Silicon oxide composite material for negative electrode of lithium ion battery and preparation method of silicon oxide composite material
By using a composite material of a specific ratio of carbon source and silicon source in lithium-ion batteries to form a solid structure and an appropriate pore structure, the performance attenuation problems caused by insufficient capacitance and volume expansion of silicon oxide-based anode materials are solved, and the battery is improved Capacitance and cycling stability.
Patent Information
- Application Number
- CN202410955956.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The capacity of the silicon oxide-based anode material of existing lithium-ion batteries is poor, unable to meet market demand, and the structural damage and battery performance decay due to volume expansion.
Using a composite material of a specific ratio of carbon source and silicon source, the silicon oxide particles are supported by forming a solid structural frame and appropriate pore structure, preventing them from fragmenting during charging and discharging, and forming a stable and thin solid electrolyte interface. The membrane improves the diffusion rate of lithium ions and the power characteristics of the battery.
It improves the reversible storage amount and capacity of lithium ions, extends the cycle life of the battery, and improves the power characteristics and electrochemical performance of the battery.
Smart Images

Figure BDA0004948775520000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium batteries, and specifically relates to a silicon oxide composite material for a negative electrode of a lithium ion battery and a preparation method thereof. Background Art
[0002] The negative electrode material of lithium-ion batteries plays a key role in the charging and discharging process of the battery. It is responsible for storing and releasing lithium ions. At present, the negative electrode materials of lithium-ion batteries can be mainly divided into two categories: carbon-based materials and other non-carbon-based materials. Carbon-based negative electrode materials, graphite materials are the most common negative electrode materials for lithium-ion batteries, including natural graphite and artificial graphite. Graphite materials have a layered structure, and lithium ions can be inserted and removed between layers. This process is called "lithium insertion" and "lithium extraction". The advantages of graphite negative electrode materials include: High Coulomb efficiency: During the charging and discharging process, graphite can efficiently accept and release lithium ions. Stable cycle performance: Graphite materials can still maintain their structural stability after multiple charging and discharging. Lower redox potential: It is conducive to improving the overall voltage and energy density of the battery. Low cost: Graphite materials are widely available and relatively low in price. In addition to graphite, there are some other carbon-based materials, such as hard carbon and soft carbon, which are also used as negative electrode materials for lithium-ion batteries, and are usually more popular in some special applications. Among non-carbon-based negative electrode materials, silicon-based materials have received widespread attention due to their high theoretical capacity. In theory, the capacity of silicon can be more than ten times that of graphite. However, silicon will have a large volume expansion during the charging and discharging process, which may lead to the destruction of the material structure and the attenuation of battery performance. Tin-based materials and alloy materials (such as silicon-based alloys, germanium-based alloys, etc.) have also been studied due to their higher theoretical capacity, but they also face the problem of volume expansion. Metallic lithium is theoretically the most ideal negative electrode material because it has a very high energy density and low electrochemical potential, but due to the formation of lithium dendrites and safety issues, metallic lithium has not yet been widely used in commercial lithium-ion batteries.
[0003] With the development of technology, some new negative electrode materials such as nanomaterials, composite materials and transition metal oxides are also being researched and developed to solve the limitations of existing materials and improve the energy density, power density and cycle life of batteries. At present, graphite is still the most widely used negative electrode material in the market, but with the advancement of technology in the future, new negative electrode materials may gradually occupy a larger market share.
[0004] As the negative electrode material of lithium-ion batteries, silicon oxide-based materials are considered to be one of the most promising negative electrode materials for the next generation of lithium-ion batteries due to their high theoretical capacity, abundant resources, and low cost. Silicon oxide-based materials mainly include silicon dioxide, silicon dioxide, and other compounds containing silicon and oxygen. The current silicon oxide-based negative electrode materials on the market have poor electrical capacity and cannot meet market demand. Therefore, there is an urgent need for a silicon oxide composite material for lithium-ion battery negative electrode and a preparation method thereof. Summary of the invention
[0005] The purpose of the present invention is to provide a silicon oxide composite material for lithium ion battery negative electrode and a preparation method thereof.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode comprises the following steps:
[0008] (1) dissolving 1 part by mass of a silicon source in 2-4 parts by mass of anhydrous ethanol, adding 4-6 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 2-4 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 30-50 g / 100 mL, and adjusting the pH value to 2-4 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.1-0.2 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.4-1.6:0.5-0.7;
[0009] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8-9, and standing for 6-10 hours to form a gel;
[0010] (3) adding 3-5 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating 1-3 times to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0011] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0012] Furthermore, the free phenol content of the phenolic resin is 10-14% by weight and is purchased from Hebei Zetian Chemical Co., Ltd. with the brand number 2127-1.
[0013] Furthermore, the epoxy resin is a glycidyl ether epoxy resin, with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25° C. It is purchased from Wanqing Chemical Technology Co., Ltd., model NPEL-128.
