Preparation method of nitrogen-doped hollow porous carbon nanospheres

By using low-cost materials such as rosinyl amino acids and 3-aminophenol, ternary complex colloidal nanospheres are constructed, which solves the complex and cost-effective preparation of hollow porous carbon nanospheres, and realizes the efficient preparation of nitrogen-doped hollow porous carbon Nanospheres are suitable for catalysis and energy storage fields.

CN118908187AActive Publication Date: 2024-11-08JIANGXI KETE CARBON-BASED NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411099372.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing hollow porous carbon nanosphere preparation methods have complex processes, high costs, and difficult to regulate the microstructure of materials, which limit their large-scale production and industrial applications.

Method used

Rosinyl amino acids are used as structural guides, 3-aminophenol is used as carbon source and nitrogen source, and inorganic copper salts are used as complex metals to construct ternary complex colloidal nanospheres in alcohol solvents, polymerize to form hollow structures, and calcination is used. Nitrogen-doped hollow porous carbon nanospheres were obtained.

Benefits of technology

The preparation process is simplified, the utilization rate of structural guide agent is improved, the production cost is reduced, the high specific surface area and rich pore structure of the material are achieved, and it is suitable for catalysis, adsorption and energy storage fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908187A_ABST
    Figure CN118908187A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of nitrogen-doped hollow porous carbon nanospheres, and belongs to the field of functional porous materials. According to the invention, rosin acyl amino acid synthesized by taking natural renewable rosin as a precursor is used as a structure-directing agent, so that the utilization rate is high; meanwhile, 3-aminophenol is used as a carbon source and a nitrogen source, and inorganic copper salt is used as complexing metal, so that the method has the advantages of low cost and wide source. The preparation method is simple and convenient to operate and mild in reaction condition, the preparation process is remarkably shortened, an ideal way is provided for large-scale production and industrial application, and the method has great popularization value. The prepared carbon nanosphere has a clear cavity structure, high dispersity and uniform particle size, surface nitrogen doping is achieved, active sites on the surface of the material are increased, and the activated material is high in specific surface area, has a rich pore structure and is suitable for the fields of catalysis, adsorption, energy storage and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional porous materials, and in particular relates to a method for preparing nitrogen-doped hollow porous carbon nanospheres. Background Art

[0002] Carbonaceous materials have the characteristics of large specific surface area, developed pores, adjustable structure, and rich surface active groups. They have been widely used in adsorption, energy storage, and catalysis (Bai J, Huang J, Yu Q, et al. One-pot synthesis of self S-doped porous carbon for efficient CO2 adsorption[J]. FuelProcessing Technology, 2023, 244: 107700. Kothandam G, Singh G, Guan X, etal. Recent Advances in Carbon-Based Electrodes for Energy Storage and Conversion[J]. Advanced Science, 2023, 10(18): 2301045. Li P, Jiao Y, Ruan Y, et al. Revealing the role of double-layer microenvironments in pH-dependent oxygen reduction activity over metal-nitrogen-carbon catalysts[J]. Nature Communications, 2023, 14(1): 6936.). In particular, various structures of carbon spheres, including hollow structures, core-shell structures, and solid structures, can give carbonaceous materials unique properties (Lan J, Wang B, Bo C, et al. Progress on fabrication and application of activated carbon sphere in recent decade[J]. Journal of Industrial and Engineering Chemistry, 2023, 120: 47-72.). Among them, hollow nanostructures have many advantages in application. For example, large specific surface area and open porous channels can provide abundant active sites for various electrochemical redox reactions.The thin permeable shell greatly reduces the rapid transfer paths of ions and electrons (Zhu J, Zhou H, Zhang C, et al. Dual active nitrogen dopedhierarchical porous hollow carbon nanospheres as an oxygen reduction electrocatalyst for zinc-air batteries[J]. Nanoscale, 2017, 9(35): 13257-13263.), and the cavity provides additional volume to relieve strain and provides sufficient space for electrolyte penetration (Bin D S, Chi ZX, Li Y, et al. Controlling the compositional chemistry in single nanoparticles for functional hollow carbon nanospheres[J]. Journal of the American Chemical Society, 2017, 139(38): 13492-13498.).

