Method for regulating and controlling number of layers of graphene

By using commercial copper foil and mixed atmosphere under normal pressure, and using high-temperature hydrogen etching technology, the problem of graphene layer control is solved, and the precise regulation of graphene layer count and the conductivity improvement of graphene layer count is achieved, which is suitable for industrial production. .

CN118908196AInactive Publication Date: 2024-11-08KUNMING UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411005106.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to accurately control the number of graphene layers under normal pressure. The traditional method requires additional vacuum control equipment, which increases cost and control difficulty. It is difficult to keep the copper foil surface consistent when adjusting the flow ratio of methane and hydrogen, resulting in graphite. The number of olefins is inconsistent.

Method used

Using commercial copper foil as a catalytic substrate under normal pressure, a small layer of graphene was prepared in advance under a mixed atmosphere of methane, hydrogen and argon, and argon and hydrogen were introduced at high temperatures above 1000°C, and hydrogen was etched gradually by using hydrogen etching. The layer is thinned and the high-temperature hydrogen etching time is regulated to achieve the preparation of double-layer or single-layer graphene.

Benefits of technology

The precise control of the number of graphene layers under normal pressure is achieved, which reduces the cost of equipment and control difficulty, is mature in the process, is safe and controllable, is suitable for industrial production, and is also improved the conductivity of single-layer or double-layer graphene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908196A_ABST
    Figure CN118908196A_ABST
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling the number of layers of graphene, and belongs to the field of new material preparation. According to the method, few-layer graphene prepared through chemical vapor deposition serves as a starting raw material, hydrogen annealing process treatment is conducted on a graphene / copper composite film at high temperature in a normal-pressure chemical vapor deposition system, the high-temperature hydrogen annealing time is regulated, and double-layer graphene and single-layer graphene can be obtained; the method is simple and easy to implement, has good reproducibility, is suitable for one-way regulation and control of the number of graphene layers from multiple layers to few layers, provides a new idea for preparation of single-layer and double-layer graphene, and has potential industrial application prospects in the fields of composite materials and electronic and electric appliances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for regulating the number of graphene layers and belongs to the field of new material preparation. Background Art

[0002] In recent years, carbon atoms have been 2 The honeycomb structure of graphene formed by hybridization has attracted extensive attention and in-depth research in the scientific community. Under the action of an electric field, the π electrons in the two-dimensional crystal plane of graphene can move freely, thereby showing ultra-high carrier mobility and thermal conductivity, and possessing both metal and semiconductor properties. In addition, graphene also exhibits excellent mechanical properties, with ultra-high strength and flexibility. However, studies have shown that graphene with different numbers of layers exhibits different physical and chemical properties. In terms of thermal conductivity, the thermal conductivity of a single-layer graphene is about 5300 Wm -1 K -1 , while the thermal conductivity of double-layer graphene and four-layer graphene is about 2800 Wm -1 K -1 and 1300Wm -1 K -1 That is, as the number of graphene layers increases, its thermal conductivity gradually decreases; in addition, in terms of electrical properties, graphene also has differences caused by changes in the number of layers; because different application scenarios have different requirements for specific performance, its performance can be effectively regulated by adjusting the number of graphene layers; therefore, when giving full play to the characteristics of graphene to meet the needs of various applications, it is crucial to accurately control its number of layers.

[0003] At present, the technology for controlling the number of graphene layers mainly focuses on regulating the gas flow ratio of methane and hydrogen and the total gas pressure in the reactor; however, many factors affect the preparation of graphene by chemical vapor deposition, including the catalytic ability of the copper foil substrate (due to the different crystal plane orientations of polycrystalline copper foil, the catalytic ability varies) and surface quality, methane and hydrogen partial pressures, growth temperature and growth time; the above growth factors will affect the quality and number of graphene layers. If control is achieved only by adjusting the gas flow ratio of methane and hydrogen, on the one hand, it is necessary to additionally control the gas pressure of the CVD system, thereby increasing the difficulty and cost of control; on the other hand, when trying to adjust the methane to hydrogen flow ratio alone, it is necessary to ensure that other factors are in a normal state; however, it is difficult to keep the surface state of the copper foil consistent, which makes it challenging for traditional methods to repeatedly produce graphene with a consistent number of layers.

