry. The obtained slurry is dried and heat-treated under the protection of an inert gas. During this process, the carbon source compound is thermally cracked, and the catalyst interacts with it to form a carbon coating film with a better degree of graphitization and crystallization, so that the prepared lithium iron phosphate positive electrode material has higher electronic conductivity, higher specific capacity and better rate performance; Chinese patent CN103247778A discloses a high-power lithium iron phosphate A positive electrode material and a preparation method thereof, wherein the method firstly mixes a lithium source, an iron source and a phosphorus source in a sufficient proportion, and then sintering the mixture under an inert atmosphere to prepare a lithium iron phosphate precursor, and then introducing a catalyst and an organic carbon source, wherein the catalyst and the organic carbon source are dispersed in a solvent, so that the catalyst is evenly distributed between the lithium iron phosphate precursor and the carbon source, and utilizing the catalytic effect of the catalyst on the carbon source in the carbonization process to effectively improve the graphitization degree of the carbon layer, thereby obtaining a composite material with high graphitization, wherein the catalyst is one or more of ferrocene, cobaltocene and titanocene; the catalyst ferrocene is added in both patents to make the graphitization crystallization degree of the coated carbon higher, but they are sintered at high temperature under an inert gas, and do not mention the improvement of the catalytic activity by the reducing gas, thereby further promoting the improvement of the graphitization degree.

[0005] Therefore, the above-mentioned methods all involve adding an appropriate amount of transition metals and their alloys or their metal salts or organic metal compounds such as ferrocene to the raw materials as a catalyst for the reaction, and utilizing the catalytic effect of the catalyst on the carbon source to promote the graphitization of the carbon material at a relatively low temperature of 500°C to 800°C, thereby obtaining a carbon-coated lithium iron phosphate positive electrode material with a higher degree of graphitization, thereby improving the conductivity between the particles of the carbon-coated lithium iron phosphate positive electrode material and improving its electrochemical performance; however, the addition of the catalyst only improves the carbon graphitization degree from one aspect. If the carbon graphitization degree is to be further improved, it is necessary to find other aspects to cooperate with each other to obtain a carbon-coated lithium iron phosphate positive electrode material with a higher degree of graphitization to achieve better electrochemical performance. Summary of the invention

[0006] In view of the above, the present invention provides a preparation method for catalyzing the graphitization of carbon on the surface of lithium iron phosphate materials, utilizing the promoting effect of reducing gas on the catalytic activity of the catalyst, thereby promoting the catalytic graphitization reaction effect of the catalyst, and improving the degree of graphitization through the synergistic effect of the catalyst and the reducing gas, thereby obtaining a carbon-coated lithium iron phosphate positive electrode material with a higher degree of graphitization and higher conductivity.

[0007] The present invention provides a preparation method for catalyzing the graphitization of carbon on the surface of a lithium iron phosphate material, comprising: mixing lithium carbonate, iron phosphate, glucose, a catalyst and water, and then sequentially performing sand milling and spray drying to obtain a dried material, and then performing a high-temperature sintering step on the obtained dried material to finally obtain a graphitized carbon-coated lithium iron phosphate positive electrode material, wherein the catalyst is ferrocene, and a mixed gas of reducing gas and nitrogen is introduced in the high-temperature sintering step.

[0008] The reducing gas is one of hydrogen or ammonia, and its content is 5wt% of the nitrogen content.

[0009] Ferrocene is used as a catalyst, and its addition amount is 1wt% of the mass of iron phosphate.

[0010] Graphitization is the use of thermal activation to achieve the orderly transformation of thermodynamically unstable carbon atoms from a chaotic layer structure to a graphite crystal structure. During the graphitization process, high-temperature heat treatment is used to provide energy for atomic rearrangement and structural transformation. In order to increase the graphitization degree of difficult-to-graphitize carbon materials, the method of adding catalysts is used to achieve this; and the reducing gas can react with the metal ions or oxides on the surface of the catalyst to form a higher oxidation state or more active metal ions, thereby activating or repairing the surface active sites of the catalyst to improve the catalytic activity of the catalyst, improve the catalytic reaction effect of the catalyst, and further improve the graphitization degree of the lithium iron phosphate material.