[0003] One of the key steps in preparing hollow porous carbon spheres is to control the formation of the hollow core. In the past few decades, the use of hard templates with different structures has been an effective method for preparing hollow porous carbon spheres with different structures. This method mainly includes the customization of spherical templates, the coating and carbonization of carbon sources on the surface of spherical templates, and the removal of templates. The synthesis strategy is relatively complicated, and environmentally unfriendly reagents are often used in the process of template removal (Liu R, Mahurin SM, Li C, et al.Dopamine as a carbon source: the controlled synthesis of hollow carbonspheres and yolk-structured carbon nanocomposites[J]. Angewandte Chemie-International Edition, 2011, 50(30): 6799. Du J, Zong S, Zhang Y, et al. Co-assembly strategy for uniform and tunable hollow carbon spheres withsupercapacitor application[J]. Journal of colloid and interface science,2020, 565: 245-253.).Different soft mold agents have also been used to synthesize porous carbon spheres, such as Triton X-100 (Xu F, Tang Z, Huang S, et al. Facile synthesis of ultrahigh-surface-area hollow carbon nanospheres for enhanced adsorption and energy storage[J]. Naturecommunications, 2015, 6(1): 72-21.), PMMA-b-PEA-b-PAA (Wang Z, Zhang S, Zhang L, et al. Hollow spherical carbonized polypyrrole / sulfur composite cathodematerials for lithium / sulfur cells with long cycle life[J]. Journal of PowerSources, 2014, 248: 337-342.) and PS-b-P2VP-b-PEO (Li Y, Tan H, Salunkhe RR, et al. Hollow carbon nanospheres using an asymmetric triblock copolymerstructure directing agent[J]. Chemical Communications, 2017, 53(1): 236-239.) Compared with the hard template method, the soft template synthesis method has simpler steps. On the one hand, the soft template can be directly removed by thermal decomposition during the carbonization process of the carbon source. On the other hand, the soft template mainly utilizes the self-assembly characteristics of the template to form a spherical core in the reaction system, which can avoid the early customization step of the spherical template. However, since the soft templates used are all amphiphilic compounds, in order to obtain the self-assembled structure of the soft template, a higher concentration is often required. After synthesizing the hollow porous carbon sphere precursor, a large amount of templates still remain in the reaction solvent, and the utilization rate of the soft template is low. However, the soft template itself is expensive, which greatly limits the large-scale production of porous carbon spheres synthesized by the soft template method. At the same time, the self-assembly structure of the soft template is poorly stable, and the control conditions required during the synthesis process are high, which is not conducive to industrial applications. Summary of the invention

[0004] The present invention aims at the problems of complex process, high cost and difficulty in controlling the microstructure of materials in the current hollow porous carbon nanosphere preparation method, and proposes a method for preparing nitrogen-doped hollow porous carbon nanospheres. The method uses rosin acyl amino acid as a structure directing agent, which is synthesized with natural renewable rosin as a precursor, is inexpensive and harmless to the human body. At the same time, 3-aminophenol is used as a carbon source and a nitrogen source, and an inorganic copper salt is used as a complex metal, which has the advantages of low cost and a wide range of sources. The synthetic method is simple to operate and has a short preparation process, and is very suitable for large-scale production and industrial promotion.

[0005] To achieve the above object, the present invention adopts the following technical solutions: The present invention provides a method for preparing nitrogen-doped hollow porous carbon nanospheres, comprising the following steps: S1, dissolving a structure directing agent, copper salt and aminophenol in an alcohol solvent, adding water and stirring to construct ternary complex colloidal nanospheres; Wherein, the structure directing agent is rosin acyl amino acid; S2, adding a polymerizing agent to the solution system obtained in S1, reacting to obtain a hollow carbon nanosphere precursor, and calcining the hollow carbon nanosphere precursor to obtain a hollow porous carbon nanosphere; S3, mixing the hollow porous carbon nanospheres obtained in S2 with an activator, and calcining again to obtain nitrogen-doped hollow porous carbon nanospheres.

