Method for optimally utilizing reclaimed water
By optimizing the calcium and salt treatment process, low concentration of reclaimed water is directly used for the second washing and salt treatment of titanium dioxide, which solves the problems of membrane blockage and resource waste during reclaimed water treatment in titanium dioxide production, and realizes effective recycling of reclaimed water and the performance of titanium dioxide.
Patent Information
- Application Number
- CN202410918221.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
AI Technical Summary
In the production of existing titanium dioxide, membrane blockage problems and waste of resources during recycled water treatment, and the amount of salt treatment agent is large, which affects production costs.
By optimizing the calcium and salt treatment process, low concentration of medium water is directly used for two-washing and salt treatment, the phosphorus, aluminum and sodium content in the titanium dioxide after calcination is controlled, and gradient heating calcination is used to reduce the amount of sodium salt and increase the titanium dioxide. performance.
Effectively recover the sodium salt in the recycled water, reduce the amount of salt treatment agent, solve the problem of membrane blockage during recycled water treatment, save the amount of softening water and subsequent treatment costs, and the performance of titanium dioxide is not weaker than that of conventional methods.
Smart Images

Figure CN118908273A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium dioxide production, and particularly relates to a method for optimizing the utilization of reclaimed water. Background Art
[0002] The production of titanium dioxide by sulfuric acid process includes the following steps: acidolysis, sedimentation, crystallization, concentration, hydrolysis, primary water washing, metatitanic acid bleaching, secondary water washing, salt treatment, calcination, intermediate crushing and surface treatment. A large amount of titanium dioxide waste acid is generated during the production process.
[0003] Existing technology of water application, such as Figure 1 As shown, first, titanium dioxide waste acid is separated into high-concentration waste acid and low-concentration waste acid and neutralized respectively to obtain high-concentration reclaimed water and low-concentration reclaimed water, wherein the sodium content in the high-concentration reclaimed water is about 3500-5000ppm, the sodium content in the low-concentration reclaimed water is about 2000-3000ppm, and the calcium content is about 600-700ppm. Then, the high-concentration reclaimed water and the low-concentration reclaimed water are combined and soda ash is added to uniformly remove calcium. After clarification, the water enters the reverse osmosis membrane treatment system after passing through a multi-media filter, catalytic adsorption and ultrafiltration to obtain softened water, which is then reused in the titanium dioxide production system. However, there is still a certain amount of calcium and sulfate in the reclaimed water after neutralization and decalcification. The presence of calcium and sulfate will cause the reverse osmosis membrane to be blocked and further cause the reverse osmosis membrane system to be paralyzed, resulting in the inability to recycle the reclaimed water, resulting in a waste of resources.
[0004] On the other hand, in order to improve the calcination performance of titanic acid, inorganic salts such as potassium salts, phosphorus salts, zinc salts, etc. are generally used to treat the filter cake after secondary water washing before calcination. If the inorganic salt components in the reclaimed water can be recovered for salt treatment, the reclaimed water can be effectively recycled and utilized, while reducing the amount of salt treatment agent used and reducing production costs.
[0005] Based on the above content, the present application aims to provide a method for optimizing the utilization of reclaimed water. Summary of the invention
[0006] The purpose of the present invention is to provide a method for optimizing the utilization of reclaimed water in order to solve the deficiencies of the prior art.
[0007] The purpose of the present invention is achieved by the following technical solutions:
[0008] A method for optimizing the utilization of reclaimed water comprises the following steps:
[0009] S1. Decalcification: Take low-concentration water and first decalcify it, and control the calcium content in the decalcified water to ≤60ppm;
[0010] S2. Second washing: taking the bleached metatitanic acid, washing it with decalcified water to obtain a second washing filter cake;
[0011] S3. Salt treatment: the secondary filter cake is pulped, and then a quantitative phosphorus source, an aluminum source and a sodium source are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the titanium dioxide after calcination are controlled to be 0.18% to 0.22%, 0.23% to 0.30% and 0.24% to 0.30%, respectively; the contents of phosphorus, aluminum and sodium are measured as P2O5, Al2O3 and Na2O, respectively.
[0012] Preferably, the sodium content of the low-concentration water is 2000-3000 ppm, and the calcium content is 600-700 ppm.
[0013] Preferably, in step S1, sodium carbonate is used for decalcification, and the amount of sodium carbonate used is 1.5 to 2 times the theoretical amount. When the pH of the low-concentration water is low, sodium hydroxide is first used to adjust the pH to ≥ 10, and then the sodium carbonate is added.
