FAU molecular sieve with high-proportion supercage Na < + > exchange sites and application of FAU molecular sieve to adsorption separation of fluorine-containing electron gas
By adjusting the composition of the organic template agent and synthesizing FAU molecular sieves with a high proportion of supercage Na+ exchange sites using a solid-phase exchange method, the problem of low removal efficiency of R115 impurities in R116 was solved, achieving efficient and low-cost adsorption and separation.
Patent Information
- Application Number
- CN202410971424.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing technologies are insufficient to efficiently remove pentafluorochloroethane (R115) impurities from hexafluoroethane (R116). Traditional methods are energy-intensive, require sophisticated equipment, and have poor thermal stability of the adsorbent. Furthermore, existing molecular sieves have a low proportion of active sites, resulting in limited adsorption capacity.
By adjusting the composition of organic template agents with different charge densities, the cage structure of FAU molecular sieves was directionally assembled and mixed with Na-containing solid salts for solid-phase exchange, directly synthesizing FAU molecular sieves with a high proportion of supercage Na+ exchange sites for adsorption and separation of R115/R116.
It achieves efficient adsorption and separation of R115/R116, avoiding the problems of high energy consumption and high equipment requirements of traditional methods, improving the thermal stability and adsorption capacity of the adsorbent, and reducing manufacturing costs.
Smart Images

Figure CN118908237A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a nanostructured carbon nanotube with a high ratio of super cage Na + The exchanged FAU molecular sieve and its application in the adsorption separation of fluorine-containing electronic gases can efficiently adsorb and separate the impurity gas pentafluoromonochloroethane (R115) from the fluorine-containing electronic gas hexafluoroethane (R116), belonging to the field of gas phase adsorption separation. Background Art
[0002] Fluorinated electronic gases are high-end electronic gas products that play a vital role in semiconductor manufacturing. They are primarily used as cleaning agents, etchants, dopants, and film-forming materials, accounting for approximately 30% of the electronic gas market. With the rapid development of the semiconductor industry in recent years, purity requirements for electronic gases have become increasingly stringent. Even trace impurities as small as one part per million can lead to a rapid increase in the rejection rate of electronic products. R116, with its advantages such as minimal lateral edge erosion, high etching rates, and high precision, addresses the limitations of conventional wet etching methods for high-precision fine line etching of deep submicron integrated circuits (DSIs) measuring 0.18-0.25μm. It can effectively meet the requirements of such narrow linewidth processes. Advanced chip manufacturing processes require purity levels of 6N or higher, making efficient removal of various impurities from industrial-grade R116 crucial. Industrial-grade R116 is primarily derived from the direct fluorination of R115. Industrial products contain a variety of impurities, including fluorine, chlorine, and hydrogen, resulting in a complex impurity profile, with R115 being the primary impurity. Currently, electronic-grade R116 is mainly purified by distillation, and R115-type chlorine-containing impurities are mainly removed by fluorination-coupled distillation.
[0003] Chinese patent CN1169505A reports on utilizing the azeotropic properties of HCl and R116 to produce 99.9999% R116 through azeotropic distillation. However, distillation requires low temperatures and high pressures, resulting in high energy consumption and strict equipment requirements. Furthermore, the fluorination process is highly corrosive, placing high demands on both operation and equipment. Adsorption separation offers significant advantages in the industrial production of electronic-grade R116, with its mild operating conditions, low energy consumption, and high removal depth. Industrial application, however, requires the use of highly efficient adsorbents.
[0004] US Patent No. 6274782B1 discloses a method for Carbonaceous adsorbents or molecular sieves with a silicon-aluminum ratio of less than 1.5 can remove Freon impurities containing 2 carbon atoms in R116, but do not contain R115 impurities. In addition, the thermal stability of carbon material adsorbents and molecular sieves with a low silicon-aluminum ratio is generally poor during the adsorption exothermic process, which is not conducive to continuous use in industrial processes. U.S. Patent US636138B1 uses a critical method to remove non-volatile impurities in R116. The adsorbent is molecular sieve NaX, but it does not achieve efficient adsorption and removal of R115. Zhang Jinke and others from Zhejiang Institute of Chemical Industry used NaX for the adsorption separation of R115 / R116 by taking advantage of the difference in polarity between the two. They found that NaX has a selectivity of 40.9 for C2F5Cl relative to C2F6 at 100kPa, 10°C, and a total flow rate of 25mL·min -1 Under the condition of (R115 / He=450ppm, R116 / He=400ppm), a breakthrough time difference of 30h can be maintained (Journal of Shanghai Jiao Tong University, 2021, 55(9):9). However, its low silicon-aluminum ratio limits the strength of the active sites, making it difficult to form a strong adsorption effect on the adsorbate, and the adsorption capacity is limited. Therefore, it is urgent to develop high-selectivity and stable high-silicon FAU molecular sieve adsorbent materials.