[0006] Furthermore, the rosin acyl amino acid in S1 is at least one of N-dehydrorosin acyl-L-phenylalanine, N-dehydrorosin acyl glycine, N-dehydrorosin acyl-L-alanine, N-dehydrorosin acyl-L-phenylglycine and N-dehydrorosin acyl-L-tyrosine.

[0007] Furthermore, the preparation method of the rosin acyl amino acid is as follows: dehydrorosin acid is reacted with oxalyl chloride to obtain dehydrorosin acyl chloride, dehydrorosin acyl chloride acetone solution and sodium hydroxide solution are simultaneously added dropwise to an acetone solution of the amino acid and stirred, the pH value is adjusted to 1-2, and the precipitated solid is filtered, dried, and purified to obtain the amino acid; the amino acid is any one of L-phenylalanine, glycine, L-alanine, L-phenylglycine and L-tyrosine, and the molar ratio of dehydrorosin acyl chloride to the amino acid is 1:2.

[0008] Furthermore, the copper salt described in S1 is at least one of copper chloride, copper nitrate and copper acetate.

[0009] Furthermore, the mass ratio of rosin acyl amino acid, copper salt and aminophenol in S1 is 1:(3-7):(1-3).

[0010] Furthermore, the alcohol solvent in S1 is at least one of methanol, ethanol, isopropanol and acetone; and the volume ratio of the alcohol solvent to water is 1:(4-18).

[0011] Furthermore, the polymerization agent in S2 is at least one of formaldehyde, glyoxal, and terephthalaldehyde; and the mass ratio of aminophenol to the polymerization agent is 1:(0.1-1).

[0012] Furthermore, the activator in S3 is at least one of ferric chloride, phosphoric acid, and zinc chloride; and the mass ratio of the hollow porous carbon nanospheres to the activator is 1:(4-8).

[0013] Furthermore, the calcination temperatures in S2 and S3 are both 800-1000° C., and the calcination time is both 4-6 h.

[0014] The present invention proposes for the first time that rosin acyl amino acid is used as a structure directing agent, 3-aminophenol is used as a carbon source, and copper ions are used as an inducing complex metal, which is dissolved in an alcohol solvent, and water is used to precipitate and construct the three-component complex colloidal nanosphere as a template, and a polymerizer is used to initiate the polymerization of 3-aminophenol. 3-aminophenol at the interface between the ternary complex colloidal nanosphere and the solvent surface is preferentially polymerized, and more 3-aminophenol quickly diffuses and copolymerizes from the inside of the complex colloid to form a hollow structure. After calcination and pyrolysis, the rosin acyl amino acid will decompose and leave, and finally generate hollow porous carbon nanospheres.

[0015] The beneficial effects of the present invention are: 1. The present invention uses rosin acyl amino acid as a structure directing agent, which is synthesized from natural renewable rosin as a precursor, is inexpensive and harmless to the human body. At the same time, 3-aminophenol is used as a carbon source and a nitrogen source, and an inorganic copper salt is used as a complex metal, which has the advantages of low cost and a wide range of sources.

[0016] 2. In the process of the present invention, due to the strong hydrophobicity of rosin acyl amino acid, the structure-directing agent will be completely precipitated when the poor solvent water is introduced into the reaction system, and will be assembled with 3-aminophenol through copper ion bridging to form complex colloidal nanospheres, which greatly improves the utilization rate of the structure-directing agent rosin acyl amino acid (close to 100%). At the same time, 3-aminophenol is both a carbon source and a self-template agent, which solves the instability of the self-assembled structure of the structure-directing agent after the introduction of the carbon source.

[0017] 3. The operation steps of the present invention are simple and easy. It is only necessary to dissolve rosin acyl amino acid, 3-aminophenol and copper salt in alcohol, and add water to form a self-assembled structure. Due to the strong self-assembly ability of rosin acyl amino acid, water can be added quickly at one time without controlling the addition rate. At the same time, since the carbon source 3-aminophenol is also complexed in the colloidal nanospheres, polymerization will preferentially occur at the interface, so the addition rate of the polymerization agent does not need to be strictly controlled, which lays a foundation for the industrial application of the present invention.

