Preparation method and application of spheroidic pseudo-boehmite cluster particles
By reacting sodium metaaluminate and nitric acid under mild conditions, the spherical quasi-thin aluminite cluster particles are solved, and the problems of high raw material costs and strict reaction conditions in the existing technology are achieved, and the efficient adsorption of Congo red is achieved. The effect is that the adsorption amount reaches 1757-2353 mg/g, and the reaction conditions are mild and the raw materials are cheap.
Patent Information
- Application Number
- CN202411082817.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to prepare phthalthy aluminite particles with excellent adsorption performance under mild conditions, and the reaction conditions are strict, which affects its application efficiency when treating high-concentration Congo red wastewater.
By heating the sodium metaaluminate solution and adding nitric acid solution, centrifugation, washing and drying, spherical phthalite cluster particles assembled from nanosheets were prepared, using mild conditions and cheap raw materials. Achieve efficient adsorption of Congo red.
The adsorption amount of Congo red by this method exceeds 1000mg/g within 10 minutes, and the adsorption amount can reach 1757-2353mg/g in 48 hours. The reaction conditions are mild, the raw materials are cheap, and the yield is high, which solves the high raw materials cost and strict reaction conditions. A harsh problem.
Smart Images

Figure CN118908258A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic non-metallic functional materials, and in particular relates to a preparation method of spherical pseudo-boehmite cluster particles and application thereof. Background Art
[0002] Congo red is an azo dye that is widely used in the textile industry. Statistics show [POOladoye, MOBamigboye, ODOgunbiyi, MTAkano. Toxicity and decontamination strategies of Congo red dye [J]. Groundwater for Sustainable Development, 2022, 19: 100844] that the annual global production of various dyes is about 108 tons, of which azo dyes such as Congo red account for 60-70%. In the production process of textiles, the dyeing process will produce a large amount of wastewater containing Congo red; in addition, Congo red is also used in acid-base analysis, optoelectronics and medicine, and these processes will also produce wastewater containing Congo red. Some scholars have evaluated the impact of Congo red wastewater on the environment. The study showed that Congo red can affect the growth and metabolic activities of photosynthetic organisms in the aquatic environment. Many aquatic animals at the bottom of the food chain feed on it and rely on the oxygen produced by it in the water. Therefore, the growth of photosynthetic organisms is hindered, which will affect the entire aquatic environment ecosystem [M. Hernández-Zamora, HVPerales-Vela, CMFlores-Ortíz, RO Physiological and biochemical responses of Chlorella vulgaris to Congo red [J]. Ecotoxicology and Environmental Safety, 2014, 108: 72-7]. In addition, the survival and reproductive rates of Daphnia pulex directly exposed to water bodies with sublethal concentrations of Congo red or consuming algae enriched with Congo red were significantly reduced [M. Hernández-Zamora, F. Martínez-Jerónimo, E. Cristiani-Urbina, RO Congo red dye affects survival and reproduction in the cladoceran Ceriodaphnia dubia. Effects of direct and dietary exposure [J]. Ecotoxicology, 2016, 25: 1832-1840], which shows that Congo red has potential risks to aquatic plants and animals, so it is necessary to detoxify wastewater containing Congo red. There are currently a variety of technical means for the treatment of Congo red wastewater, including membrane separation, biodegradation, coagulation and adsorption. Among them, adsorption is recognized as one of the feasible methods because of its simple operation and high cost-effectiveness [Y. Zheng, B. Cheng, J. Fan, J. Yu, W. Ho. Review on nickel-based adsorption materials for Congo red [J]. Journal of Hazardous Materials, 2021, 403: 123559], especially when treating large amounts of high-concentration wastewater. Therefore, it is of practical significance to develop a low-cost Congo red adsorbent with excellent adsorption performance.