[0005] Zhang Jinke et al. clarified the adsorption separation mechanism by studying the adsorption equilibrium constant, adsorption heat and other parameters of R116 and its key impurity R115 on NaX molecular sieves, and pointed out that the reason affecting the adsorption separation of R115 and R116 in the adsorption separation process of NaX molecular sieves is not the pore size confinement effect of the molecular sieve, but a certain number of active sites and the strength of their active sites (Journal of Advanced Chemical Engineering, 2020, 34(02): 311-317). At the same time, Johannes A. Lercher et al. used ex situ and in situ spectroscopy to study the dynamics of the process from the formation of hydrogel to the FAU zeolite lattice. 23Na MAS NMR confirmed that during the synthesis of X-type zeolites, Na ions were distributed in sodalite cages and supercages at a ratio of 30:70, proving that the lower silicon-aluminum ratio of NaX zeolites limits the strength of active sites, shielding the active sites and resulting in low utilization of active sites (Chemistry of Materials 2018, 30, 3, 888-897). At the same time, zeolites with a higher silicon-aluminum ratio have stronger active site strength. As a type of active site, the proportion of cation exchange sites in high-silicon zeolite supercages is higher than that in NaX zeolites. However, the current method to increase the exposure of active sites is mainly acid-base post-treatment, but the specific surface area and strength will be significantly reduced (Journal of Environmental Health Science and Engineering 2021, 19: 1435-1445); at the same time, the defect sites generated during the dealumination process will cause the proportion of cation exchange sites to decrease. In contrast, the one-time synthesis method avoids the acidification process, which can effectively avoid the problems of specific surface area, strength reduction and defect sites. At the same time, increasing the silicon content of the molecular sieve helps to improve the structural stability. Therefore, it is urgent to develop a new method for regulating the active sites of high-silicon FAU molecular sieves. Our previous patent reported high The acid site ratio of FAU molecular sieve, but it does not involve the Na + Exchange site regulation and electron gas separation applications (CN116514138A)
[0006] In view of the current research on the directional regulation of Na + The synthesis method of the exchange site ratio has not been reported. The present invention adjusts the organic template with different charge density to assemble the different cage structures of FAU molecular sieve, and directly obtains the super cage Na with high ratio by mixing with solid salt containing Na element and solid phase exchange. + The FAU molecular sieve with exchanged positions will eventually be applied to the adsorption separation of fluorine-containing electronic gases, especially the adsorption separation of R115 and R116. Summary of the Invention
[0007] The following will describe in detail the purpose of the invention, implementation points, synthesis process and specific implementation methods of the present invention:
[0008] The purpose of the present invention is to provide a high ratio of super cage Na + The FAU molecular sieve adsorbent with exchange position is used to assemble different cage structures of FAU molecular sieve by adjusting the composition of organic templates with different charge densities, and directly obtains a high proportion of super cage Na by mixing with solid salt containing Na element and solid phase exchange. +The exchanged FAU molecular sieve can achieve effective separation of R115 / R116.
[0009] To achieve the above objectives, the present invention successfully synthesized a high ratio of super cage Na by adjusting the composition of templates with different charge densities and selecting appropriate synthesis conditions. + The FAU molecular sieve with exchange position realizes the effective separation of R115 / R116.
[0010] The technical solution adopted in the present invention is as follows:
[0011] A high ratio of super cage Na + The exchanged-site FAU molecular sieve has a FAU molecular sieve configuration recognized by the International Zeolite Association (IZA). The molar ratio of its chemical composition is Al2O3:mSiO2:nNa2O, and the molar ratio m of the oxide SiO2 / Al2O3 is between 5 and 20. When subjected to X-ray diffraction measurement, it has characteristic peaks within at least the following four crystal plane spacings d: the first crystal plane spacing d=14.4±0.2, the second crystal plane spacing d=8.9±0.2, the third crystal plane spacing d=7.6±0.2, and the fourth crystal plane spacing d=5.8±0.2.