[0014] Furthermore, the acidic catalyst is hydrochloric acid, nitric acid or acetic acid.
[0015] Further, the third solution is added dropwise to the second solution so that the mass ratio of carbon to silicon is 2-4:1.
[0016] Furthermore, the normal pressure drying is drying at 100-120° C. for 15-20 hours.
[0017] Furthermore, the silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:2-4.
[0018] Furthermore, the medium- and long-chain trialkoxysilane is one or more of propyltriethoxysilane, butyltriethoxysilane, and propyltrimethoxysilane.
[0019] Furthermore, the medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.2-0.5:1.6-1.8.
[0020] The invention provides a silicon oxide composite material for a negative electrode of a lithium ion battery prepared by the preparation method.
[0021] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0022] 1. The present invention uses a specific ratio of carbon source for mixing. The carbon material plays a key conductive role in the composite material, ensuring the rapid transmission of lithium ions in the material. Silicon oxide undergoes significant volume changes during lithiation and delithiation, which may lead to the destruction of the material structure. An appropriate amount of carbon source helps to alleviate this problem. The present invention forms a solid structural framework to support silicon oxide particles to prevent them from breaking or peeling off during charging and discharging. During the first charge and discharge process, a layer of solid electrolyte interface (SEI) film will be formed on the surface of the negative electrode. The appropriate carbon source ratio helps to form a stable and thin SEI film, which is crucial for improving the first charge and discharge efficiency and extending the cycle life of the battery. The carbon source will produce a certain pore structure during the high-temperature carbonization process, which is beneficial for improving the diffusion rate of lithium ions and the power characteristics of the battery. Appropriate porosity can balance the capacity and power performance. Carbon materials not only provide electron conduction paths, but also serve as additional lithium ion storage sites. A specific carbon source ratio can increase the reversible storage capacity of lithium ions in the composite material, thereby increasing the capacity.
[0023] 2. In the process of preparing silicon oxide composite materials for negative electrodes of lithium ion batteries, the selection and proportion of silicon sources have a significant effect on the electrochemical properties of the final composite materials, especially the capacitance. The silicon source of the present invention is a mixture of medium- and long-chain trialkoxysilane and tetraethyl orthosilicate with a mass ratio of 1:2-4. The different proportions of trialkoxysilane and tetraethyl orthosilicate can affect the microstructure of the final composite material. Trialkoxysilane contains longer organic side chains, which helps to form a more open pore structure, while TEOS tends to form a denser network structure. Materials with different structures have different effects on the diffusion capacity, electronic conductivity and mechanical stability of lithium ions, and thus affect the capacitance. The proportion of silicon sources determines the size and aggregation state of the generated silicon oxide particles. Smaller particle size helps to increase the diffusion rate of lithium ions, while moderate aggregation can enhance the mechanical strength of the material. Suitable particle size and aggregation state are crucial to improving capacitance and cycle stability; the amount of silicon source directly affects the content of silicon oxide in the composite material. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] This embodiment provides a method for preparing a silicon oxide composite material for a negative electrode of a lithium ion battery, comprising the following steps:
[0027] (1) dissolving 1 part by mass of a silicon source in 3 parts by mass of anhydrous ethanol, adding 5 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 3 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 40 g / 100 mL, and adjusting the pH value to 3 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.15 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.5:0.6;
[0028] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8.5, and standing for 8 hours to form a gel;
[0029] (3) adding 4 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating twice to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0030] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0031] The free phenol content of the phenolic resin is 10-14% by weight and is purchased from Hebei Zetian Chemical Co., Ltd. with the brand number 2127-1.
[0032] The epoxy resin is a glycidyl ether epoxy resin, with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25° C. It was purchased from Wanqing Chemical Technology Co., Ltd., model NPEL-128.
[0033] The acidic catalyst is 0.1 mol / L hydrochloric acid.
[0034] The third solution was added dropwise to the second solution so that the mass ratio of carbon to silicon was 3:1.
[0035] Normal pressure drying is drying at 110°C for 17 hours.
[0036] The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:3.
[0037] The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.3:1.7.
[0038] Comparative Example 1
[0039] The difference between this comparative example and Example 1 is that the phenolic resin is different.
[0040] A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode comprises the following steps:
[0041] (1) dissolving 1 part by mass of a silicon source in 3 parts by mass of anhydrous ethanol, adding 5 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 3 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 40 g / 100 mL, and adjusting the pH value to 3 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.15 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.5:0.6;
[0042] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8.5, and standing for 8 hours to form a gel;
[0043] (3) adding 4 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating twice to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0044] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0045] Phenolic resin, free phenol content ≤4.5%. Hebei Zetian Chemical Co., Ltd., brand 4123B.