[0003] Pseudoboehmite is often used as an adsorbent and can also be used in the field of Congo red adsorption. Li et al. [K.Li, G.Yuan, L.Dong, G.Deng, H.Duan, Q.Jia, H.Zhang, S.Zhang.Boehmite aerogel with ultrahigh adsorption capacity for Congo Red removal: Preparation and adsorption mechanism [J]. Separation and Purification Technology, 2022, 302: 122065] used aluminum isopropoxide as the aluminum source, adopted the sol-gel method and combined it with freeze-drying process to prepare pseudoboehmite aerogel, which has an adsorption capacity of 1761 mg / g for Congo red and an adsorption removal rate of 70.4%. Zhou et al. [J.Zhou, W.Cai, Z.Yang, Q.Xia, J.Chen, J.Fan, C.Du.N,N-dimethylformamide assisted facile hydrothermal synthesis of boehmite microspheres for highly effective removal of Congo red from water[J].Journal of Colloid and Interface Science, 2021, 583:128-38] used aluminum sulfate as the aluminum source and prepared pseudo-boehmite hollow microsphere particles by a high-temperature hydrothermal method. The adsorption capacity of Congo red reached 847.5 mg / g and the adsorption removal rate was 84.8%. Li et al. [Z.Li, L.He, W.Tian, R.Huang, X.Wang, D.Li, P.Tang, Y.Feng. Batch and fixed-bed adsorption behavior of porous boehmite with high percentage of exposed(020)facets and surface area towards Congo red[J]. Inorganic Chemistry Frontiers, 2021, 8(3): 735-45] used aluminum nitrate as the aluminum source, prepared pseudo-boehmite powder by a high-temperature hydrothermal method and formed it with sodium alginate. The adsorption capacity of pseudo-boehmite for Congo red reached 1298.3 mg / g, and the adsorption removal rate was 86.6%.
[0004] The pseudo-boehmite prepared by the above method has a high adsorption capacity for Congo red, but there are problems such as high raw material cost or harsh reaction conditions. So far, there is no report on the preparation of pseudo-boehmite particles with excellent adsorption performance using low-cost raw materials under mild conditions. Summary of the invention
[0005] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing spherical pseudo-boehmite cluster particles.
[0006] The invention provides a method for preparing spherical pseudo-boehmite cluster particles with cheap raw materials and mild reaction conditions. The particles are assembled by interweaving a large number of nanosheets and have faster adsorption kinetics and higher adsorption capacity for azo dye Congo red.
[0007] Another object of the present invention is to provide an application of the above-mentioned spherical pseudo-boehmite cluster particles.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing spherical pseudo-boehmite cluster particles comprises the following steps:
[0010] (1) heating the sodium aluminate solution to 30-60° C. and then adding nitric acid solution to react;
[0011] (2) After the addition of the nitric acid solution in step (1) is completed, the slurry product is centrifuged, and the filter cake is washed and dried to obtain the pseudo-boehmite product.
[0012] Preferably, in step (1), the concentration of the sodium aluminate solution is 0.1-1 mol / L, and the concentration of the nitric acid solution is 0.1-1 mol / L; the volume ratio of the sodium aluminate solution to the nitric acid solution is 1:1, and the concentrations are the same.
[0013] In some preferred embodiments, the concentration of the sodium aluminate solution in step (1) is selected from 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.7 mol / L or 1.0 mol / L.
[0014] In some preferred embodiments, the concentration of the nitric acid solution in step (1) is selected from 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.7 mol / L or 1.0 mol / L.
[0015] Preferably, the reaction temperature in step (1) is 30-60°C.
[0016] Preferably, the addition rate of the nitric acid solution in step (1) is 0.5-5 mL / min.
[0017] Preferably, in step (2), the washing is performed sequentially with water and anhydrous ethanol; further preferably, the washing is performed sequentially with water twice and then with anhydrous ethanol twice.
[0018] Preferably, the drying in step (2) refers to drying at 60° C. for 12 hours.
[0019] In the method for preparing the spherical pseudo-boehmite cluster particles, the reaction solution and the water used for washing are both deionized water.
[0020] The spherical pseudo-boehmite cluster particles of the present invention are prepared by the above-mentioned preparation method and are assembled from a large number of interwoven nanosheets.
[0021] The particle size of the spherical pseudo-boehmite particles is about 50-200 nm.
[0022] The present invention also provides the use of the spherical pseudo-boehmite cluster particles in absorbing Congo red dye in water.
[0023] Preferably, the application is to put the spherical pseudo-boehmite cluster particles into water containing Congo red dye for adsorption treatment.
[0024] Preferably, in this application, the adsorption treatment time is 1 min-48 h.