[0004] The present invention realizes precise control of the number of graphene layers under normal pressure, and prepares few-layer graphene, double-layer graphene and single-layer graphene without the need for an additional vacuum control unit; compared with traditional methods, this method can significantly reduce control costs and equipment investment. Summary of the invention

[0005] The purpose of the present invention is to provide a method for regulating the number of graphene layers by atmospheric pressure chemical vapor deposition; using commercial copper foil as a catalytic substrate and methane as a carbon source, a few-layer graphene is pre-prepared on an ordinary commercial copper foil in a mixed atmosphere of methane, hydrogen and argon, then the methane is turned off, a certain amount of argon and hydrogen are continuously introduced at a high temperature above 1000°C, and the etching effect of hydrogen on the graphene at high temperature is utilized to achieve layer-by-layer thinning of the few-layer graphene; double-layer or single-layer graphene can be obtained by regulating the etching time of high-temperature hydrogen; the present invention is simple and easy to implement, has good reproducibility, is suitable for unidirectional regulation of the number of graphene layers (from more to less), provides a new idea for the preparation of single-layer and double-layer graphene, and has potential industrial application prospects in the fields of composite materials and electronic appliances.

[0006] In order to achieve the above invention object, the technical solution of the present invention is:

[0007] (1) Using copper foil as a catalyst substrate, pollutants and oxides on the copper foil are removed, and reduction is performed under a constant temperature and a mixed atmosphere of hydrogen and argon to obtain a clean copper foil surface.

[0008] (2) After the reduction is completed, the temperature is continued to be raised to 1020°C through a temperature control program, and a certain flow rate of methane, hydrogen and argon are introduced under normal pressure and kept warm for 20 minutes to obtain few-layer graphene.

[0009] (3) After the growth of the few-layer graphene is completed, the introduction of methane is stopped, and the temperature is continued to be 1020° C. and kept in a mixed atmosphere of hydrogen and argon for 30 min-40 min to obtain double-layer graphene or single-layer graphene.

[0010] Preferably, in step (1) of the present invention, the thickness of the copper foil is 100 μm, 1 mol / L dilute hydrochloric acid is used to remove oxides and pollutants on the surface of the copper foil, and the copper foil is reduced at 300° C. for 120 min in a mixed atmosphere of hydrogen and argon.

[0011] Preferably, the flow ratio of hydrogen to argon in step (1) of the present invention is 1:5.

[0012] Preferably, the purity of the copper foil in step (1) of the present invention is greater than or equal to 99.99%.

[0013] Preferably, in step (2) of the present invention, the flow ratio of methane, hydrogen and argon is 1:20:500, and the flow rate of the mixed gas is 521 sccm.

[0014] Preferably, in step (3) of the present invention, the flow ratio of hydrogen to argon is 2:15, and the flow rate of the mixed gas is 170 sccm.

[0015] The principle of the present invention is as follows: through conventional atmospheric pressure chemical vapor deposition, a few-layer graphene is pre-prepared on an ordinary commercial copper foil in a mixed atmosphere of methane, hydrogen and argon, and then the methane is turned off, and a certain amount of argon and hydrogen are continuously introduced at a high temperature above 1000°C, and the etching effect of hydrogen on graphene at high temperature is utilized to achieve layer-by-layer thinning of the few-layer graphene, and the time of high-temperature hydrogen etching is regulated to obtain double-layer and single-layer graphene.

[0016] Beneficial effects of the present invention:

[0017] (1) In the present invention, all preparation processes are completed under normal pressure, and no additional vacuum control equipment is required, which saves equipment costs compared with traditional methods.

[0018] (2) The present invention provides a new idea for controlling the preparation of graphene with different numbers of layers, and it is simple and easy to implement.

[0019] (3) The process of the present invention is mature, safe, controllable and highly repeatable, and is suitable for industrial production.

[0020] (4) The single-layer or double-layer graphene / copper wire prepared by this process exhibits better electrical conductivity than pure copper wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a process flow chart of the present invention.

[0022] Figure 2 This is the Raman spectrum of few-layer graphene transferred to silicon wafer.

[0023] Figure 3 This is the Raman spectrum of bilayer graphene transferred to a silicon wafer.

[0024] Figure 4 This is the Raman spectrum of a single layer of graphene transferred to a silicon wafer. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the described contents.

[0026] Example 1

[0027] A method for regulating the number of graphene layers, comprising the following steps:

[0028] (1) A 100 μm thick commercial copper foil was used as the catalyst substrate and cut into 5*5 cm 2The copper foil was prepared by preliminarily removing pollutants and oxides on the copper foil using 1 mol / L dilute hydrochloric acid, and then rinsed with deionized water and alcohol for several times to remove residual acid. The copper foil was then placed in a CVD system and reduced at a constant temperature of 300°C in a mixed atmosphere of 50 sccm of hydrogen and 250 sccm of argon for 120 minutes to further remove the oxides and obtain a clean copper foil.