[0014] Preferably, step S3 uses softened water or the solution obtained by solid-liquid separation of the material after the salt treatment for pulping.
[0015] Preferably, the slurry concentration obtained by the slurrying is 280-340 g / L in terms of titanium dioxide content.
[0016] Preferably, the phosphorus source is phosphoric acid.
[0017] Preferably, the aluminum source is aluminum sulfate.
[0018] Preferably, the sodium source is sodium sulfate.
[0019] Preferably, after step S3, the method further includes the steps of solid-liquid separation of the slurry after the salt treatment and calcination to obtain titanium dioxide;
[0020] The calcination to rutile conversion rate is 98% to 99.3%.
[0021] Preferably, the calcination adopts the following process:
[0022] a. Raise the temperature from room temperature to 180-220℃ within 15-25min;
[0023] b. Raise the temperature to 330-370°C within 25-35 minutes;
[0024] c. Raise the temperature to 630-670°C within 25-35 minutes;
[0025] d. Raise the temperature to 720-760°C within 10-20 minutes;
[0026] e. Keep at 720-760℃ for 40-80min;
[0027] f. Raise the temperature to 850-880°C within 12-18 minutes;
[0028] g. Keep at 850-880℃ for 100-140min;
[0029] h. Raise the temperature to 945-955°C within 8-12 minutes;
[0030] i. Keep warm at 945-955℃ for 1-4h.
[0031] The present application uses low-concentration reclaimed water directly for the secondary washing of titanium dioxide in the sulfuric acid process without passing through a membrane treatment system, which can save the amount of softened water used in titanium dioxide production and the cost of subsequent reclaimed water treatment stages, solve the problem of membrane clogging during reclaimed water treatment, and effectively recycle and utilize sodium salts in the reclaimed water, reducing the amount of salt treatment agent used. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a process flow chart of reclaimed water application in the prior art. DETAILED DESCRIPTION
[0033] The present application provides a method for optimizing the utilization of reclaimed water, comprising the following steps:
[0034] S1. Decalcification: low-concentration water is first decalcified to control the calcium content to ≤60ppm after decalcification; low-concentration water is obtained by neutralizing low-concentration titanium dioxide waste acid, wherein the sodium content is about 2000-3000ppm and the calcium content is about 600-700ppm;
[0035] S2. Second washing: taking the bleached metatitanic acid, washing it with decalcified water to obtain a second washing filter cake;
[0036] S3. Salt treatment: the second-wash filter cake is pulped, and then a quantitative phosphorus source, an aluminum source and a sodium source are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the titanium dioxide after calcination are controlled to be 0.18% to 0.22%, 0.23% to 0.30% and 0.24% to 0.30%, respectively; the contents of phosphorus, aluminum and sodium are measured as P2O5, Al2O3 and Na2O, respectively.
[0037] This application uses the reclaimed water directly for secondary washing without membrane treatment, and recovers the sodium ions contained in the reclaimed water as a salt treatment agent, thereby achieving the purpose of both recovering the reclaimed water and reducing the amount of salt treatment agent. There are several obstacles when recycling reclaimed water as a salt treatment agent:
[0038] 1. First, in the prior art, calcium removal is to use sodium carbonate and calcium ions in water to form calcium carbonate precipitation to remove calcium. The calcium concentration in the water after calcium removal is about 400-500ppm. Calcium ions have a great influence on the performance of titanium dioxide. If the calcium content is too high, it will increase the viscosity of the kiln product and cause uneven distribution of materials in the post-processing process. The calcium ions in the decalcified water obtained by the existing decalcification process are relatively high and cannot meet production requirements;
[0039] 2. The content of calcium and sodium ions in high-concentration water is very high. First, it increases the difficulty of calcium removal. Second, experiments have found that excessive sodium ion content as a salt treatment agent will also affect the performance of titanium dioxide;
[0040] 3. Although sodium ions and potassium ions belong to the same main group and have similar properties, their effects on the calcination of titanium dioxide are not exactly the same.