[0025] Preferably, in this application, the amount of spherical pseudo-boehmite cluster particles is 20 mg, and the concentration and amount of Congo red solution are 500 mg / L and 100 mL, respectively.
[0026] The preparation method of the spherical pseudo-boehmite cluster particles of the present invention is simple, the reaction conditions are mild, and the adsorption performance of the azo dye Congo red is excellent. Specifically, compared with the prior art, the advantages of the present invention are as follows:
[0027] (1) The reaction raw materials are relatively cheap sodium aluminate and nitric acid, and the reaction is carried out under mild conditions at normal pressure and 30-60°C. The preparation can be carried out under conditions of higher raw material concentrations, with a yield of more than 86% (based on the pseudo-boehmite chemical formula AlOOH), wherein the yields of pseudo-boehmite in Examples 1-6 are 86%, 86%, 85%, 86%, 88% and 88%, respectively; and no aging is required after the addition of nitric acid.
[0028] (2) The prepared spherical pseudo-boehmite cluster particles exhibited faster adsorption kinetics and higher adsorption capacity for Congo red dye. The adsorption capacity of Congo red exceeded 1000 mg / g within 10 min, and the adsorption capacity could reach 1757-2353 mg / g after 48 h. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is the XRD spectrum of the pseudo-boehmite prepared in each embodiment;
[0030] Figure 2 This is a SEM image of the pseudo-boehmite prepared in Example 1;
[0031] Figure 3 This is a SEM image of pseudo-boehmite prepared in Example 2;
[0032] Figure 4 This is a SEM image of pseudo-boehmite prepared in Example 3;
[0033] Figure 5 This is a SEM image of pseudo-boehmite prepared in Example 4;
[0034] Figure 6 This is a SEM image of pseudo-boehmite prepared in Example 5;
[0035] Figure 7 This is a SEM image of pseudo-boehmite prepared in Example 6;
[0036] Figure 8 It is the fitting curve diagram of the pseudo-second-order adsorption kinetics of each embodiment. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. The raw materials involved in the present invention can be purchased directly from the market. For process parameters not particularly noted, conventional techniques can be used.
[0038] Example 1
[0039] A method for preparing spherical pseudo-boehmite cluster particles is carried out according to the following steps:
[0040] (1) Sodium aluminate is dissolved in deionized water to prepare a 50 mL, 0.1 mol / L solution, which is then placed in an oil bath and heated to 53° C.; concentrated nitric acid is diluted to prepare a 50 mL, 0.1 mol / L nitric acid solution, and the nitric acid solution is added to the stirred sodium aluminate solution at a flow rate of 2 mL / min using a peristaltic pump.
[0041] (2) After the addition of the nitric acid solution, the reaction slurry was centrifuged, washed, and dried to obtain the product. The product was washed twice with deionized water and then twice with anhydrous ethanol. The drying temperature was 60°C and the drying time was 12 hours. The XRD spectrum of the product is shown in Figure 1 , indicating that the product prepared in this example is pseudo-boehmite; the SEM photo of the product is shown in Figure 2 As shown, its morphology is a cluster particle composed of nano-spherical particles assembled from nano-flakes and with a particle size of about 100-200nm.
[0042] (3) Congo red static adsorption experiment: 20 mg of the sample prepared in this example was dispersed in 100 mL of a 500 mg / L Congo red solution under stirring at room temperature. According to the experimental requirements, about 4 mL of the suspension was measured with a 5 mL syringe after different time periods, filtered through a filter membrane with a pore size of 0.45 μm, and the Congo red content in the filtrate was analyzed using a TU-1901 double beam UV-visible spectrophotometer. The adsorption of Congo red by the sample at different time periods is shown in Table 1. Among them, the adsorption of Congo red was measured to be 1312 mg / g at 10 min of adsorption, and the adsorption was 2107 mg / g at 48 h of adsorption.
[0043] Example 2
[0044] A method for preparing spherical pseudo-boehmite cluster particles is carried out according to the following steps:
[0045] (1) Sodium aluminate is dissolved in deionized water to prepare a 50 mL, 0.3 mol / L solution, which is then placed in an oil bath and heated to 60° C. Concentrated nitric acid is diluted to prepare a 50 mL, 0.3 mol / L nitric acid solution, which is then added to the stirred sodium aluminate solution at a flow rate of 5 mL / min using a peristaltic pump.
