Method for extracting vanadium pentoxide from composite oxidized ore doped lepidolite

By using lepidolite adsorption-exchange technology under alkaline conditions, the problems of low impurity removal efficiency and environmental pollution in the extraction process of vanadium pentoxide from composite oxide ores have been solved, achieving efficient extraction and purification of vanadium pentoxide.

CN118908276APending Publication Date: 2024-11-08XICHUAN HAOYANG VANADIUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010574.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies for extracting vanadium pentoxide from complex oxide ores suffer from problems such as low impurity removal efficiency, severe environmental pollution, and low raw material utilization. In particular, the low beneficiation efficiency of vanadium ore in complex oxide ores leads to a waste of vanadium resources.

Method used

Lithium mica was used as the adsorbent to adsorb and exchange non-vanadium ion substances in vanadium leaching solution under alkaline conditions. By adjusting the pH and temperature, the adsorption capacity of lepidolite was enhanced, removing impurity metal ions and retaining vanadium ions. Vanadium pentoxide was then obtained by vanadium extraction.

Benefits of technology

It improves the leaching rate of vanadium ions, reduces the difficulty of subsequent extraction, saves resources, reduces environmental pollution, and increases the yield and purity of vanadium pentoxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908276A_ABST
    Figure CN118908276A_ABST
Patent Text Reader

Abstract

The invention provides a method for extracting vanadium pentoxide from composite oxidized ore doped with lepidolite, and belongs to the technical field of chemical metallurgy. Lepidolite is adopted as an adsorption substance, non-vanadium ion substances in vanadium leachate are subjected to adsorption exchange under the alkaline condition, vanadium ion mother liquor mainly containing vanadium ions is obtained, and vanadium pentoxide is extracted from the mother liquor. The alkaline condition and the main steps are as follows: S1, the composite oxidized ore is leached by an alkaline solution, so that vanadium substances and soluble metal elements in the composite oxidized ore are converted into a salt ion form, and vanadium-containing alkaline leachate is obtained; s2, flaky lepidolite is added, stirring is started, the vanadium-containing alkaline leachate flows circularly, the pH is adjusted to 8.5-11.3, the temperature is adjusted to 25-60 DEG C, the time is 8-12 h, lepidolite and insoluble substances are removed, and vanadium ion mother liquor is obtained; according to the method, miscellaneous metal ions can be efficiently removed, so that the vanadium ions in the solution are retained, and the leaching rate of the vanadium ions is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical metallurgy, and in particular to a method for extracting vanadium pentoxide from lepidolite doped with composite oxide ore. Background Art

[0002] Vanadium pentoxide is an inorganic compound with the chemical formula V2O5. It is an important vanadium compound, widely used in industry and chemistry. Vanadium pentoxide is a light yellow solid, which is crystalline or powdery at room temperature. It has good chemical and thermal stability, and can be used as an industrial catalyst for oxidation, desalination and oxidation deacidification reactions. It can also be used as a battery material to improve battery performance and cycle life. It has high color stability and photocorrosion resistance, and can be used as an anti-corrosion material added to glass or ceramic glazes.

[0003] The existing vanadium pentoxide is mainly obtained through four methods, namely, sulfuric acid method, hydrochloric acid method, ammonium carbonate method and alkali method; among them, the sulfuric acid method will produce a large amount of waste gas and wastewater during the production process, causing certain pollution to the environment, the hydrochloric acid method requires the use of high-purity oxygen, and has high requirements for equipment; the ammonium carbonate method has a slow reaction speed, a high reaction temperature, and a low product purity; finally, the alkali method requires the use of a large amount of alkali and acid, which causes certain pollution to the environment; and the raw materials of the sulfuric acid method and the hydrochloric acid method are mostly metallic vanadium and waste vanadium materials. Therefore, for composite oxide ores that account for about 98% of oxidized impurities in the raw materials, a large amount of sulfuric acid and hydrochloric acid are required to generate vanadium pentoxide, and the economic value is too low. The raw material of the ammonium carbonate method is ammonium carbonate, so it is impossible to extract a large amount of composite oxide ores; therefore, before the vanadium ore in a large amount of composite oxide ores is subjected to the alkali method to produce sodium metavanadate, it is necessary to beneficiate, but the ore dressing efficiency is low, and some vanadium is not apparent in the ore, thus causing a waste of vanadium, and directly reacting the raw materials with alkali is inefficient. Summary of the invention

[0004] In view of this, the present invention provides a method for extracting vanadium pentoxide from composite oxide ore doped with lepidolite, which can efficiently remove heterometallic ions, thereby retaining vanadium ions in the solution and improving the leaching rate of vanadium ions.