[0041] In view of the above problems, the present application first separates high-concentration water from low-concentration water, reuses only low-concentration water, and then optimizes the decalcification process, so that the calcium concentration in the water after decalcification is reduced to ≤60ppm, and the concentration of the water after decalcification is strictly controlled to avoid adverse effects on subsequent production. Finally, the type and dosage of salt treatment are optimized, and P, Al and Na ions are selected for use to obtain a better salt treatment effect. Among them, Na is opposite to potassium ions, and can promote rutile crystal transformation within a limited range, reduce calcination temperature, and P and Al can inhibit crystal transformation speed, avoid grain sintering and growth, and P, Al and sodium ions are combined to make rutile crystal stable transformation, and regulate grain size and shape. The sodium ion content in low-concentration water cannot meet the use of salt treatment, so an additional sodium source is added for supplementation.
[0042] The performance of the titanium dioxide obtained by calcining after salt treatment using the above method is not inferior to that of the titanium dioxide obtained by the conventional method, which proves that other impurity ions in the reclaimed water have no adverse effects on the performance of the titanium dioxide.
[0043] Therefore, the present application uses low-concentration reclaimed water directly for the secondary washing of titanium dioxide in the sulfuric acid process without passing through a membrane treatment system, which can save the amount of softened water used in titanium dioxide production and the cost of subsequent reclaimed water treatment stages, solve the problem of membrane clogging during reclaimed water treatment, and effectively recycle and utilize sodium salts in reclaimed water, reducing the amount of salt treatment agent used.
[0044] Preferably, sodium carbonate is used for decalcification in step S1. In order to improve the decalcification effect, the amount of sodium carbonate used is 1.5 to 2 times the theoretical amount. When the pH of the low-concentration water is low, sodium hydroxide is first used to adjust the pH to ≥ 10, and then sodium carbonate is added. When sodium carbonate is used for decalcification, on the one hand, the introduced sodium ions can serve as a partial salt treatment agent, and on the other hand, the excess carbonate ions can be removed during the calcination process, so it will not have an adverse effect on the performance of titanium dioxide.
[0045] Preferably, the second washing is performed until Fe in the material is ≤20 ppm.
[0046] Preferably, step S3 uses softened water or a solution obtained by solid-liquid separation of the material after salt treatment (generally referred to as pre-kiln filter press water) for pulping to reduce the impact of impurity ions on titanium dioxide production. The solution obtained by solid-liquid separation of the material after salt treatment contains a salt treatment agent, and pulping the solution can effectively recycle the salt treatment agent.
[0047] Preferably, the slurry concentration obtained by slurrying is 280 to 340 g / L in terms of titanium dioxide content.
[0048] Phosphoric acid can be used as a phosphorus source, aluminum sulfate can be used as an aluminum source, and sodium sulfate can be used as a sodium source. The use of phosphoric acid, aluminum sulfate, and sodium sulfate will not introduce new impurities and will not affect product quality.
[0049] Preferably, after step S3, the method further includes the steps of solid-liquid separation of the slurry after the salt treatment and calcination to obtain titanium dioxide;
[0050] The calcination to rutile conversion rate is 98% to 99.3%.
[0051] The dehydration, desulfurization and crystal transformation of metatitanic acid are carried out in different temperature ranges. Preferably, the calcination adopts a gradient temperature increase, as follows:
[0052] a. Raise the temperature from room temperature to 180-220℃ within 15-25min;
[0053] b. Raise the temperature to 330-370°C within 25-35 minutes;
[0054] c. Raise the temperature to 630-670°C within 25-35 minutes;
[0055] d. Raise the temperature to 720-760°C within 10-20 minutes;
[0056] e. Keep at 720-760℃ for 40-80min;
[0057] f. Raise the temperature to 850-880°C within 12-18 minutes;
[0058] g. Keep at 850-880℃ for 100-140min;
[0059] h. Raise the temperature to 945-955°C within 8-12 minutes;
[0060] i. Keep warm at 945-955℃ for 1-4h.
[0061] Sodium salt can promote the transformation of rutile crystal relative to potassium salt, so the maximum calcination temperature and time are lower than those of potassium salt (the maximum calcination temperature of potassium salt is generally 955-965°C, and the insulation time is 5-8h).
