Preparation method of activated carbon for polar solvent recovery
By employing a two-stage preparation method using biomass and phosphoric acid activators derived from phosphaphenanthrene derivatives, the problem of insufficient adsorption capacity of activated carbon for polar solvents was solved, and activated carbon with excellent adsorption performance for methanol and ethanol was prepared, meeting the recycling needs of the pharmaceutical and chemical industries.
Patent Information
- Application Number
- CN202411274899.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-12
AI Technical Summary
Existing activated carbon has poor adsorption capacity for polar organic solvents such as methanol and ethanol, making it difficult to meet the needs of pharmaceutical companies and the chemical industry for the recovery of polar solvents.
Using biomass as raw material and phosphoric acid as activating agents, activated carbon with a large specific surface area and rich pore structure is prepared through a two-stage activation process, which is suitable for the recovery of polar solvents.
The prepared activated carbon exhibits excellent adsorption performance for methanol and ethanol, enabling efficient recovery of polar solvents.
Smart Images

Figure BDA0005039854960000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of activated carbon, and in particular relates to a method for preparing activated carbon for recovering polar solvents. Background Art
[0002] With the development of economy, the environmental pollution, high cost and high energy consumption caused by the initial extensive economic model have become increasingly prominent, and the transformation to a sustainable economic model is imperative. This transformation will focus on improving resource utilization efficiency, reducing energy consumption, reducing pollutant emissions, protecting the ecological environment, and achieving coordinated development of economic development and environmental protection. The recycling of organic solvents not only meets the social needs of environmental protection, but also meets the urgent needs of solvent users to reduce production costs and improve market competitiveness.
[0003] Adsorption is a representative recovery technology for separating and concentrating organic solvents. The most common method is to use the adsorption properties of adsorption materials such as activated carbon, activated carbon fiber, zeolite, molecular sieve, porous clay ore, activated alumina, silica gel and polymer adsorption resin to first adsorb and concentrate the organic solvent onto the adsorption material, and then use temperature, pressure or other methods to desorb the concentrated organic solvent from the adsorption material and then recycle it. The technology has the advantages of a wide range of applications and relatively stable effects.
[0004] Activated carbon is a commonly used hydrophobic adsorbent. Compared with other adsorbent materials, it has the advantages of strong adsorption capacity, good selectivity, strong regeneration, and low cost. It has been widely used in the fields of air purification and industrial waste gas treatment. Common activated carbons include charcoal, coal, coconut shell charcoal, etc. For example, the patent CN103588200B discloses a method for producing wood coal-based molded activated carbon, which includes: (1) mixing sawdust and coal powder in proportion, soaking them in a phosphoric acid solution, taking them out, putting them in an oil bath pot, and plasticizing them until the color of the mixture changes from brown to black and produces greater viscosity, then ending the plasticization to obtain a plasticized product; (2) quickly transferring the obtained plasticized product to a mold, molding it on a hydraulic press, and placing the pressed carbonaceous precursor molded product in a drying oven for slow constant temperature drying and hardening; (3) carbonizing and activating the prepared molded carbonaceous precursor in an activation furnace to obtain a wood coal-based molded activated carbon. Patent CN1290606C discloses wood-based automotive activated carbon and a preparation method thereof. The method of the invention comprises the following steps: mixing wood and a catalyst, and then subjecting the mixture to shaping (granulation), shaping (carbonization), activation, and drying steps to prepare a high-performance wood-based shaped activated carbon.
[0005] Activated carbon is composed of graphitized carbon microcrystals and non-graphitized amorphous carbon. It is a hydrophobic adsorbent with the characteristic of selectively adsorbing non-polar saturated hydrocarbon compounds. However, a large amount of methanol and ethanol with high polarity are used in pharmaceutical companies, adhesive tapes, and chemical industries. Methanol and ethanol are the main industrial waste gases, and activated carbon has poor selective adsorption performance for polar solvents such as methanol. Therefore, it is necessary to prepare an activated carbon with high efficiency in adsorbing polar solvents to meet the demand for polar solvent recovery in pharmaceutical companies, adhesive tapes, chemical industries, and other fields. Summary of the invention
[0006] In order to solve the technical problem of poor adsorption capacity of activated carbon for polar organic solvents in the prior art, the present invention provides a method for preparing activated carbon for polar solvent recovery, using biomass as raw material, phosphaphenanthrene derivatives and phosphoric acid as activators, and through two stages of activation, the prepared activated carbon has a large specific surface area, rich pore structure and appropriate surface chemical structure, so that it exhibits excellent adsorption performance for organic solvents with high polarity such as methanol and ethanol.