[0029] (2) After the reduction is completed, the furnace temperature is further raised to 1020°C within 70 minutes through the temperature control program, and 1sccm of methane, 20sccm of hydrogen and 500sccm of argon are introduced under normal pressure, and the growth is kept warm for 20 minutes. After the growth is completed, the methane valve is closed, and the temperature is continued to be kept at 1020°C for 30 minutes under 20sccm of hydrogen and 150sccm of argon, and then cooled to room temperature under 20sccm of hydrogen and 500sccm of argon to obtain a double-layer graphene / copper composite film.

[0030] (3) The prepared double-layer graphene-copper composite film is attached to the surface of a thermal release tape, and placed in a ferric chloride solution (prepared with 10 g of ferric chloride, 10 ml of 28% hydrochloric acid and 100 ml of deionized water) to dissolve the copper foil. After 24 hours, the thermal release tape is taken out, rinsed with deionized water and dried. Subsequently, the thermal release tape is adhered to a SiO2 / Si sheet with a thickness of 300 nm and heated at 120°C for 120 seconds to transfer the grown graphene to the surface of the SiO2 / Si sheet. The morphology of the graphene is observed by a metallographic microscope or the Raman spectrum is tested to detect the quality of the graphene. The Raman spectrum of the obtained few-layer graphene is as follows: Figure 3 As shown in the figure, it can be seen that the Raman spectrum of graphene is about 1356cm -1 The intensity of the defect peak D is very low, and at about 1585cm -1 The intensity of the characteristic peak G near the D / I G =0.29, the defect level is low, indicating that the quality of graphene is high, and at 2712cm -1 The nearby 2D peak height is lower than 1585.7cm -1 The characteristic peak G near the 2D / I G =1.36, indicating that the number of graphene layers is 2. Therefore, high-quality double-layer graphene was prepared on the copper foil.

[0031] Example 2

[0032] A method for regulating the number of graphene layers, comprising the following steps:

[0033] (1) A 100 μm thick commercial copper foil was used as the catalyst substrate and cut into 5*5 cm 2 The copper foil was prepared by preliminarily removing pollutants and oxides on the copper foil using 1 mol / L dilute hydrochloric acid, and then rinsed with deionized water and alcohol for several times to remove residual acid. The copper foil was then placed in a CVD system and reduced at a constant temperature of 300°C in a mixed atmosphere of 50 sccm of hydrogen and 250 sccm of argon for 120 minutes to further remove the oxides and obtain a clean copper foil.

[0034] (2) After the reduction is completed, the furnace temperature is further raised to 1020°C within 70 minutes through the temperature control program, and 1 sccm of methane, 20 sccm of hydrogen and 500 sccm of argon are introduced under normal pressure, and the growth is kept warm for 20 minutes. After the growth is completed, the methane valve is closed, and the temperature is continued to be kept at 1020°C for 40 minutes under 20 sccm of hydrogen and 150 sccm of argon, and then cooled to room temperature under 20 sccm of hydrogen and 500 sccm of argon to obtain a single-layer graphene / copper composite film.

[0035] (3) The prepared single-layer graphene-copper composite film is attached to the surface of a thermal release tape, and placed in a ferric chloride solution (prepared with 10 g of ferric chloride, 10 ml of 28% hydrochloric acid and 100 ml of deionized water) to dissolve the copper foil. After 24 hours, the thermal release tape is taken out, rinsed with deionized water and dried. Subsequently, the thermal release tape is adhered to a SiO2 / Si sheet with a thickness of 300 nm and heated at 120°C for 120 seconds to transfer the grown graphene to the surface of the SiO2 / Si sheet. The morphology of the graphene is observed by a metallographic microscope or the Raman spectrum is tested to detect the quality of the graphene. The Raman spectrum of the obtained few-layer graphene is as follows: Figure 4 As shown in the figure, it can be seen that the Raman spectrum of graphene is about 1356cm -1 The intensity of the defect peak D is very low, and at about 1585cm -1 The intensity of the characteristic peak G near the D / I G =0.14, the defect level is low, indicating that the quality of graphene is high, and at 2712cm -1 The nearby 2D peak height is lower than 1585.7cm -1 The characteristic peak G near the 2D / I G =2.03, indicating that the number of graphene layers is 1. Therefore, a high-quality single-layer graphene was prepared on the copper foil.