[0011] In addition, there is a certain selectivity between the catalyst and the reducing gas. The present invention uses ferrocene as the catalyst. The synergistic catalytic effect of ferrocene and hydrogen has a better synergistic catalytic effect than that of ferrocene and ammonia. Hydrogen can better catalyze the active molecules of ferrocene, thereby making ferrocene have a higher catalytic activity and promoting a further improvement in the graphitization degree of carbon.

[0012] The added amount of glucose is 8wt% of the iron phosphate.

[0013] The molar ratio of Li / Fe in lithium carbonate and iron phosphate is 1.04.

[0014] The sand grinding step is carried out at 30°C, the sand grinding particle size D50 is 0.38-0.40 μm, and the total solid content is 40 wt%.

[0015] In the spray drying step, the feed inlet temperature is 200° C., the discharge outlet temperature is 100° C., the particle size D50 of the obtained dried material is 20-25 μm, and the solid moisture content is 1.0-2.0%.

[0016] The high-temperature sintering step has a temperature of 760°C and a sintering time of 8 hours. The particle size D50 of the graphitized carbon-coated lithium iron phosphate positive electrode material is finally obtained to be 0.91 μm, and the average primary particle size is 200-500 nm.

[0017] The primary particle size will affect the discharge capacity of LiFePO4 material. The smaller the primary particle size, the higher the discharge capacity of the material. The larger the primary particle size, the more serious the polarization phenomenon of the material, causing the discharge potential to decrease. The charge transfer impedance of LiFePO4 material decreases with the decrease of primary particle size. When the material particles are not agglomerated, the finer the primary particle size, the lower the tap density of the material.

[0018] In summary, the method of the present invention promotes the graphitization of lithium iron phosphate materials by adding a catalyst, lowering the graphitization temperature, and adding a reducing gas to increase the reaction activity of the catalyst, promote the catalytic reaction effect of the catalyst, and further increase the graphitization degree of the lithium iron phosphate material. Under the dual action of the catalyst and the reducing gas, the carbon graphitization degree of the lithium iron phosphate material is greatly improved, thereby improving the electrochemical properties of the lithium iron phosphate material. At the same time, there is selectivity between the catalyst and the reducing gas. Under the conditions of ferrocene as a catalyst and hydrogen as a reducing gas, a higher degree of graphitization can be obtained; and the process of the present invention is simple, the production cost is low, and it is suitable for industrial mass production. The material has a highly graphitized carbon coating layer, which can increase the conductivity of the electrode material and is beneficial to the electron transmission process during the charge and discharge process. The prepared iron-based phosphate positive electrode material has a uniform primary particle size, a full morphology, and good rate performance and long cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a test diagram of the electrochemical performance of lithium iron phosphate obtained in the embodiment and the comparative example.

[0020] Figure 2 It is the Raman spectrum of the lithium iron phosphate obtained in the embodiment and the comparative example. DETAILED DESCRIPTION

[0021] The embodiments of the present application will be described in more detail below. The application can be implemented in various forms, and should not be construed as being limited to the embodiments set forth herein, but rather these embodiments are provided to provide a more thorough and complete understanding of the present application. It should be understood that the embodiments of the present application are only for exemplary purposes and are not intended to limit the scope of protection of the present application.

[0022] The present invention is implemented according to the following technical scheme, and the specific steps include: (1) mixing lithium carbonate, iron phosphate, a carbon source, a catalyst and water, wherein the lithium carbonate and the iron phosphate are mixed at a Li / Fe molar ratio of 1.04, the amount of the carbon source added is 8wt% of the iron phosphate, and the amount of ferrocene added is 1wt% of the iron phosphate; (2) then sand grinding was performed at 30° C., the sand grinding particle size D50 was controlled to be 0.38-0.40 μm, and the solid content was 40 wt % to obtain a homogeneous slurry; (3) spray drying the homogenized slurry, wherein the feed inlet temperature of the spray drying is controlled to be 200° C. and the discharge port temperature is controlled to be 100° C.; the particle size D50 of the obtained dried material is controlled to be 20 to 25 μm, and the moisture content is 1 to 2%, to obtain a dried material; (4) sintering the dried material at high temperature in an inert atmosphere containing reducing gas, wherein the reducing gas content is 5wt% of the inert gas, the sintering temperature is 760°C, and the sintering time is 8h; and then crushing the dried material. The particle size D50 of the lithium iron phosphate positive electrode material obtained after crushing is 0.91μm, and the average primary particle size is 200-500nm, thus obtaining the high-conductivity lithium iron phosphate positive electrode material.