[0012] Furthermore, the one with a high ratio of super cage Na + The FAU molecular sieve of the exchange position is 23 Na MAS NMR determination of Na in FAU molecular sieve supercage + Content accounts for the total Na + The ratio of exchanged bits is 50%-75%, preferably 56-60%.
[0013] The present invention provides a high ratio of super cage Na + The FAU molecular sieve adsorbent with exchange position is used to assemble different cage structures of FAU molecular sieve by adjusting the organic template with different charge density, and then directly obtains a high proportion of super cage Na by mixing with solid salt containing Na element and solid phase exchange. + The exchanged FAU molecular sieve can efficiently adsorb and separate the impurity gas R115 from the fluorine-containing electronic gas R116. The synthesis method is a hydrothermal method, which specifically includes the following steps:
[0014] (a) Al source, Si source, NaCl and organic template are dissolved in deionized water, and then FAU seed crystals are added thereto, stirred evenly, aged to obtain an initial gel, transferred into a pressure-resistant container and sealed, and subjected to a hydrothermal synthesis reaction. Different cage structures of FAU molecular sieves are assembled under the action of organic templates with different charge densities to obtain different Na + Molecular sieve precursor with exchange site ratio;
[0015] (b) filtering, washing, and drying the molecular sieve precursor after the reaction in step (a), and then heating and activating the molecular sieve precursor in a muffle furnace to remove organic matter in the molecular sieve precursor to obtain a calcined matrix;
[0016] (c) mixing the calcined matrix obtained in step (b) with a solid containing a solid salt of the Na element, grinding the mixture in a mortar, and calcining the ground mixture in an argon gas flow to obtain the supercage Na + Exchange position FAU molecular sieve.
[0017] Furthermore, the Al source in step (a) comprises one or more of aluminum alkoxide, aluminum salt, activated alumina, pseudo-boehmite or pseudo-boehmite, preferably aluminum alkoxide, aluminum salt, activated alumina or pseudo-boehmite, more preferably aluminum alkoxide or aluminum salt;
[0018] The Si source comprises one or more of silica sol, silica gel, activated silica or ethyl orthosilicate, preferably silica sol, silica gel or ethyl orthosilicate; the molar ratio of the Si source in the form of SiO2 to the Al source in the form of Al2O3 is 10-20:1, preferably 15-16:1;
[0019] The organic templates include two types, the first template is TEAOH or TPAOH, and the second template is TBAOH or a choline compound. The molar ratio of the first template to the second template is 2-10:1, preferably 5-8:1. The choline compound is at least one of choline hydroxide and choline chloride. The molar ratio of the organic template to the Al source in the form of Al2O3 is 25-52.5:1, preferably 42.5-52.5:1.
[0020] The molar ratio of NaCl to Al source in the form of Al2O3 is 5-10:1, preferably 7.5-8:1;
[0021] The SAR value of the FAU seed crystal is 50-70, preferably 60, and its mass concentration in the initial gel is 10-30 g / L, preferably 17.5-20 g / L, where SAR is the molar ratio of SiO2 to Al2O3;
[0022] The aging time of step (a) is selected to be 12-36h, preferably 20-28h, the temperature of the hydrothermal synthesis reaction is 380-410K, preferably 400-405K, and the reaction time is 30-45h, preferably 35-40h.
[0023] Furthermore, the temperature of the heating activation in step (b) is 500-600° C., and the heating activation time is 2-8 hours.
[0024] Furthermore, the solid salt containing the Na element in step (c) includes sodium chloride, sodium nitrate, sodium carbonate, sodium acetate or disodium ethylenediaminetetraacetate, preferably disodium ethylenediaminetetraacetate; the mass ratio of the Na element compound to the calcined matrix is 2-8:1, preferably 4-6:1.
[0025] Furthermore, in step (c), the heating temperature is 450-550° C., and the heating time is 10-15 h.
[0026] The present invention also provides a high ratio of super cage Na + Application of exchanged FAU molecular sieves in the adsorption and separation of fluorine-containing electronic gases in gas phase systems.