[0005] The present invention provides a method for extracting vanadium pentoxide from lepidolite doped with composite oxide ore, characterized in that lepidolite is used as an adsorbent, non-vanadium ion substances in a vanadium leaching solution are adsorbed and exchanged under alkaline conditions to obtain a vanadium ion mother liquor mainly containing vanadium ions, and then vanadium extraction treatment is performed to obtain vanadium pentoxide. The alkaline conditions and main steps are as follows: S1. Leaching the composite oxide ore with an alkaline solution to convert the vanadium substance and soluble metal elements therein into salt ion form to obtain a vanadium-containing alkaline leaching solution; S2, adding flaky lithium mica to the vanadium-containing alkaline leachate, stirring and circulating the vanadium-containing alkaline leachate, adjusting the pH to 8.5-11.3, adjusting the temperature to 25° C. to 60° C. for 8-12 hours, removing the lithium mica and insoluble substances to obtain a vanadium ion mother liquor; S3, extracting vanadium from the vanadium ion mother liquor to obtain vanadium pentoxide.

[0006] The present invention performs alkaline leaching on the composite oxide ore to obtain various metal ion mixed solutions, wherein the mixed solution contains soluble ions in the composite oxide ore, and then adds lithium mica to the mixed solution. Under high alkaline conditions, the structure of the lithium mica changes, and the adsorption and exchange capabilities of the lithium mica for metal ions are enhanced, so that specific metal ions can be adsorbed or exchanged. These metal ions are adsorbed or fixed in the structure of the lithium mica. Under alkaline conditions, some metal ions are not easy to form bonds with oxygen atoms in the lithium mica. However, after adjusting pH and temperature, the metal ions in the composite oxide ore will still undergo adsorption reactions with the lithium mica. Moreover, since vanadium ions exist in the form of hydroxide ions, the competitive effect between vanadium ions and lithium mica is stronger than that of other metal ions. Therefore, the adsorption effect of vanadium ions in lithium mica is the worst. In comparison, the adsorption of most ions such as iron, zinc, and magnesium on lithium mica is more efficient under alkaline conditions. The present invention has found the pH and temperature ranges in which other metal ions can be adsorbed after multiple experiments and verifications, and the vanadium ions will not be adsorbed within this range.

[0007] The present invention uses lithium mica for adsorption and exchange in an alkaline environment, and can wash away the metal ions adsorbed thereon by washing afterwards, thereby obtaining lithium mica that can be used again. This is economical and environmentally friendly, and can greatly save resources compared to the traditional alkaline method.

[0008] Furthermore, the solution used in the leaching step in S1 is a sodium hydroxide solution, the concentration of the sodium hydroxide solution is 4 mol / L, the temperature is 55-70° C., and the stirring speed is 120 rpm / min.

[0009] Furthermore, the thickness of the lepidolite flakes in S2 is 3-5 mm, and the distance between each piece of lepidolite is controlled at 1-2 cm.

[0010] Furthermore, the vanadium extraction process comprises the following steps: S31, reducing the vanadium ion mother liquor in S2, using a reducing agent to change the valence state of vanadium, and filtering to obtain sodium metavanadate; S32, performing acid hydrolysis and oxidation on sodium metavanadate, dissolving the sodium metavanadate in water to obtain a sodium metavanadate solution, and then adding an acid solution to the sodium metavanadate solution for oxidation reaction to produce a vanadium pentoxide precipitate; S33. Finally, the obtained vanadium pentoxide is dried to remove residual moisture and impurities to obtain pure vanadium pentoxide.

[0011] Furthermore, the reducing agent in S31 is sodium bisulfite, sodium sulfite and thiosulfur.

[0012] Furthermore, the acid in S32 is hydrochloric acid or sulfuric acid.

[0013] Furthermore, the temperature of the reaction of the sodium metavanadate and the acid solution is 20-60° C., the concentration range of the acid solution is 1-5 mol / L, and the reaction is terminated when no gas is generated.

[0014] Furthermore, after the oxidation reaction, a secondary oxidation may be performed, and an oxidant is used to perform the secondary oxidation reaction.

[0015] Furthermore, the oxidant is hydrogen peroxide or oxygen.

[0016] In summary, compared with the prior art, the present application has at least one of the following beneficial technical effects: 1. The present invention can reduce the amount of other ions except vanadium ions in the alkaline leachate, thereby reducing the difficulty of subsequent extraction of vanadium ions. In the composite multi-ion solution, ions such as iron, aluminum, zinc and magnesium are adsorbed, leaving only vanadium ions that are not adsorbed, thereby reducing the use of precipitation solvents and the removal of impurities in the subsequent precipitation process. In addition, in the presence of a large amount of composite oxide ore, vanadium ions can be extracted to the greatest extent, avoiding the neglect of ores containing vanadium elements in the mineral processing process, thereby reducing the output of vanadium pentoxide.