[0062] Example 1
[0063] Take low-concentration titanium dioxide waste acid water and neutralize it to pH 10.5 to obtain low-concentration water, in which the calcium concentration is 650ppm and the sodium concentration is 2600ppm. Add 1.6 times the theoretical amount of sodium carbonate for decalcification. The calcium content after decalcification is 55ppm, ≤60ppm; then take the bleached metatitanic acid and use the decalcified water for secondary washing to obtain the secondary washing filter cake; add softened water to the secondary washing filter cake for pulping, control the slurry concentration to 320g / L, and then add quantitative phosphoric acid, aluminum sulfate and sodium sulfate for salt treatment, and control the mass percentage of phosphorus, aluminum and sodium in the calcined titanium dioxide to be 0.195%, 0.277% and 0.278% respectively, and the contents of phosphorus, aluminum and sodium are calculated as P2O5, Al2O3 and Na2O respectively. Then calcination is carried out, and the calcination heating program is as follows:
[0064] 200℃20min (this means rising from room temperature to 200℃ within 20min, the following expressions are the same) → 350℃30min → 650℃30min → 740℃15min → keep at 740℃ for 60min → 865℃15min → keep at 865℃ for 120min → 955℃10min → keep at 955℃ for 2h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0065] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0066] Table 1
[0067] project result <![CDATA[Na2O%]]> 0.278 <![CDATA[K2O%]]> 0.026 <![CDATA[P2O5%]]> 0.195 <![CDATA[Al2O3%]]> 0.277 Fe / ppm 13.54 R% 99.45 Blue light whiteness 90.7 brightness 94.5 Black removal -2.14 CS 0.291 CSD 1.448
[0068] Example 2
[0069] Low-concentration titanium dioxide waste acid water is neutralized to pH 11 to obtain low-concentration reclaimed water, wherein the calcium concentration is 685ppm and the sodium concentration is 2400ppm, and 1.8 times the theoretical amount of sodium carbonate is added for decalcification. The calcium content after decalcification is tested to be 54ppm, ≤60ppm; then the bleached metatitanic acid is taken and the decalcified reclaimed water is used for secondary washing to obtain a secondary washing filter cake; softened water is added to the secondary washing filter cake for pulping, the slurry concentration is controlled to be 290g / L, and then a certain amount of phosphoric acid, aluminum sulfate and sodium sulfate are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the calcined titanium dioxide are controlled to be 0.188%, 0.265% and 0.262% respectively, and the contents of phosphorus, aluminum and sodium are calculated as P2O5, Al2O3 and Na2O respectively.
[0070] Then calcination is carried out, and the calcination temperature program is as follows:
[0071] 200℃20min→350℃30min→650℃30min→740℃15min→740℃keep for 60min→865℃15min→865℃keep for 120min→950℃10min→950℃keep for 3h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0072] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0073] Table 2
[0074] project result <![CDATA[Al2O3%]]> 0.265 <![CDATA[K2O%]]> 0.014 <![CDATA[P2O5%]]> 0.188 <![CDATA[Na2O%]]> 0.262 Fe / ppm 8 R% 99.2 Whiteness 91.22 brightness 95.2 Black removal -1.97 Scattering power 103 CS 0.2583 CSD 1.4004
[0075] Example 3
[0076] Low-concentration titanium dioxide waste acid is neutralized to pH 11 to obtain low-concentration reclaimed water, wherein the calcium concentration is 680 ppm and the sodium concentration is 2700 ppm. Sodium carbonate twice the theoretical amount is added for decalcification. The calcium content after decalcification is tested to be 48 ppm, ≤ 60 ppm. Then, the bleached metatitanic acid is taken and second-washed with the decalcified reclaimed water to obtain a second-wash filter cake. Softened water is added to the second-wash filter cake for pulping, and the slurry concentration is controlled to be 300 g / L. Then, a certain amount of phosphoric acid, aluminum sulfate and sodium sulfate are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the calcined titanium dioxide are controlled to be 0.209%, 0.285% and 0.281 respectively. The contents of phosphorus, aluminum and sodium are calculated as P2O5, Al2O3 and Na2O respectively.
[0077] Then calcination is carried out, and the calcination temperature program is as follows:
[0078] 200℃20min→350℃30min→650℃30min→740℃15min→740℃keep for 60min→865℃15min→865℃keep for 120min→945℃10min→945℃keep for 4h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0079] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0080] Table 3
[0081] project result <![CDATA[Al2O3%]]> 0.285 <![CDATA[K2O%]]> 0.063 <![CDATA[P2O5%]]> 0.209 <![CDATA[Na2O%]]> 0.281 Fe / ppm 10 R% 98.4 Whiteness 91.33 brightness 95.25 Black removal -1.83 Scattering power 104 CS 0.2975 CSD 1.4314
[0082] Comparative Example 1
[0083] The pulped material after secondary washing produced by the conventional method is directly added with a certain amount of phosphoric acid, aluminum sulfate and potassium sulfate for salt treatment, and the mass percentages of phosphorus, aluminum and potassium in the titanium dioxide after calcination are controlled to be 0.183%, 0.271% and 0.278%, respectively. The contents of phosphorus, aluminum and potassium are calculated as P2O5, Al2O3 and K2O, respectively.