[0018] 4. The carbon nanospheres prepared by the present invention have a clear cavity structure, high dispersion and uniform particle size. Surface nitrogen doping increases the surface active sites of the material. The material obtained after activation has a high specific surface area and a rich pore structure, and is suitable for catalysis, adsorption, energy storage and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 These are the SEM images of carbon materials prepared with different rosin acyl amino acids as structure directing agents under the addition of CuCl2: N-dehydrorosin acyl-L-phenylalanine (A), N-dehydrorosin acyl glycine (B), N-dehydrorosin acyl-L-alanine (C), N-dehydrorosin acyl-L-phenylglycine (D), N-dehydrorosin acyl-L-tyrosine (E) and without template addition (F).

[0020] Figure 2 These are SEM images of carbon materials prepared with N-dehydroabietoyl-L-phenylalanine as the structure-directing agent with the addition of different metal salts: CuCl2 (A), FeCl3 (B), CoCl2 (C), NiCl2 (D), ZnCl2 (E) and without added metal salt (F).

[0021] Figure 3 SEM images of iron-activated nitrogen-doped hollow porous carbon nanospheres (A) and unactivated nitrogen-doped hollow carbon nanospheres (B).

[0022] Figure 4 This is the XPS image of nitrogen-doped hollow porous carbon nanospheres.

[0023] Figure 5 TEM image of iron-activated nitrogen-doped hollow porous carbon nanospheres. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0026] The synthetic method of raw material rosin acyl amino acid is specifically as follows: 9 g of dehydroabietic acid was dissolved in dichloromethane, and 5.49 g of oxalyl chloride was added dropwise, and then stirred at room temperature for 4 h. After the reaction was completed, the excess solvent was removed by rotary evaporation to obtain dehydroabietic acid chloride. A certain amount of L-phenylalanine was added to a mixed solution of acetone and water, and the pH value of L-phenylalanine was adjusted to 10 with an aqueous sodium hydroxide solution. Then, 0.5 times the molar amount of L-phenylalanine in dehydroabietic acid chloride acetone solution and an aqueous sodium hydroxide solution were simultaneously added to the solution. After the addition was completed, stirring was continued at room temperature for 3 h. After the reaction was completed, the pH value was adjusted to 1-2 with a 6 M hydrochloric acid solution, and a white solid was precipitated. After suction filtration and drying, a crude N-dehydroabietic acid-L-phenylalanine product was obtained. Finally, it was purified by recrystallization (acetic acid and water) to obtain N-dehydroabietic acid-L-phenylalanine (C da -L-Phe).

[0027] Using the same method, N-dehydroabietyl glycine (C da Gly), N-dehydroabietoyl-L-alanine (C da -L-Ala), N-dehydroabietoyl-L-phenylglycine (C da -L-Phg) and N-dehydroabietoyl-L-tyrosine (C da -L-Tyr).

[0028] Example 1 1. Dissolve 0.1 g N-dehydroabietyl-L-phenylalanine, 0.2 g 3-aminophenol and 0.3 g cupric chloride in 14 mL anhydrous methanol, add 108.5 mL deionized water at 333 K, and stir at 1000 rpm for 40 min.

[0029] 2. Add 0.12 mL of formaldehyde solution (37%) to the obtained solution system, react for 2 h, filter, wash repeatedly with deionized water and ethanol, and obtain the hollow carbon nanosphere precursor under vacuum drying at 313 K. The obtained phenolic resin was placed in a tubular furnace and calcined at 1173 K for 4 h in a N2 atmosphere (heating rate of 3 K / min) to obtain hollow porous carbon nanospheres.

[0030] Example 2 The step parameters are as in Example 1, except that N-dehydroabietoyl-L-phenylalanine is replaced with an equal mass of N-dehydroabietoylglycine.

[0031] Example 3 The step parameters are as in Example 1, except that N-dehydroabietoyl-L-phenylalanine is replaced with an equal mass of N-dehydroabietoyl-L-alanine.

[0032] Example 4 The step parameters are as in Example 1, except that N-dehydroabietoyl-L-phenylalanine is replaced with an equal mass of N-dehydroabietoyl-L-phenylglycine.

[0033] Example 5 The step parameters are as in Example 1, except that N-dehydroabietoyl-L-phenylalanine is replaced with an equal mass of N-dehydroabietoyl-L-tyrosine.