[0046] The epoxy resin is a glycidyl ether epoxy resin, with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25° C. It was purchased from Wanqing Chemical Technology Co., Ltd., model NPEL-128.
[0047] The acidic catalyst is 0.1 mol / L hydrochloric acid.
[0048] The third solution was added dropwise to the second solution so that the mass ratio of carbon to silicon was 3:1.
[0049] Normal pressure drying is drying at 110°C for 17 hours.
[0050] The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:3.
[0051] The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.3:1.7.
[0052] Comparative Example 2
[0053] The difference between this comparative example and Example 1 is that the epoxy resin is different.
[0054] A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode comprises the following steps:
[0055] (1) dissolving 1 part by mass of a silicon source in 3 parts by mass of anhydrous ethanol, adding 5 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 3 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 40 g / 100 mL, and adjusting the pH value to 3 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.15 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.5:0.6;
[0056] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8.5, and standing for 8 hours to form a gel;
[0057] (3) adding 4 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating twice to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0058] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0059] The free phenol content of the phenolic resin is 10-14% by weight and is purchased from Hebei Zetian Chemical Co., Ltd. with the brand number 2127-1.
[0060] The epoxy resin is different. The epoxy resin is a glycidyl ether epoxy resin with an epoxy equivalent of 120-150 g / eq and a viscosity of 7000-10000 cps at 25° C. It was purchased from Nan Ya Epoxy Resin 901.
[0061] The acidic catalyst is 0.1 mol / L hydrochloric acid.
[0062] The third solution was added dropwise to the second solution so that the mass ratio of carbon to silicon was 3:1.
[0063] Normal pressure drying is drying at 110°C for 17 hours.
[0064] The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:3.
[0065] The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.3:1.7.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 1 is that the organic carbon source is a mixture of sucrose, phenolic resin and epoxy resin in a mass ratio of 1:1:1.
[0068] A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode comprises the following steps:
[0069] (1) dissolving 1 part by mass of a silicon source in 3 parts by mass of anhydrous ethanol, adding 5 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 3 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 40 g / 100 mL, and adjusting the pH value to 3 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.15 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1:1;
[0070] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8.5, and standing for 8 hours to form a gel;
[0071] (3) adding 4 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating twice to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0072] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0073] The free phenol content of the phenolic resin is 10-14% by weight and is purchased from Hebei Zetian Chemical Co., Ltd. with the brand number 2127-1.
[0074] The epoxy resin is a glycidyl ether epoxy resin, with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25° C. It was purchased from Wanqing Chemical Technology Co., Ltd., model NPEL-128.
[0075] The acidic catalyst is 0.1 mol / L hydrochloric acid.
[0076] The third solution was added dropwise to the second solution so that the mass ratio of carbon to silicon was 3:1.
[0077] Normal pressure drying is drying at 110°C for 17 hours.
[0078] The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:3.
[0079] The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.3:1.7.
[0080] Comparative Example 4
[0081] The difference between this comparative example and Example 1 is that the silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:1.
[0082] A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode comprises the following steps:
[0083] (1) dissolving 1 part by mass of a silicon source in 3 parts by mass of anhydrous ethanol, adding 5 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 3 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 40 g / 100 mL, and adjusting the pH value to 3 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.15 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.5:0.6;
[0084] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8.5, and standing for 8 hours to form a gel;
[0085] (3) adding 4 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating twice to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0086] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0087] The free phenol content of the phenolic resin is 10-14% by weight and is purchased from Hebei Zetian Chemical Co., Ltd. with the brand number 2127-1.
[0088] The epoxy resin is a glycidyl ether epoxy resin, with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25° C. It was purchased from Wanqing Chemical Technology Co., Ltd., model NPEL-128.
[0089] The acidic catalyst is 0.1 mol / L hydrochloric acid.
[0090] The third solution was added dropwise to the second solution so that the mass ratio of carbon to silicon was 3:1.
[0091] Normal pressure drying is drying at 110°C for 17 hours.
[0092] The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:1.
[0093] The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.3:1.7.
[0094] Comparative Example 5
[0095] The difference between this comparative example and Example 1 is that the medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:1:1.
[0096] A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode comprises the following steps:
[0097] (1) dissolving 1 part by mass of a silicon source in 3 parts by mass of anhydrous ethanol, adding 5 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 3 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 40 g / 100 mL, and adjusting the pH value to 3 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.15 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.5:0.6;
[0098] (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8.5, and standing for 8 hours to form a gel;
[0099] (3) adding 4 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating twice to obtain an aged gel, and drying at normal pressure to obtain a precursor product;
[0100] (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
[0101] The free phenol content of the phenolic resin is 10-14% by weight and is purchased from Hebei Zetian Chemical Co., Ltd. with the brand number 2127-1.