[0084] Then calcination is carried out, and the calcination temperature program is as follows:
[0085] 200℃20min→350℃30min→650℃30min→740℃15min→740℃keep for 60min→865℃15min→865℃keep for 120min→960℃10min→960℃keep for 6h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0086] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0087] Table 4
[0088] project result <![CDATA[Na2O%]]> 0.026 <![CDATA[K2O%]]> 0.278 <![CDATA[P2O5%]]> 0.183 <![CDATA[Al2O3%]]> 0.271 Fe / ppm 15.01 R% 99.25 Blue light whiteness 90.9 brightness 94.1 Black removal -1.89 CS 0.313 CSD 1.538 Scattering power 105
[0089] Comparative Example 2
[0090] The pulped material after secondary washing produced by the conventional method is directly added with a certain amount of phosphoric acid, aluminum sulfate and potassium sulfate for salt treatment, and the mass percentages of phosphorus, aluminum and potassium in the titanium dioxide after calcination are controlled to be 0.182%, 0.286% and 0.283%, respectively. The contents of phosphorus, aluminum and potassium are calculated as P2O5, Al2O3 and K2O, respectively.
[0091] Then calcination is carried out, and the calcination temperature program is as follows:
[0092] 200℃20min→350℃30min→650℃30min→740℃15min→740℃keep for 60min→865℃15min→865℃keep for 120min→960℃10min→965℃keep for 6h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0093] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0094] Table 5
[0095]
[0096]
[0097] Comparative Example 3
[0098] Low-concentration titanium dioxide waste acid is neutralized to pH 11 to obtain low-concentration reclaimed water, wherein the calcium concentration is 680 ppm and the sodium concentration is 2700 ppm; sodium carbonate is added in an amount of 1 times the theoretical amount for decalcification, and the calcium content after decalcification is tested to be 474 ppm, and then the bleached metatitanic acid is taken and second-washed with reclaimed water to obtain a second-wash filter cake; softened water is added to the second-wash filter cake for pulping, and the slurry concentration is controlled to be 300 g / L, and then a certain amount of phosphoric acid, aluminum sulfate and sodium sulfate are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the calcined titanium dioxide are controlled to be 0.193%, 0.277% and 0.284 respectively; the contents of phosphorus, aluminum and sodium are calculated as P2O5, Al2O3 and Na2O respectively.
[0099] Then calcination is carried out, and the calcination temperature program is as follows:
[0100] 200℃20min→350℃30min→650℃30min→740℃15min→740℃keep for 60min→865℃15min→865℃keep for 120min→945℃10min→945℃keep for 4h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0101] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0102] Table 6
[0103] project result <![CDATA[Al2O3%]]> 0.277 <![CDATA[K2O%]]> 0.030 <![CDATA[P2O5%]]> 0.193 <![CDATA[Na2O%]]> 0.284 CaO 0.044 Fe / ppm 6.8 R% 99.08 Whiteness 91.21 brightness 95.1 Black removal -1.76 Scattering power 94 CS 0.2868 CSD 1.4742
[0104] The increase of calcium content will increase the blackening and weaken the scattering power, which will affect the hiding power of the product. At the same time, it will lead to increased viscosity, poor fluidity and uneven distribution. Normally it is below 200. The viscosity value results are shown in Table 7.
[0105] Table 7
[0106] CaO / % Viscosity 0.044 700
[0107] Comparative Example 4
[0108] Low-concentration titanium dioxide waste acid is neutralized to pH 10.5 to obtain low-concentration reclaimed water, in which the calcium concentration is 650 ppm and the sodium concentration is 2600 ppm; sodium carbonate is added in an amount of 1 times the theoretical amount for decalcification, and the calcium content after decalcification is tested to be 438 ppm; then the bleached metatitanic acid is taken and washed twice with reclaimed water to obtain a second-wash filter cake; softened water is added to the second-wash filter cake for pulping, and the pulp concentration is controlled to be 300 g / L, and then a certain amount of phosphoric acid, aluminum sulfate and sodium sulfate are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the calcined titanium dioxide are controlled to be 0.195%, 0.285% and 0.283 respectively; the contents of phosphorus, aluminum and sodium are calculated as P2O5, Al2O3 and Na2O respectively.