[0023] Table 1 shows the process conditions of the embodiments and comparative examples and the test results of the obtained lithium iron phosphate, wherein the Raman spectrum I D / I G It is the data that directly reflects the graphitization degree of the material. It is the ratio of the peak intensity of the D-peak and the G-peak in the Raman spectrum. Both the D-peak and the G-peak are Raman characteristic peaks of C atomic crystals, at 1300cm -1 and 1580cm -1 The D-peak represents the defect of C atom lattice, and the G-peak represents the sp 2 Hybridized in-plane stretching vibration, that is, graphite structure, so I D / I G The smaller the value, the more graphite structures there are and the higher the degree of graphitization. In addition, the higher the degree of graphitization, the better the conductivity of the material will be, and the electrochemical performance will also be relatively improved.

[0024] From the test results of lithium iron phosphate materials in Table 1 and the attached Figure 1 Electrochemical performance test diagram and attached Figure 2 The Raman spectra of can confirm the above, wherein the graphitization degree, electrical conductivity and electrochemical properties of the lithium iron phosphate materials of Examples 1 to 4 are higher than those of the comparative example, indicating that the addition of a catalyst or a reducing gas can promote the improvement of the graphitization degree, electrical conductivity and electrochemical properties of the lithium iron phosphate material, but the graphitization degree, electrical conductivity and electrochemical properties of the lithium iron phosphate material of Examples 1 to 2 are higher than those of Examples 3 to 4, indicating that the synergistic catalysis of the catalyst and the reducing gas can better promote the improvement of the graphitization degree, electrical conductivity and electrochemical properties of the lithium iron phosphate material; further, the graphitization degree, electrical conductivity and electrochemical properties of the lithium iron phosphate material under the synergistic catalysis of ferrocene and hydrogen in Example 1 are higher than the graphitization degree, electrical conductivity and electrochemical properties of the lithium iron phosphate material under the synergistic catalysis of ferrocene and ammonia in Example 2, indicating that there is selectivity between ferrocene and the reducing gas, and the catalytic activity of ferrocene can be better promoted in a hydrogen atmosphere, thereby being more conducive to the improvement of the graphitization degree of carbon.

[0025] Table 1 Process conditions of the embodiments and comparative examples and test results of the obtained lithium iron phosphate.

[0026] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. For example, any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in this application, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A preparation method for catalyzing the graphitization of carbon on the surface of a lithium iron phosphate material, comprising mixing lithium carbonate, iron phosphate, glucose, a catalyst and water, and then sequentially sand-milling and spray-drying to obtain a dried material, and then subjecting the obtained dried material to a high-temperature sintering step to finally obtain a graphitized carbon-coated lithium iron phosphate positive electrode material, characterized in that: The catalyst is ferrocene; a mixed gas of reducing gas and nitrogen is introduced in the high-temperature sintering step.

2. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The reducing gas is one of hydrogen and ammonia, and its content is 5wt% of the nitrogen content.

3. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The added amount of ferrocene is 1wt% of the mass of ferric phosphate.

4. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The added amount of glucose is 8wt% of the ferric phosphate.

5. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The molar ratio of Li / Fe in the lithium carbonate and iron phosphate is 1.

04.

6. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The sand grinding step is carried out at 30°C, the sand grinding particle size D50 is 0.38-0.40 μm, and the total solid content is 40 wt%.

7. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: In the spray drying step, the feed inlet temperature is 200°C, the discharge outlet temperature is 100°C, the particle size D50 of the obtained dried material is 20-25 μm, and the solid moisture content is 1.0-2.0%.

8. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The high temperature sintering step has a temperature of 760° C. and a sintering time of 8 hours.

9. The method for preparing a catalytic graphitization of carbon on the surface of a lithium iron phosphate material according to claim 1, characterized in that: The particle size D50 of the graphitized carbon-coated lithium iron phosphate positive electrode material finally obtained is 0.91 μm, and the average primary particle size is 200-500 nm.

Citation Information

Patent Citations

  • Preparation method of high-performance lithium iron phosphate

    CN114162801A

  • Lithium iron phosphate positive electrode material as well as preparation method and application thereof

    CN114261952A

  • Method of making nanostructured lithium iron phosphate—based powders with an olivine type structure

    US7390472B1