[0046] (2) After the addition of the nitric acid solution, the reaction slurry was centrifuged, washed, and dried to obtain the product. The product was washed twice with deionized water and then twice with anhydrous ethanol. The drying temperature was 60°C and the drying time was 12 hours. The XRD spectrum of the product is shown in Figure 1 , indicating that the product prepared in this example is pseudo-boehmite; the SEM photo of the product is shown in Figure 3 As shown, its morphology is a cluster particle composed of nano-spherical particles with a particle size of about 100-200nm assembled from nano-flakes.
[0047] (3) The sample of this example was subjected to a Congo red static adsorption experiment under the adsorption conditions described in Example 1, and the amount of Congo red adsorbed by the sample at different times is shown in Table 1. Among them, the amount of Congo red adsorbed by the sample at 10 min of adsorption was 1260 mg / g, and the amount of Congo red adsorbed at 48 h of adsorption was 1770 mg / g.
[0048] Example 3
[0049] A method for preparing spherical pseudo-boehmite cluster particles is carried out according to the following steps:
[0050] (1) Sodium aluminate is dissolved in deionized water to prepare a 50 mL, 0.5 mol / L solution, which is then placed in an oil bath and heated to 30° C. Concentrated nitric acid is diluted to prepare a 50 mL, 0.5 mol / L nitric acid solution, which is then added to the stirred sodium aluminate solution at a flow rate of 0.5 mL / min using a peristaltic pump.
[0051] (2) After the addition of the nitric acid solution, the reaction slurry was centrifuged, washed, and dried to obtain the product. The product was washed twice with deionized water and then twice with anhydrous ethanol. The drying temperature was 60°C and the drying time was 12 hours. The XRD spectrum of the product is shown in Figure 1 , indicating that the product prepared in this example is pseudo-boehmite; the SEM photo of the product is shown in Figure 4 As shown, its morphology is a cluster particle composed of nano-spherical particles with a particle size of about 50-150nm assembled from nano-flakes.
[0052] (3) The sample of this example was subjected to a Congo red static adsorption experiment under the adsorption conditions described in Example 1. The adsorption amount of Congo red by the sample at different times is shown in Table 1. Among them, the adsorption amount of Congo red measured at 10 min of adsorption was 1234 mg / g, and the adsorption amount at 48 h of adsorption was 1981 mg / g.
[0053] Example 4
[0054] A method for preparing spherical pseudo-boehmite cluster particles is carried out according to the following steps:
[0055] (1) Sodium aluminate is dissolved in deionized water to prepare a 50 mL, 0.7 mol / L solution, which is then placed in an oil bath and heated to 30° C.; concentrated nitric acid is diluted to prepare a 50 mL, 0.7 mol / L nitric acid solution, and the nitric acid solution is added to the stirred sodium aluminate solution at a flow rate of 1 mL / min using a peristaltic pump.
[0056] (2) After the addition of the nitric acid solution, the reaction slurry was centrifuged, washed, and dried to obtain the product. The product was washed twice with deionized water and then twice with anhydrous ethanol. The drying temperature was 60°C and the drying time was 12 hours. The XRD spectrum of the product is shown in Figure 1 , indicating that the product prepared in this example is pseudo-boehmite; the SEM photo of the product is shown in Figure 5 As shown, its morphology is a cluster particle composed of nano-spherical particles with a particle size of about 50-100nm assembled from nano-flakes.
[0057] (3) The sample of this example was subjected to a Congo red static adsorption experiment under the adsorption conditions described in Example 1, and the adsorption amount of Congo red by the sample at different times is shown in Table 1. Among them, the adsorption amount of Congo red measured at 10 minutes of adsorption was 1152 mg / g, and the adsorption amount at 48 hours of adsorption was 2353 mg / g.
[0058] Example 5
[0059] A method for preparing spherical pseudo-boehmite cluster particles is carried out according to the following steps:
[0060] (1) Sodium aluminate is dissolved in deionized water to prepare a 50 mL, 0.5 mol / L solution, which is then placed in an oil bath and heated to 40° C.; concentrated nitric acid is diluted to prepare a 50 mL, 0.5 mol / L nitric acid solution, and the nitric acid solution is added to the stirred sodium aluminate solution at a flow rate of 1 mL / min using a peristaltic pump.