[0109] Then calcination is carried out, and the calcination temperature program is as follows:
[0110] 200℃20min→350℃30min→650℃30min→740℃15min→740℃keep for 60min→865℃15min→865℃keep for 120min→945℃10min→945℃keep for 4h, the rutile conversion rate after calcination is controlled to be 98%~99.3%.
[0111] Take the calcined samples and test the whiteness, brightness, black paste b*, CS and scattering power according to conventional methods.
[0112] Table 8
[0113] project result <![CDATA[Al2O3%]]> 0.285 <![CDATA[K2O%]]> 0.029 <![CDATA[P2O5%]]> 0.195 <![CDATA[Na2O%]]> 0.283 CaO 0.041 Fe / ppm 2.3 R% 99.1 Whiteness 91.43 brightness 94.95 Black removal -1.72 Scattering power 98 CS 0.2973 CSD 1.4946
[0114] The increase of calcium content will increase the blackening and weaken the scattering power, which will affect the hiding power of the product. At the same time, it will lead to increased viscosity, poor fluidity and uneven distribution. The normal viscosity is below 200. The viscosity value results are shown in Table 9.
[0115] Table 9
[0116] CaO / % Viscosity 0.041 680
[0117] The above comparative examples prove that the quality of the titanium dioxide product obtained by recycling water in Examples 1 to 3 of the present application is not inferior to that of the titanium dioxide obtained by conventional methods, and the maximum calcination temperature is also reduced, which effectively saves costs.
[0118] Although preferred embodiments of the present invention have been described, additional changes and modifications may be made to these embodiments by those skilled in the art once the basic inventive concepts are known. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for optimizing the utilization of reclaimed water, characterized in that: The following steps are involved: S1. Decalcification: Take low-concentration water and first decalcify it, and control the calcium content in the decalcified water to ≤60ppm; S2. Second washing: taking the bleached metatitanic acid, washing it with decalcified water to obtain a second washing filter cake; S3. Salt treatment: the secondary filter cake is pulped, and then a quantitative phosphorus source, an aluminum source and a sodium source are added for salt treatment, and the mass percentages of phosphorus, aluminum and sodium in the titanium dioxide after calcination are controlled to be 0.18% to 0.22%, 0.23% to 0.30% and 0.24% to 0.30%, respectively; the contents of phosphorus, aluminum and sodium are measured as P2O5, Al2O3 and Na2O, respectively.
2. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: The sodium content of the low-concentration water is 2000-3000 ppm, and the calcium content is 600-700 ppm.
3. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: In step S1, sodium carbonate is used for decalcification, and the amount of sodium carbonate used is 1.5 to 2 times of the theoretical amount. When the pH of the low-concentration water is low, sodium hydroxide is first used to adjust the pH to ≥ 10, and then the sodium carbonate is added.
4. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: In step S3, softened water or the solution obtained by solid-liquid separation of the material after the salt treatment is used for pulping.
5. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: The slurry concentration obtained by the slurrying is 280-340 g / L in terms of titanium dioxide content.
6. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: The phosphorus source is phosphoric acid.
7. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: The aluminum source is aluminum sulfate.
8. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: The sodium source is sodium sulfate.
9. The method for optimizing the utilization of reclaimed water according to claim 1, characterized in that: After step S3, the method further includes performing solid-liquid separation on the slurry after the salt treatment and calcining to obtain titanium dioxide; The calcination to rutile conversion rate is 98% to 99.3%.
10. The method for optimizing the utilization of reclaimed water according to claim 9, characterized in that: The calcination process is as follows: a. Raise the temperature from room temperature to 180-220℃ within 15-25min; b. Raise the temperature to 330-370°C within 25-35 minutes; c. Raise the temperature to 630-670°C within 25-35 minutes; d. Raise the temperature to 720-760°C within 10-20 minutes; e. Keep at 720-760℃ for 40-80min; f. Raise the temperature to 850-880°C within 12-18 minutes; g. Keep at 850-880℃ for 100-140min; h. Raise the temperature to 945-955°C within 8-12 minutes; i. Keep warm at 945-955℃ for 1-4h.