[0027] Furthermore, the molecular sieve of the present invention is used for the adsorption separation of pentafluoromonochloroethane R115 and hexafluoroethane R116, and the FAU molecular sieve adsorption separation gas is operated at 273-323K, preferably 293-303K.
[0028] The beneficial effects achieved by the present invention are:
[0029] (1) The FAU molecular sieve synthesis in the present invention uses templates with different charge densities, and the prepared product has a high proportion of super cage Na + The exchange site can avoid the problem of low proportion of effective active sites in traditional one-time synthesis Y molecular sieve and improve the adsorption efficiency of the molecular sieve. At the same time, compared with commercial Y molecular sieve, it effectively avoids the specific surface area, strength reduction and defects caused by acid treatment, so as to avoid the decline of adsorption activity and regeneration performance, as well as coking and carbon deposition during the activation treatment.
[0030] (2) The FAU molecular sieve of the present invention has a relatively high silicon-aluminum ratio, and the Na + The dosage is small, while the cost of Li and Ag currently used for ion exchange is high and the dosage is large, so the use of the Na-FAU molecular sieve with the best performance in the present invention is conducive to reducing the manufacturing cost of the molecular sieve.
[0031] (3) The FAU molecular sieve in the present invention has a high silicon-aluminum ratio, low polarity, and strong hydrophobicity, which can avoid the high powder loss rate in the adsorbent manufacturing.
[0032] (4) The present invention can directly prepare an all-Na type FAU molecular sieve, and secondly, the exposure of the Na site can be adjusted. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the adsorption separation test curve of NaY-2.6 molecular sieve for R115 / R116 system;
[0034] Figure 2It is the adsorption separation measurement curve of NaY-3.3 molecular sieve for the R115 / R116 system;
[0035] Figure 3 It is the adsorption separation measurement curve of NaY-5.0 molecular sieve for the R115 / R116 system;
[0036] Figure 4 It is the adsorption separation measurement curve of NaY-5.6 molecular sieve for the R115 / R116 system;
[0037] Figure 5 It is the adsorption separation measurement curve of NaY-8.0 molecular sieve for the R115 / R116 system;
[0038] Figure 6 It is a schematic diagram of the XRD test results of different molecular sieve adsorbents;
[0039] Figure 7 It is the sodium ion distribution diagram of different molecular sieves. Specific implementation mode
[0040] The present invention will be described in detail below through examples, but the present invention is not limited to these examples.
[0041]
Instrument characterization
[0042] <X-ray diffraction measurement>
[0043] The X-ray diffraction measurement instrument is Panalytical X’Pert PRO, the detection light source is Cu Kα, the tube voltage is 40 kV, the tube current is 40 mA, the detection angle range is 5-50°, and the detection time is 10 min. The present invention determines the phase structure of the synthesized molecular sieve by X-ray diffraction. The milled sample powder is added into the square hole on the glass plate, and then the glass plate is inserted into the axis position of the goniometer. Under the irradiation of the Cu Kα light source, the probe rotates at a speed of 2θ / min. In addition, the light source is not limited to CuKα, and Co Kα, Mo Kα, and Ag Kα can also be used as the light source for phase analysis. The raw material form for testing can be powder, emulsion or solid particles.
[0044] <Inductively coupled plasma spectroscopy measurement>
[0045] Inductively coupled plasma spectroscopy (ICP) measurement is carried out using PerkinElmer Optima8x00. The present invention determines the contents of the tetravalent element Si, the trivalent element Al, and the monovalent element or monovalent cation Na in the synthesized molecular sieve by inductively coupled plasma spectroscopy. The standard sample is diluted to make a concentration gradient absorption curve. The sample is dissolved with hydrofluoric acid and then diluted with water, and then the concentration of each element in the sample is determined by measuring the absorption peak intensity.
[0046] <NMR measurement of molecular sieve>
[0047] Adopt 23 Na nuclear magnetic resonance ( 23 NaMAS NMR) was used to measure the proportion of the Na exchange sites in the supercages of FAU molecular sieve among the total Na exchange sites. The sample was heated to 400 °C (at a rate of 5 °C / min) and held at this temperature for 10 h to achieve dehydration. Experiments were carried out at different magnetic field strengths. A Bruker 500 MHz spectrometer equipped with a triple resonance wide-bore probe was used. The resonance frequency was set at 132.3 MHz, and the sample was rotated at 10 kHz. The π / 20 pulse corresponded to a pulse width of 1.4 μs. Scans were accumulated 5000 times at a rotation speed of 16 kHz, and the pulse delay was 1 s. The signal reference was set to 0 ppm with respect to solid NaCl.