[0017] 2. In the present invention, reduction reaction, oxidation and re-oxidation reaction are successively carried out in steps S31 and S32. Because direct oxidation is not easy under normal conditions, it is difficult to directly convert vanadium from a low oxidation state (such as vanadium tetroxide) to vanadium pentoxide by direct oxidation reaction. The reaction kinetics of direct oxidation reaction are poor and require higher temperature and oxidant concentration to achieve. Therefore, the vanadium element is first reduced to a lower oxidation state and then oxidized, which can increase the reaction rate and product purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the change of vanadium concentration in the present invention; Figure 2 It is a schematic diagram of the preservation rate of various embodiments of the present invention and comparative examples. DETAILED DESCRIPTION

[0019] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the following will be combined with the appended drawings of the embodiments of the present invention. Figure 1-2, the technical scheme of the embodiment of the present invention is clearly and completely described. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0020] Embodiment 1 A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The vanadium content of the composite oxide ore used in this embodiment is 1.78%. The ore slag with a particle size of no more than 3 cm is obtained by crushing, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick lepidolite in the leaching tank, the spacing of each lepidolite is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH to 10.5, adjusting the temperature to 40 ° C, using the upper stirring speed of 120rpm, the time is 12h, the stirring is turned off after the time is up, and the precipitation is allowed to stand to obtain a vanadium ion mother liquor, and the vanadium ion mother liquor is discharged from the leaching tank; S3, reducing the vanadium ion mother liquor in S2, adding a reducing agent, sodium bisulfite, to the vanadium ion mother liquor to change the valence state of vanadium, filtering and leaving the precipitate, and obtaining sodium metavanadate; S32, acid-hydrolyzing and oxidizing sodium metavanadate, dissolving sodium metavanadate in a sufficient amount of water to obtain a sodium metavanadate solution, and then adding 3 mol / L hydrochloric acid to the sodium metavanadate solution for oxidation reaction, the reaction environment temperature is 40° C., and vanadium pentoxide precipitation is generated; S33. Finally, the obtained vanadium pentoxide is dried to remove residual moisture and impurities to obtain pure vanadium pentoxide.

[0021] In this example, the concentration of vanadium substance (V) in the vanadium-containing alkaline leaching solution before adjusting the pH in step S2 was detected, and it was found that the concentration of vanadium was 4.53 g / L. After the vanadium ion mother liquor was detected, the concentration of vanadium was 4.17 g / L, and the preservation rate of vanadium ions was 92%.

[0022] Embodiment 2 The difference between this embodiment and the first embodiment is that the pH is adjusted, and the specific changes are as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick lepidolite in the leaching tank, the spacing of each lepidolite is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH to 8.5, adjusting the temperature to 40 ° C, using the upper stirring speed of 120rpm, the time is 12h, the time is closed after the stirring is closed, and the vanadium ion mother liquor is obtained, and the vanadium ion mother liquor is discharged from the leaching tank; The remaining steps are the same as those in the first embodiment.

[0023] In this example, the concentration of vanadium substance (V) in the vanadium-containing alkaline leaching solution before adjusting the pH in step S2 was detected, and it was found that the concentration of vanadium was 3.74 g / L. After the vanadium ion mother liquor was detected, the concentration of vanadium was 3.40 g / L, and the preservation rate of vanadium ions was 91%.

[0024] Embodiment 3 The difference between this embodiment and the first embodiment is that the pH is adjusted, and the specific changes are as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick flaky lithium mica in the leaching tank, the spacing of each lithium mica is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH to 11.3, adjusting the temperature to 40 ° C, using the upper stirring speed of 120rpm, the time is 12h, the time is closed after the stirring is completed, and the vanadium ion mother liquor is obtained, and the vanadium ion mother liquor is discharged from the leaching tank; The remaining steps are the same as those in the first embodiment.

[0025] In this example, the concentration of vanadium substance (V) in the vanadium-containing alkaline leaching solution before adjusting the pH in step S2 was detected, and it was found that the concentration of vanadium was 4.15 g / L. After the vanadium ion mother liquor was detected, the concentration of vanadium was 3.74 g / L, and the preservation rate of vanadium ions was 90%.

[0026] Comparative Example 1 The difference between this comparative example and Example 1 is that the pH is changed, and the specific changes are as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick lepidolite in the leaching tank, the spacing of each lepidolite is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH, adjusting the temperature to 40 ° C, using the stirring speed of 120rpm, the time is 12h, the stirring is turned off after the time is up, and the precipitation is allowed to stand to obtain a vanadium ion mother liquor, and the vanadium ion mother liquor is discharged from the leaching tank; The remaining steps are the same as those in the first embodiment.