[0061] (2) After the addition of the nitric acid solution, the reaction slurry was centrifuged, washed, and dried to obtain the product. The product was washed twice with deionized water and then twice with anhydrous ethanol. The drying temperature was 60°C and the drying time was 12 hours. The XRD spectrum of the product is shown in Figure 1 , indicating that the product prepared in this example is pseudo-boehmite; the SEM photo of the product is shown in Figure 6 As shown, its morphology is a cluster particle composed of nano-spherical particles with a particle size of about 100-200nm assembled from nano-flakes.
[0062] (3) The sample of this example was subjected to a Congo red static adsorption experiment under the adsorption conditions described in Example 1. The amount of Congo red adsorbed by the sample at different times is shown in Table 1. Among them, the amount of Congo red adsorbed by the sample at 10 min of adsorption was 1230 mg / g, and the amount of Congo red adsorbed at 48 h of adsorption was 2037 mg / g.
[0063] Example 6
[0064] A method for preparing spherical pseudo-boehmite cluster particles is carried out according to the following steps:
[0065] (1) Sodium aluminate is dissolved in deionized water to prepare a 50 mL, 1 mol / L solution, which is then placed in an oil bath and heated to 30° C. Concentrated nitric acid is diluted to prepare a 50 mL, 1 mol / L nitric acid solution, which is then added to the stirred sodium aluminate solution at a flow rate of 1 mL / min using a peristaltic pump.
[0066] (2) After the addition of the nitric acid solution, the reaction slurry was centrifuged, washed, and dried to obtain the product. The product was washed twice with deionized water and then twice with anhydrous ethanol. The drying temperature was 60°C and the drying time was 12 hours. The XRD spectrum of the product is shown in Figure 1 , indicating that the product prepared in this example is pseudo-boehmite; the SEM photo of the product is shown in Figure 7 As shown, its morphology is a cluster particle composed of nano-spherical particles with a particle size of about 50-100nm assembled from nano-flakes.
[0067] (3) The sample of this example was subjected to a Congo red static adsorption experiment under the adsorption conditions described in Example 1. The amount of Congo red adsorbed by the sample at different times is shown in Table 1. Among them, the amount of Congo red adsorbed by the sample at 10 minutes of adsorption was 1001 mg / g, and the amount of Congo red adsorbed at 48 hours of adsorption was 1757 mg / g.
[0068] The yields of pseudo-boehmite in Examples 1-6 were 86%, 86%, 85%, 86%, 88% and 88%, respectively.
[0069] Table 1 Adsorption of Congo red by samples prepared in various embodiments at different times
[0070]
[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing spherical pseudo-boehmite cluster particles, characterized in that: The following steps are involved: (1) heating the sodium aluminate solution to 30-60° C. and then adding nitric acid solution to react; (2) After the addition of the nitric acid solution in step (1) is completed, the slurry product is centrifuged, and the filter cake is washed and dried to obtain the pseudo-boehmite product.
2. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the sodium aluminate solution is 0.1-1 mol / L, and the concentration of the nitric acid solution is 0.1-1 mol / L; the volume ratio of the sodium aluminate solution to the nitric acid solution is 1:1, and the concentrations are the same.
3. The preparation method according to claim 2, characterized in that: The concentration of the sodium aluminate solution in step (1) is selected from 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.7 mol / L or 1.0 mol / L.
4. The preparation method according to claim 2, characterized in that: The concentration of the nitric acid solution in step (1) is selected from 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.7 mol / L or 1.0 mol / L.
5. The preparation method according to claim 1, characterized in that: The addition rate of the nitric acid solution in step (1) is 0.5-5 mL / min.
6. The preparation method according to claim 1, characterized in that: In step (2), the washing is carried out sequentially with water and anhydrous ethanol.
7. The preparation method according to claim 1, characterized in that: The drying in step (2) refers to drying at 60° C. for 12 hours.
8. A spherical pseudo-boehmite cluster particle, characterized in that: The spherical pseudo-boehmite cluster particles are prepared by the preparation method according to any one of claims 1 to 7, and are assembled from a large number of interwoven nanosheets.
9. Use of the spherical pseudo-boehmite cluster particles according to claim 8 in adsorbing Congo red dye in water.