[0048] <R115 / R116 adsorption separation measurement>
[0049] In this invention, the gas adsorption capacity was tested by gas adsorption measurement. R115 / R116 was measured at 298 K. Approximately 190 mg of the sample was placed in a U-shaped tube, and then a mixed gas with a total gas flow rate of 90 mL / min and a concentration ratio of R115 / R116 / He of 1:9:90 was passed through. The tail gas after the sample adsorption was introduced into a gas chromatograph for detection. All samples were calcined at 400 - 600 °C for more than 6 h before adsorption.
[0050] In the actual gas adsorption measurement, the calculation formula for the R115 / R116 adsorption selectivity is
[0051]
[0052] Here, S represents selectivity, q represents the saturated adsorption capacity of the molecular sieve for different gases (mmol g -1 ), and p represents the partial pressure of a specific gas in the mixed gas (kPa).
[0053]
Example
[0054] The FAU seed crystals (SAR = 60) in the examples of this invention were purchased from Tianjin Nanhua Catalyst Co., Ltd., model NKF-3. ChOH is choline hydroxide, and ChCl is choline chloride.
[0055] Example 1
[0056] Aluminum sec-butoxide, TEAOH, ethyl orthosilicate, ChOH, ChCl, and NaCl were dissolved in deionized water according to the molar ratio of 1.5NaCl: 0.2Al2O3 (the amount of aluminum sec-butoxide is calculated in the form of Al2O3): 8SiO2 (the amount of ethyl orthosilicate is calculated in the form of SiO2): 8TEAOH: 0.5ChOH: 2ChCl, wherein the molar concentration of aluminum sec-butoxide in deionized water is determined to be 0.14 mol / L, and FAU seeds with a final concentration of 17.8 g / L were added thereto, and aged for 24 hours to obtain an initial gel. The gel mixture was transferred into a pressure-resistant container, sealed, and reacted at 403K for 36 hours. After the hydrothermal reaction was completed, the reaction solution was cooled, filtered, and washed to obtain a crystalline product. The obtained crystals were dried at 373K for 12 hours to obtain a powdery product, i.e., a catalyst precursor.
[0057] The resulting powdered product (catalyst precursor) was calcined at 550°C in a muffle furnace for 6 hours, then cooled to room temperature. One gram of the calcined product was ground and mixed with 5g of disodium ethylenediaminetetraacetic acid for 1 hour. After grinding, the product was heated to 500°C (at a heating rate of 2°C / min) in an argon flow (25 mL / min) and maintained at 500°C for 12 hours. After the reaction, the product was cooled in an argon flow. The resulting powdered molecular sieve was named NaY-3.3.
[0058] The obtained product NaY-3.3 was analyzed by XRD. The interplanar spacing of the characteristic peaks in NaY-3.3 is shown in Table 1. The schematic diagram of the XRD test results is shown in Figure 6 , indicating that the synthesized molecular sieve has the FAU molecular sieve configuration recognized by IZA. The elemental composition analysis of the above sample by ICP showed that the SAR value of NaY-3.3 is 6.6. SAR is the molar ratio of SiO2 to Al2O3.
[0059] Table 1 Characteristic interplanar spacing of NaY-3.3
[0060] Interplanar spacing (d) 1 14.250 2 8.746 3 7.458 4 5.660 5 4.897 6 4.755 7 4.366 8 3.759
[0061] Example 2
[0062] Example 2 Preparation Method of Molecular Sieve Repeat Example 1, except that "the molar ratio of all raw materials is replaced by 1.5NaCl:0.2Al2O3 (the feeding amount of aluminum sec-butoxide is calculated in the form of Al2O3):8SiO2 (the feeding amount of tetraethyl orthosilicate is calculated in the form of SiO2):8TEAOH:1.0TBAOH, and aluminum sec-butoxide, TEAOH, TBAOH, tetraethyl orthosilicate and NaCl are dissolved in deionized water, wherein the molar concentration of aluminum sec-butoxide in deionized water is determined to be 0.14 mol / L unchanged", and other conditions remain unchanged. The final powdered product molecular sieve is named NaY-5.0.