[0034] Example 6 The step parameters are the same as those in Example 1, except that no rosin acyl amino acid is added.

[0035] Figure 1 The following are SEM images of carbon materials prepared with different rosin acyl amino acids as structure directing agents under the addition of CuCl2: N-dehydrorosin acyl-L-phenylalanine (A), N-dehydrorosin acyl glycine (B), N-dehydrorosin acyl-L-alanine (C), N-dehydrorosin acyl-L-phenylglycine (D), N-dehydrorosin acyl-L-tyrosine (E) and without template (F). Figure 1 As shown in AE, the carbon materials added with different rosin acyl amino acids during preparation all have certain regular morphologies, among which N-dehydrorosin acyl-L-phenylalanine ( Figure 1 A), N-dehydroabietoyl-L-phenylglycine ( Figure 1 D) and N-dehydroabietoyl-L-tyrosine ( Figure 1 E) is a uniformly dispersed hollow sphere; the carbon material with N-dehydroabietoylglycine as the structure-directing agent is spherical, but the size is uneven and the agglomeration is serious ( Figure 1 B); The carbon material with N-dehydroabietoyl-L-alanine as the structure-directing agent has a mixed morphology of spherical and tubular shapes ( Figure 1 C); while the carbon material without rosin acyl amino acid addition was irregular granular and agglomerated in large quantities ( Figure 1 F). Therefore, rosin acyl amino acid plays an important role in the formation of hollow spherical structure, and the presence of benzene ring on the amino acid is more conducive to the formation of hollow spheres with stable structure and uniform shape.

[0036] Example 7 Refer to the step parameters of Example 1, except that cupric chloride is replaced with an equal mass of ferric chloride.

[0037] Example 8 Refer to the step parameters of Example 1, except that cupric chloride is replaced with an equal mass of cobalt chloride.

[0038] Example 9 Refer to the step parameters of Example 1, except that cupric chloride is replaced with an equal mass of nickel chloride.

[0039] Example 10 Refer to the step parameters of Example 1, except that cupric chloride is replaced with an equal mass of zinc chloride.

[0040] Embodiment 11 The step parameters are as in Example 1, except that no metal salt is added.

[0041] Figure 2 The following are SEM images of carbon materials prepared with N-dehydroabietyl-L-phenylalanine as the structure-directing agent under the addition of different metal salts: CuCl2 (A), FeCl3 (B), CoCl2 (C), NiCl2 (D), ZnCl2 (E) and without adding metal salt (F). Figure 2 As shown in AF, for the carbon material without adding metal salt, its morphology is a single tubular ( Figure 2 F), when metal salts are introduced into the system, the morphology of the obtained carbon material changes. The carbon material with CuCl2 added is a single hollow sphere ( Figure 2 A); the carbon material with FeCl3 added is a mixture of spheres, rods and flakes ( Figure 2 B); The carbon material with added CoCl2 and NiCl2 is a mixture of spheres and rods ( Figure 2 C and D); while the carbon material with ZnCl2 added is a mixture of spheres and flakes ( Figure 2 E). The above results show that the introduction of metal salts will change the original system structure, and the introduction of CuCl2 is of great significance to the formation of hollow spherical structure.

[0042] Example 12 Referring to the step parameters of Example 1, an activation treatment step was added. The specific activation method was to mix the obtained hollow porous carbon nanospheres with FeCl3, and the mass ratio of the hollow porous carbon nanospheres to FeCl3 was 1:4. After drying, the mixture was placed in a tube furnace and calcined for 4 h at 1173 K in a N2 atmosphere (heating rate of 3 K / min), and finally washed with a 10% hydrochloric acid solution, and then repeatedly washed with deionized water until neutral (pH = 7), to obtain nitrogen-doped hollow porous carbon nanospheres.

[0043] Figure 3 The SEM images of iron-activated nitrogen-doped hollow porous carbon nanospheres (A) and unactivated nitrogen-doped hollow carbon nanospheres (B). Figure 3 A shows that after activation, the sample still maintains a good hollow carbon nanosphere structure. There are a lot of cracks on the surface of the sphere, indicating that it has a rich pore structure, which is formed by the activation of FeCl3. The specific surface area of ​​the obtained material is 1137.18 m 2 / g, pore volume is 0.27 cm 3 / g, which once again proves that the obtained hollow carbon material has a rich pore structure.