[0102] The epoxy resin is a glycidyl ether epoxy resin, with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25° C. It was purchased from Wanqing Chemical Technology Co., Ltd., model NPEL-128.
[0103] The acidic catalyst is 0.1 mol / L hydrochloric acid.
[0104] The third solution was added dropwise to the second solution so that the mass ratio of carbon to silicon was 3:1.
[0105] Normal pressure drying is drying at 110°C for 17 hours.
[0106] The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:3.
[0107] The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:1:1.
[0108] Performance Testing
[0109] The silicon oxide composite material of the embodiment and the comparative example is used as the negative electrode material of the lithium ion battery, and the mass ratio of the composite material, acetylene black and PVDF is 85:7:8, and N-methylpyrrolidone (NMP) solvent is used to prepare a uniform slurry; the slurry is applied on the copper foil, and it is evenly coated into a film sheet with a scraper, and evenly attached to the surface of the copper foil. The prepared coating is placed in an oven and dried at 110°C for 12 hours; after drying, it is moved into a vacuum drying oven and vacuum dried at 120°C for 10 hours; the dried composite coating is then pressed by a roller machine or a tablet press; the electrode sheet is cut by a mechanical cutting machine, and the lithium sheet is used as the counter electrode. The electrolyte is a commercially available 1mol / L LiPF6 / EC+DMC solution, and the current density is 100mA / g. The battery tester is used to test the charge and discharge performance. The results are shown in Table 1.
[0110] Table 1 Performance test results
[0111]
[0112] It can be seen from the above performance test results that Example 1 has a high specific capacity and good cycle stability, while the comparative example does not adopt the necessary technical solution, resulting in its corresponding performance test being significantly worse than that of the embodiment. The above experimental results further prove the importance of the technical solution defined in the present invention to its technical effect.
[0113] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a silicon oxide composite material for a lithium ion battery negative electrode, characterized in that: The following steps are involved: (1) dissolving 1 part by mass of a silicon source in 2-4 parts by mass of anhydrous ethanol, adding 4-6 parts by mass of deionized water, stirring evenly, dropping an acidic catalyst, and adjusting the pH value to 2-4 to obtain a first solution; dissolving an organic carbon source in anhydrous ethanol, stirring evenly, the concentration of the organic carbon source is 30-50 g / 100 mL, and adjusting the pH value to 2-4 to obtain a second solution; dissolving ammonia water in deionized water, stirring evenly, and controlling the concentration of ammonia water to 0.1-0.2 mol / 100 mL to obtain a third solution; wherein the organic carbon source is a mixture of sucrose, phenolic resin, and epoxy resin in a mass ratio of 1:1.4-1.6:0.5-0.7; (2) adding the third solution dropwise to the second solution, adjusting the pH value to 8-9, and standing for 6-10 hours to form a gel; (3) adding 3-5 times the volume of anhydrous ethanol to the gel for aging, replacing the anhydrous ethanol every 24 hours, repeating 1-3 times to obtain an aged gel, and drying at normal pressure to obtain a precursor product; (4) Under a nitrogen protective atmosphere, the precursor product is heated to 1100° C. and kept at this temperature for 3 h, and then cooled to room temperature along with the furnace to obtain a silicon oxide composite material for a negative electrode of a lithium ion battery.
2. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 1, characterized in that: The free phenol content of the phenolic resin is 10-14% by mass.
3. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 1, characterized in that: The epoxy resin is a glycidyl ether epoxy resin with an epoxy equivalent of 180-190 g / eq and a viscosity of 11000-15000 cps at 25°C.
4. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 1, characterized in that: The acidic catalyst is hydrochloric acid, nitric acid or acetic acid.
5. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 1, characterized in that: The third solution is added dropwise to the second solution so that the mass ratio of carbon to silicon is 2-4:
1.
6. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 1, characterized in that: Normal pressure drying is drying at 100-120℃ for 15-20h.
7. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 1, characterized in that: The silicon source is a mixture of medium- and long-chain trialkoxysilane and ethyl orthosilicate in a mass ratio of 1:2-4.
8. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 7, characterized in that: The medium- and long-chain trialkoxysilane is one or more of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane.
9. The method for preparing the silicon oxide composite material for lithium ion battery negative electrode according to claim 8, characterized in that: The medium- and long-chain trialkoxysilane is a mixture of propyltriethoxysilane, butyltriethoxysilane and propyltrimethoxysilane in a mass ratio of 1:0.2-0.5:1.6-1.
8.
10. A silicon oxide composite material for lithium ion battery negative electrode prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of lithium ion battery silicon oxide / carbon composite negative pole material
CN103236520A
Preparation method of lithium ion battery silicon oxide / carbon composite negative pole material
CN103236534A
Preparation method of composite cathode material SiOx@Si / C for lithium ion battery
CN103996837A
Method for preparing silica / carbon nanometer material with micropores and ordered mesopores
CN107117623A