[0063] The obtained product NaY-5.0 was analyzed by XRD. The interplanar spacing of the characteristic peaks of NaY-5.0 is shown in Table 2. The schematic diagram of the XRD test results is shown in Figure 6 , indicating that the synthesized molecular sieve has the FAU molecular sieve configuration recognized by IZA. The elemental composition of the above samples was analyzed by ICP, and the analysis results showed that the SAR value of NaY-5.0 was 10.0.
[0064] Table 2 Characteristic interplanar spacing of NaY-5.0
[0065] Interplanar spacing (d) 1 14.264 2 8.717 3 7.387 4 5.682 5 4.751 6 4.152 7 3.893 8 3.762
[0066] Example 3
[0067] Example 3 Preparation Method of Molecular Sieve Repeat Example 1, except that "the molar ratio of all raw materials is replaced by 1.5NaCl:0.2Al2O3 (the feeding amount of aluminum sec-butoxide is calculated in the form of Al2O3):8SiO2 (the feeding amount of tetraethyl orthosilicate is calculated in the form of SiO2):6TPAOH:2.5ChCl, and aluminum sec-butoxide, TPAOH, tetraethyl orthosilicate, ChCl, and NaCl are dissolved in deionized water, wherein the molar concentration of aluminum sec-butoxide in deionized water is determined to be 0.14 mol / L unchanged", and other conditions remain unchanged. The final powdered product molecular sieve is named NaY-5.6.
[0068] The obtained product NaY-5.6 was analyzed by XRD. The interplanar spacing of the characteristic peaks of NaY-5.6 is shown in Table 3. The schematic diagram of the XRD test results is shown in Figure 6 , indicating that the synthesized molecular sieve has the FAU molecular sieve configuration recognized by IZA. The elemental composition of the above sample was analyzed by ICP, and the analysis results showed that the SAR value of NaY-5.6 was 11.2.
[0069] Table 3 Characteristic interplanar spacing of NaY-5.6
[0070] Interplanar spacing (d) 1 14.274 2 8.773 3 7.492 4 5.688 5 4.762 6 4.380 7 3.915 8 3.774
[0071] Example 4
[0072] Example 4 Preparation Method of Molecular Sieve Repeat Example 1, except that "the molar ratio of all raw materials is replaced by 1.5NaCl:0.2Al2O3 (the feeding amount of aluminum sec-butoxide is calculated in the form of Al2O3):8SiO2 (the feeding amount of tetraethyl orthosilicate is calculated in the form of SiO2):8TBAOH, and aluminum sec-butoxide, TBAOH, tetraethyl orthosilicate, and NaCl are dissolved in deionized water, wherein the molar concentration of aluminum sec-butoxide in deionized water is determined to be 0.14 mol / L unchanged", and other conditions remain unchanged. The final powdered product molecular sieve is named NaY-8.0.
[0073] The obtained product NaY-8.0 was analyzed by XRD. The interplanar spacing of the characteristic peaks of NaY-8.0 is shown in Table 4. The schematic diagram of the XRD test results is shown in Figure 6 , indicating that the synthesized molecular sieve has the FAU molecular sieve configuration recognized by IZA. The elemental composition analysis of the above sample by ICP showed that the SAR value of NaY-8.0 was 16.0.
[0074] Table 4 Characteristic interplanar spacing of NaY-8.0
[0075] Interplanar spacing (d) 1 14.345 2 8.817 3 7.529 4 5.716 5 4.786 6 4.380 7 3.933 8 3.793
[0076] Comparative Example 1
[0077] To prepare commercial USY-2.6 molecular sieve, 1g was ground with 5g of disodium ethylenediaminetetraacetic acid for 1 hour. After grinding, the mixture was heated to 500°C (at a heating rate of 2°C / min) under an argon flow (25mL / min) and maintained at 500°C for 12 hours. After the reaction, the mixture was cooled under an argon flow. The resulting powdered product was designated NaY-2.6.