[0044] Figure 4 This is the XPS image of nitrogen-doped hollow porous carbon nanospheres. Figure 4 It can be seen that the high-resolution XPS spectrum of material N1s can be divided into four characteristic peaks, namely pyridinic nitrogen (397.31 eV), pyrrolic nitrogen (398.66 eV), graphitic nitrogen (400.83 eV) and quaternary ammonium nitrogen (401.60 eV), which further proves that N in 3-aminophenol is successfully doped into the carbon material.

[0045] Figure 5 TEM image of iron-activated nitrogen-doped hollow porous carbon nanospheres. Figure 5 It can be seen that the prepared carbon nanospheres have a clear cavity structure, and rich pore structures can be observed on the surface of the carbon shell, which once again proves that the obtained material is a hollow porous carbon nanosphere.

[0046] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing nitrogen-doped hollow porous carbon nanospheres, It is characterized in that The steps include: S1, dissolving a structure directing agent, copper salt and aminophenol in an alcohol solvent, adding water and stirring to construct ternary complex colloidal nanospheres; Wherein, the structure directing agent is rosin acyl amino acid; S2, adding a polymerizing agent to the solution system obtained in S1, reacting to obtain a hollow carbon nanosphere precursor, and calcining the hollow carbon nanosphere precursor to obtain a hollow porous carbon nanosphere; S3, mixing the hollow porous carbon nanospheres obtained in S2 with an activator, and calcining again to obtain nitrogen-doped hollow porous carbon nanospheres.

2. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that S1 The rosin acyl amino acid is at least one of N-dehydrorosin acyl-L-phenylalanine, N-dehydrorosin acyl glycine, N-dehydrorosin acyl-L-alanine, N-dehydrorosin acyl-L-phenylglycine and N-dehydrorosin acyl-L-tyrosine.

3. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 2, It is characterized in that The preparation method of the rosin acyl amino acid comprises the following steps: reacting dehydrorosin acid with oxalyl chloride to obtain dehydrorosin acyl chloride, simultaneously dropping dehydrorosin acyl chloride acetone solution and sodium hydroxide solution into an acetone solution of the amino acid and stirring, adjusting the pH value to 1-2, filtering, drying and purifying the precipitated solid to obtain the amino acid; the amino acid is any one of L-phenylalanine, glycine, L-alanine, L-phenylglycine and L-tyrosine, and the molar ratio of dehydrorosin acyl chloride to the amino acid is 1:

2.

4. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that The copper salt in S1 is at least one of copper chloride, copper nitrate and copper acetate.

5. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that The mass ratio of rosin acyl amino acid, copper salt and aminophenol in S1 is 1:(3-7):(1-3).

6. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that S1 The alcohol solvent is at least one of methanol, ethanol, isopropanol and acetone; the volume ratio of the alcohol solvent to water is 1:(4-18).

7. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that S2 The polymerization agent is at least one of formaldehyde, glyoxal, and terephthalaldehyde; the mass ratio of aminophenol to the polymerization agent is 1:(0.1-1).

8. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that S3 The activator is at least one of ferric chloride, phosphoric acid, and zinc chloride; the mass ratio of the hollow porous carbon nanospheres to the activator is 1:(4-8).

9. The method for preparing nitrogen-doped hollow porous carbon nanospheres according to claim 1, It is characterized in that The calcination temperatures in S2 and S3 are both 800-1000° C., and the calcination time is both 4-6 h.

Citation Information

Patent Citations

  • Rosin organic acid metal salt resin with chemical structural characteristics and performances of acrylate metal salt resin and preparation method and application of rosin organic acid metal salt resin

    CN104530986A

  • Three-dimensional porous nitrogen-doped hollow carbon nanosphere, and controllable preparation method and application thereof

    CN110407194A

  • Modified rosin phenolic resin and preparation method thereof

    CN113402686A

  • Preparation method of nitrogen-doped carbon nanospheres with ultrahigh specific surface area

    CN113493204A