[0007] In order to achieve the above purpose, the following technical solutions are adopted:
[0008] A method for preparing activated carbon for polar solvent recovery comprises the following steps:
[0009] 1) crushing and drying the biomass to obtain biomass powder;
[0010] 2) preparing a mixed solution of an activator, a surfactant and an alcohol, uniformly mixing the biomass powder with the mixed solution, kneading the mixture with a vacuum kneader, and then extruding and granulating, hardening, first-stage low-temperature activation, second-stage high-temperature activation, cooling, washing and drying to obtain activated carbon for polar solvent recovery;
[0011] The activator is prepared by compounding a phosphaphenanthrene derivative and a phosphoric acid solution in a mass ratio of 5-10:100.
[0012] Step 1) The biomass is selected from one or a combination of two or more of coconut shell, apricot shell, palm shell, wood powder, sawdust, wood chips, and wood shavings. The biomass is crushed to 100-150 mesh. The drying is performed at 100-150° C. to a constant weight.
[0013] Step 2) The phosphaphenanthrene derivative is selected from 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide (CAS No.: 99208-50-1), [(6-oxo-6H-dibenzo[C,E][1,2]oxaphosphanin-6-yl)methyl]succinic acid (CAS No.: 63562-33-4), 9,10-dihydro-9-oxa-10-phosphaphenanthrene-1 0-ethanol 10-oxide (CAS No.: 63562-41-4), 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-methanol 10-oxide (CAS No.: 35948-26-6), or a combination of two or more thereof, preferably 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide (CAS No.: 99208-50-1).
[0014] Furthermore, the phosphoric acid solution has a concentration of 60-80 wt%.
[0015] Furthermore, the surfactant is selected from one or a combination of two or more of alkylphenol polyoxyethylene ether, stearate, sodium alkylbenzene sulfonate, and sodium alkylnaphthalene sulfonate.
[0016] Furthermore, the surfactant is an alkylphenol polyoxyethylene ether, selected from one or a combination of two or more of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, nonylphenol polyether-3, nonylphenol polyether-2, preferably nonylphenol polyoxyethylene ether. The alcohol is selected from one or a combination of two of methanol, ethanol, and isopropanol.
[0017] Furthermore, the mass ratio of the activator, surfactant, alcohol and biomass powder is 105-110:0.05-0.1:10-20:70-90.
[0018] Further, the kneading conditions are kneading at a vacuum degree of -0.01MPa to -0.1MPa and 100-180°C for 1-5h. The hardening is hardening the particles obtained by granulation at 100-150°C for 1-3h. The first stage low-temperature activation is activation at 350-400°C for 10-30min, and the second stage high-temperature activation is activation at 500-600°C for 1-3h. The cooling is natural cooling to room temperature. The washing is washing with water to a pH of 5-7. The drying is drying at 100-150°C to constant weight.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention uses biomass as raw material, phosphaphenanthrene derivatives and phosphoric acid as activators, and through two stages of activation, the prepared activated carbon has a large specific surface area, rich pore structure and appropriate surface chemical structure, so that it exhibits excellent adsorption performance for organic solvents with high polarity such as methanol and ethanol. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.
[0022] Example 1
[0023] 1) Grinding coconut shell into 150 mesh and drying at 100° C. to constant weight to obtain coconut shell powder;
[0024] 2) A mixed solution prepared by mixing 10 parts of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide and 100 parts of 60wt% phosphoric acid solution, 0.1 part of nonylphenol polyoxyethylene ether and 20 parts of ethanol, 70 parts of coconut shell powder and the mixed solution are uniformly mixed, and then kneaded for 2 hours at a vacuum degree of -0.08MPa and 150°C using a vacuum kneader, followed by extrusion granulation, hardening at 150°C for 1 hour, first-stage low-temperature activation at 350°C for 30 minutes, second-stage high-temperature activation at 500°C for 3 hours, natural cooling to room temperature, washing with water to a pH of 7, and drying at 100°C to constant weight to obtain columnar activated carbon for solvent recovery with a diameter of 3.4 mm and a length of 5.7 mm.
[0025] Example 2
[0026] The rest of the examples are the same as in Example 1, except that the amount of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide used is 5 parts.