[0078] The ratio of supercage Na cation exchange sites to total Na cation exchange sites in different molecular sieves of Examples 1-4 and Comparative Example 1 was determined. The specific process was as follows: the sample was heated to 400°C at a heating rate of 5°C / min and kept at this temperature for 10 hours to achieve dehydration. The experiment was carried out under different field strengths. A Bruker 500MHz spectrometer was used, equipped with a triple-resonance wide-aperture probe. The resonant frequency was set to 132.3MHz, and the sample was rotated at 10kHz. The π / 20 pulse corresponds to a pulse width of 1.4μs. A cumulative scan was performed 5000 times at a rotation speed of 16khz, with a pulse delay of 1s. The signal reference solid NaCl was set to 0ppm. The ratio of supercage Na cation exchange sites to total Na cation exchange sites of different molecular sieves is, for example Figure 3 As shown in Table 5.
[0079] Determination of the adsorption performance of different molecular sieves in Examples 1-4 and Comparative Example 1: The samples were calcined at 500°C for more than 6 hours before adsorption, and then cooled to room temperature before being used to test the adsorption performance. A molecular sieve of about 190 mg was placed in a U-shaped tube, and then a mixed gas with a total gas flow rate of 90 mL / min and a R115 / R116 / He volume concentration ratio of 1:9:90 was introduced. The tail gas after sample adsorption was passed through a gas chromatograph for detection. The adsorption separation determination curves of different molecular sieves for the R115 / R116 system are shown in FIG. Figure 1-5 As shown in Table 5, the adsorption capacity of different molecular sieves for R115 and the adsorption selectivity of R115 / R116 are shown.
[0080] Table 5 Adsorption capacity of molecular sieve adsorbent material R115, R115 / R116 selectivity and Na in super cage + Proportion
[0081]
[0082] As can be seen from Table 5, the FAU molecular sieve synthesis uses templates with different charge densities. Compared with commercial FAU molecular sieves, the molecular sieve products prepared by the present invention have a high proportion of supercage Na + Exchange position (i.e., super cage Na in molecular sieve + Exchange position accounts for the total Na + The exchange site ratio is relatively high), which can avoid the problem of low effective active site ratio of traditional high-silicon Y molecular sieve synthesized in one step, and improve the adsorption capacity of molecular sieve for R115 and the adsorption selectivity of R115 / R116. + 4(SC) ratio is the ratio of super cage Na in molecular sieve + Exchange position accounts for the total Na + Swap bit ratio.
[0083] Determination of the curve by adsorption separation Figure 1-5 It can be seen that the adsorption curve of R115 / R116 shows that the larger the closed area surrounded by the two lines, the better the separation effect of the adsorbent material for the two. Corresponding to Table 5, it can be expressed as the specific numerical values of the molecular sieve adsorbent for R115 adsorption capacity and R115 / R116 selectivity. Therefore, it can be found that the high-silicon FAU molecular sieve prepared with TEA and TBA co-templates and TPA and Ch co-templates has a better effect in the adsorption separation of the R115 / R116 system because it has a higher proportion of supercage cation exchange sites. The high-silicon FAU molecular sieve using TBA single template also has a good effect on the adsorption separation of the R115 / R116 system.
[0084] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be considered as being limited to the specific forms described in the embodiments.
Claims
1. A high proportion of super cage Na + The exchanged FAU molecular sieve has the FAU molecular sieve configuration recognized by the International Molecular Sieve Association IZA, and its chemical composition molar ratio is Al2O3:mSiO2:nNa2O, the molar ratio m of the oxide SiO2 / Al2O3 is 5-20, and when subjected to X-ray diffraction measurement, it has characteristic peaks within at least the following four crystal plane spacings d: the first crystal plane spacing d=14.4±0.2, the second crystal plane spacing d=8.9±0.2, the third crystal plane spacing d=7.6±0.2, and the fourth crystal plane spacing d=5.8±0.
2.
2. A method as claimed in claim 1 having a high proportion of super cage Na + The FAU molecular sieve of the exchange position is characterized by go through 23 NaMAS NMR determination of Na in FAU molecular sieve supercage + Content accounts for the total Na + The ratio of exchange positions is 50%-75%, preferably 56-60%.