[0036] Comparative Example 1

[0037] A method for regulating the number of graphene layers, comprising the following steps:

[0038] (1) A 100 μm thick commercial copper foil was used as the catalyst substrate and cut into 5*5 cm 2 The copper foil was prepared by preliminarily removing pollutants and oxides on the copper foil using 1 mol / L dilute hydrochloric acid, and then rinsed with deionized water and alcohol for several times to remove residual acid. The copper foil was then placed in a CVD system and reduced at a constant temperature of 300°C in a mixed atmosphere of 50 sccm of hydrogen and 250 sccm of argon for 120 minutes to further remove the oxides and obtain a clean copper foil.

[0039] (2) After the reduction is completed, the furnace temperature is further raised to 1020°C within 70 minutes through the temperature control program, and 1 sccm of methane, 20 sccm of hydrogen and 500 sccm of argon are introduced under normal pressure, and the growth is kept warm for 20 minutes. After the growth is completed, the methane valve is closed and the film is cooled to room temperature under 20 sccm of hydrogen and 500 sccm of argon to obtain a composite film of few-layer graphene / copper foil.

[0040] (3) The prepared few-layer graphene-copper composite film is attached to the surface of a thermal release tape, and placed in a ferric chloride solution (prepared with 10 g of ferric chloride, 10 ml of 28% hydrochloric acid and 100 ml of deionized water) to dissolve the copper foil. After 24 hours, the thermal release tape is taken out, rinsed with deionized water and dried. Subsequently, the thermal release tape is adhered to a SiO2 / Si sheet with a thickness of 300 nm and heated at 120°C for 120 seconds to transfer the grown graphene to the surface of the SiO2 / Si sheet. The morphology of the graphene is observed by a metallographic microscope or the Raman spectrum is tested to detect the quality of the graphene. The Raman spectrum of the obtained few-layer graphene is as follows: Figure 2 As shown in the figure, it can be seen that the Raman spectrum of graphene is about 1356cm -1 The intensity of the defect peak D is very low, and at about 1585cm -1 The intensity of the characteristic peak G near the D / I G =0.08, the defect level is very low, indicating that the quality of graphene is high, and at 2712cm -1 The nearby 2D peak height is lower than 1585.7cm -1 The characteristic peak G near the 2D / I G =0.77, indicating that the number of graphene layers is about 4 to 6. Therefore, high-quality few-layer graphene is prepared on the copper foil.

Claims

1. A method for regulating the number of graphene layers, characterized in that: The specific steps include: (1) Using copper foil as a catalyst substrate, removing pollutants and oxides on the copper foil, and reducing it under a constant temperature and a mixed atmosphere of hydrogen and argon to obtain a clean copper foil surface; (2) After the reduction is completed, the temperature is continued to be raised to 1020°C through the temperature control program, and a certain flow rate of methane, hydrogen and argon are introduced under normal pressure, and the temperature is kept for 20 minutes to obtain few-layer graphene; (3) After the growth of the few-layer graphene is completed, the introduction of methane is stopped, and the temperature is continued to be 1020° C. and kept in a mixed atmosphere of hydrogen and argon for 30-40 min to obtain double-layer graphene or single-layer graphene.

2. The method for controlling the number of graphene layers according to claim 1, characterized in that: In step (1), the thickness of the copper foil is 100 μm, and 1 mol / L dilute hydrochloric acid is used to remove oxides and pollutants on the surface of the copper foil, and the copper foil is reduced at 300° C. for 120 min in a mixed atmosphere of hydrogen and argon.

3. The method for controlling the number of graphene layers according to claim 2, characterized in that: In step (1), the flow ratio of hydrogen to argon is 1:

5.

4. The method for controlling the number of graphene layers according to claim 2, characterized in that: Step (1) The purity of the copper foil is greater than or equal to 99.99%.

5. The method for controlling the number of graphene layers according to claim 1, characterized in that: In step (2), the flow ratio of methane, hydrogen and argon is 1:20:500, and the flow rate of the mixed gas is 521 sccm.

6. The method for controlling the number of graphene layers according to claim 1, characterized in that: In step (3), the flow ratio of hydrogen to argon is 2:15, and the flow rate of the mixed gas is 170 sccm.

Citation Information

Patent Citations

  • Method for preparing thin layer graphene on surface of metal catalyst

    CN103572247A

  • Atmospheric pressure controlled growth method for graphene

    CN103708448A

  • Double-layer graphene and preparation method thereof

    CN111777062A

  • Two-dimensional single-layer dendritic crystal graphene film and preparation method thereof

    CN116199211A

  • High quality large scale single and multilayer graphene production by chemical vapor deposition

    US20130174968A1