[0027] Example 3
[0028] The rest of the examples are the same as in Example 1, except that the amount of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide used is 3 parts.
[0029] Example 4
[0030] The rest of the examples are the same as in Example 1, except that the amount of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide used is 12 parts.
[0031] Example 5
[0032] The rest of Example 1 is the same, except that an equal mass of [(6-oxo-6H-dibenzo[C,E][1,2]oxaphosphorin-6-yl)methyl]succinic acid is used to replace 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide.
[0033] Example 6
[0034] The rest of Example 1 is the same, except that octylphenol polyoxyethylene ether is used instead of nonylphenol polyoxyethylene ether with the same mass.
[0035] Example 7
[0036] The rest of Example 1 is the same, except that calcium stearate of the same mass is used to replace nonylphenol polyoxyethylene ether.
[0037] Example 8
[0038] The rest of the examples are the same as in Example 1, except that the amount of ethanol used is 10 parts.
[0039] Example 9
[0040] The rest of Example 1 is the same, except that, in step 2), 5 parts of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, 100 parts of 80wt% phosphoric acid solution, 0.05 parts of nonylphenol polyoxyethylene ether, and 10 parts of ethanol are prepared into a mixed solution, 90 parts of coconut shell powder are evenly mixed with the mixed solution, and then kneaded with a vacuum kneader at -0.08MPa and 150°C for 2h, followed by extrusion granulation, hardening at 150°C for 1h, low-temperature activation at 400°C for 10min in the first stage, high-temperature activation at 500°C for 3h in the second stage, naturally cooled to room temperature, washed with water to pH 7, and dried at 100°C to constant weight to obtain activated carbon for polar solvent recovery.
[0041] Comparative Example 1
[0042] The rest of the embodiment is the same as in Example 1, except that:
[0043] Step 2) 10 parts of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, 100 parts of 60wt% phosphoric acid solution compounded activator, 0.1 parts of nonylphenol polyoxyethylene ether, 20 parts of ethanol are prepared into a mixed solution, 70 parts of coconut shell powder are taken and mixed with the mixed solution, and then kneaded for 2 hours at -0.08MPa and 150°C with a vacuum kneader, and then extruded and granulated, hardened at 150°C for 1 hour, activated at 500°C for 3 hours, naturally cooled to room temperature, washed with water to pH 7, and dried at 100°C to constant weight, to obtain activated carbon for polar solvent recovery. That is, only the second stage of high temperature activation is performed.
[0044] Comparative Example 2
[0045] The rest of Example 1 is the same, except that the activator is 110 parts of 60 wt % phosphoric acid solution.
[0046] Comparative Example 3
[0047] The rest of the process is the same as in Example 1, except that no ethanol is added.
[0048] The activated carbon prepared in the above examples and comparative examples was subjected to the following performance tests:
[0049] 1. Pore structure characterization: measured by NOVA 1000e pore structure specific surface area tester. The sample was degassed at 350℃ for 2h, and liquid nitrogen was used as the adsorption medium at 77K and relative pressure (P / P0) 10 -6 N2 adsorption was carried out in the range of -1, and the specific surface area was calculated by BET equation.
[0050] 2. Dynamic adsorption test: The test equipment TP-5080 fully automatic multi-purpose adsorption instrument (Tianjin Xianquan Industry and Trade Development Co., Ltd.) is connected to the gas chromatograph. The activated carbon is first dried at 200°C for 2h and loaded into the quartz adsorption column. The cylinder is opened and the pressure reducing valve and flow meter are adjusted to make the flow rate 30mL / min. The mass ratio of methanol or ethanol to nitrogen is 8%, and the pressure is one atmosphere. Nitrogen is blown into the adsorption column at room temperature (15-20°C) through the liquid storage tank. The organic gas concentration at the sampling port is measured every 3 minutes. When the concentration remains unchanged and is maintained for 30 minutes, it is considered that the activated carbon adsorption has reached adsorption equilibrium, and the equilibrium adsorption amount is recorded in mg / g.
[0051] Table 1 Test results
[0052]
[0053] It can be seen from Table 1 that the present invention uses a compound of a phosphaphenanthrene derivative and a phosphoric acid solution as an activator, and the activated carbon prepared has a large specific surface area and a rich pore structure, and exhibits excellent adsorption performance for organic solvents with high polarity such as methanol and ethanol.