3. A kind of high ratio super cage Na as claimed in claim 1 + A method for preparing a FAU molecular sieve having an exchange position, characterized in that The process includes: (a) Al source, Si source, NaCl and organic template are dissolved in deionized water, and then FAU seed crystals are added thereto, stirred evenly, aged to obtain an initial gel, transferred into a pressure-resistant container and sealed, and subjected to a hydrothermal synthesis reaction to assemble different cage structures of FAU molecular sieves under the action of organic templates with different charge densities to obtain FAU molecular sieves with different Na + Molecular sieve precursor with exchange site ratio; (b) filtering, washing, and drying the molecular sieve precursor after the reaction in step (a), and then heating and activating the molecular sieve precursor in a muffle furnace to remove organic matter in the molecular sieve precursor to obtain a calcined matrix; (c) mixing the calcined matrix obtained in step (b) with a solid salt containing the Na element, grinding the mixture in a mortar, and calcining the ground mixture in an argon gas flow for solid phase exchange, thereby obtaining the supercage Na + Exchange position of FAU molecular sieve.
4. A method as claimed in claim 1 having a high proportion of super cage Na + A method for preparing a FAU molecular sieve having an exchange position, characterized in that The Al source in step (a) comprises one or more of alkoxy aluminum, aluminum salt, activated alumina, pseudo-boehmite or pseudo-boehmite, preferably alkoxy aluminum, aluminum salt, activated alumina or pseudo-boehmite, more preferably alkoxy aluminum or aluminum salt; The Si source includes one or more of silica sol, silica gel, active silica or tetraethyl orthosilicate, preferably silica sol, silica gel or tetraethyl orthosilicate; the molar ratio of the Si source in the form of SiO2 to the Al source in the form of Al2O3 is 10-20:1, preferably 15-16:1; The organic template comprises two types, the first template is TEAOH or TPAOH, the second template is TBAOH or a choline compound, the molar ratio of the first template to the second template is 2-10:1, preferably 5-8:1, the choline compound is at least one of choline hydroxide and choline chloride; the molar ratio of the organic template to the Al source in the form of Al2O3 is 25-52.5:1, preferably 42.5-52.5:1; The molar ratio of the NaCl to the Al source in the form of Al2O3 is 5-10:1, preferably 7.5-8:1; The SAR value of the FAU seed crystal is 50-70, preferably 60, and its mass concentration in the initial gel is 10-30 g / L, preferably 17.5-20 g / L, SAR is the molar ratio of SiO2 to Al2O3; The aging time of step (a) is 12-36h, preferably 20-28h, the temperature of the hydrothermal synthesis reaction is 380-410K, preferably 400-405K, and the reaction time is 30-45h, preferably 35-40h.
5. A method as claimed in claim 1 having a high proportion of super cage Na + A method for preparing a FAU molecular sieve having an exchange position, characterized in that The temperature of heating activation in step (b) is 500-600° C., and the heating activation time is 2-8 hours.
6. A method as claimed in claim 1 having a high proportion of super cage Na + A method for preparing a FAU molecular sieve having an exchange position, characterized in that The solid salt containing the Na element in step (c) includes sodium chloride, sodium nitrate, sodium carbonate, sodium acetate or disodium ethylenediaminetetraacetate, preferably disodium ethylenediaminetetraacetate; the mass ratio of the solid salt containing the Na element to the calcined matrix is 2-8:1, preferably 4-6:
1.
7. A method as claimed in claim 1 having a high proportion of super cage Na + A method for preparing a FAU molecular sieve having an exchange position, characterized in that In step (c), the heating temperature is 450-550° C. and the heating time is 10-15 h.
8. A method as claimed in claim 1 having a high proportion of super cage Na + Application of exchanged FAU molecular sieves in the adsorption and separation of fluorine-containing electronic gases in gas phase systems.
9. The use according to claim 8, characterized in that The molecular sieve is used for the adsorption separation of pentafluoromonochloroethane R115 and hexafluoroethane R116. The FAU molecular sieve adsorption separation gas is operated at 273-323K, preferably 293-303K.
Citation Information
Patent Citations
High-silicon FAU molecular sieve with high-proportion exposed acid site as well as preparation method and application of high-silicon FAU molecular sieve
CN116514138A
Exhaust gas heating system for in-cylinder injection internal combustion engine
CN1169505A
Method for purifying hexafluoroethane
US6274782B1
Method for preparing high-performance molecular sieve membrane through ion exchange at melting state
CN103894076A
Ultra-high purity hexafluoroethane preparation method
CN103910599A