[0054] It can be seen from the microporosity test results of Examples 1-4 that the change in the relative amount of tiny phosphaphenanthrene derivatives causes a large change in the equilibrium adsorption amount. It is speculated that the phosphaphenanthrene derivatives and phosphoric acid solution have different chemical structures and properties, and have different penetration and catalytic hydrolysis rates on biomass raw materials, resulting in the pore structure and surface polarity of the activated carbon being greatly affected by the composite ratio of the two. The pore structure formed by the excessively large composite ratio of the two is relatively complex, and the adsorption sites are unevenly distributed, which increases the diffusion resistance, slows down or even hinders the polar molecules from reaching the adsorption sites; the composite ratio is too small, the pore size is larger, the surface polarity is smaller, the interaction force is weakened, and the polar solvent is quickly discharged, which is not conducive to adsorption. Therefore, the selection of the composite of phosphaphenanthrene derivatives and phosphoric acid solution needs to be appropriate.
[0055] It can be seen from Example 1 and Comparative Example 2 that if the activator is all phosphoric acid, although the specific surface area is large, the surface chemical structure of the activated carbon is not conducive to promoting the adsorption of methanol and ethanol, and the equilibrium adsorption amount of methanol and ethanol is still low.
[0056] It can be seen from Example 1, Example 8 and Comparative Example 3 that as the amount of ethanol used decreases, the average pore size increases, the microporosity decreases, and the specific surface area decreases. It is speculated that ethanol helps the dissolution of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, promoting its more uniform mixing with coconut shell powder and more conducive to penetration.
Claims
1. A method for preparing activated carbon for polar solvent recovery, It is characterized in that The steps include: 1) crushing and drying the biomass to obtain biomass powder; 2) preparing a mixed solution of an activator, a surfactant and an alcohol, uniformly mixing the biomass powder with the mixed solution, kneading the mixture with a vacuum kneader, and then extruding and granulating, hardening, first-stage low-temperature activation, second-stage high-temperature activation, cooling, washing and drying to obtain activated carbon for polar solvent recovery; The activator is prepared by compounding a phosphaphenanthrene derivative and a phosphoric acid solution in a mass ratio of 5-10:
100.
2. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that Step 1) The biomass is selected from one or a combination of two or more of coconut shells, apricot shells, palm shells, wood powder, sawdust, wood chips, and wood shavings.
3. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The method comprises crushing the powder to 100-150 mesh and drying the powder at 100-150° C. to a constant weight.
4. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that Step 2) The phosphaphenanthrene derivative is selected from 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, [(6-oxo-6H-dibenzo[C,E][1,2]oxaphosphahexanin-6-yl)methyl]succinic acid, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-ethanol 10-oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-methanol 10-oxide, or a combination of two or more thereof, preferably 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide.
5. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The concentration of the phosphoric acid solution is 60-80 wt %.
6. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The surfactant is selected from one or a combination of two or more of alkylphenol polyoxyethylene ether, stearate, sodium alkylbenzene sulfonate, and sodium alkylnaphthalene sulfonate.
7. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The surfactant is an alkylphenol polyoxyethylene ether, selected from one or a combination of two or more of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, nonylphenol polyether-3, nonylphenol polyether-2, preferably nonylphenol polyoxyethylene ether. The alcohol is selected from one or a combination of two of methanol, ethanol, and isopropanol.
8. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The mass ratio of the activator, surfactant, alcohol and biomass powder is 105-110: 0.05-0.1: 10-20: 70-90.
9. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The kneading conditions are kneading at a vacuum degree of -0.01 MPa to -0.1 MPa and 100-180° C. for 1-5 hours; The hardening is to harden the particles obtained by granulation at 100-150° C. for 1-3 hours.
10. The method for preparing activated carbon for polar solvent recovery according to claim 1, It is characterized in that The first stage of low-temperature activation is activation at 350-400°C for 10-30 minutes, and the second stage of high-temperature activation is activation at 500-600°C for 1-3 hours.
Citation Information
Patent Citations
Preparation method of high purity cyclic phosphonate 9,10-dihydro-9-oxa-10-phosphaphenanathrene-10-oxide
CN102219806A
Light-curing thermal-curing resin composition
CN103576452A
Composite material for electrodes, method for producing same, and secondary battery
CN105122519A
Method for preparing biomass formed activated carbon by low-temperature pre-pyrolysis and raw material ultra refinement
CN108439403A
Preparation method of phosphorus-silicon-containing hybrid nanometer oxyhydroxide for improving application of epoxy resin in liquid oxygen
CN108976473A