[0027] In this comparative example, the vanadium-containing alkaline leaching solution is divided into multiple stages and adjusted to different pH values ​​for verification. The specific stage adjustments are shown in Table 1 below: Table 1

[0028] It can be seen from the above comparative examples that the preservation rates of vanadium ions are 60%, 68%, 70% and 52%, respectively, which are far from the preservation rates of the embodiments.

[0029] Embodiment 4 The difference between this embodiment and the first embodiment is that the temperature of the vanadium-containing alkaline leaching solution during the adsorption stage is changed. The specific changes are as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick lepidolite in the leaching tank, the spacing of each lepidolite is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH to 10.5, adjusting the temperature to 25 ° C, using the upper stirring speed of 120rpm, the time is 12h, the time is closed after the stirring is closed, and the vanadium ion mother liquor is obtained, and the vanadium ion mother liquor is discharged from the leaching tank; The remaining steps are the same as those in the first embodiment.

[0030] In this example, the concentration of vanadium substance (V) in the vanadium-containing alkaline leaching solution before adjusting the pH in step S2 was detected, and it was found that the concentration of vanadium was 3.58 g / L. After the vanadium ion mother liquor was detected, the concentration of vanadium was 3.22 g / L, and the preservation rate of vanadium ions was 90%.

[0031] Embodiment 5 The difference between this embodiment and the first embodiment is that the temperature of the vanadium-containing alkaline leaching solution during the adsorption stage is changed. The specific changes are as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick lepidolite in the leaching tank, the spacing of each lepidolite is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH to 10.5, adjusting the temperature to 60 ° C, using the upper stirring speed of 120rpm, the time is 12h, the stirring is turned off after the time is up, and the precipitation is allowed to stand to obtain a vanadium ion mother liquor, and the vanadium ion mother liquor is discharged from the leaching tank; The remaining steps are the same as those in the first embodiment.

[0032] In this example, the concentration of vanadium substance (V) in the vanadium-containing alkaline leaching solution before adjusting the pH in step S2 was detected, and it was found that the concentration of vanadium was 4.21 g / L. After the vanadium ion mother liquor was detected, the concentration of vanadium was 3.70 g / L, and the preservation rate of vanadium ions was 88%.

[0033] Comparative Example 2 The difference between this comparative example and Example 1 is that the temperature is changed, and the specific changes are as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, in the leaching tank, stack and place 3-5mm thick flaky lithium mica, the spacing of each lithium mica is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, hydrochloric acid is used to adjust the pH to 10.5, the temperature is adjusted, the stirring speed is 120rpm, the time is 12h, the stirring is closed after the time is up, and static precipitation is performed to obtain a vanadium ion mother liquor, and the vanadium ion mother liquor is discharged from the leaching tank; The remaining steps are the same as those in the first embodiment.

[0034] In this comparative example, the vanadium-containing alkaline leaching solution is divided into multiple channels and adjusted to different temperatures for verification. The specific temperature adjustment is shown in Table 2 below: Table 2

[0035] The preservation rates of the embodiments and comparative examples are plotted in line graphs, as shown in FIG. Figure 2 shown.

[0036] Embodiment 6 The difference between this embodiment and the first embodiment is that the acid solution in S32 is added to the sodium metavanadate solution for oxidation reaction, and secondary oxidation is performed. The oxidant used is 35% concentration of hydrogen peroxide, and the specific implementation is as follows: A method for extracting vanadium pentoxide from composite oxide ore doped with lithium mica The composite oxide ore is crushed to obtain ore slag with a particle size of no more than 3 cm, and vanadium pentoxide is extracted from the ore slag. The specific extraction steps are as follows: S1. Leaching the crushed composite oxide ore with a sodium hydroxide solution having a concentration of 4 mol / L, and adjusting the temperature at 65° C. to convert the vanadium substance and soluble metal elements therein into salt ion form, thereby obtaining a vanadium-containing alkaline leaching solution; S2, stacking and placing 3-5mm thick lepidolite in the leaching tank, the spacing of each lepidolite is controlled at 1-2cm, the vanadium-containing alkaline leachate is pumped into the leaching tank, stirring and circulating the vanadium-containing alkaline leachate, using hydrochloric acid to adjust the pH to 10.5, adjusting the temperature to 40 ° C, using the upper stirring speed of 120rpm, the time is 12h, the stirring is turned off after the time is up, and the precipitation is allowed to stand to obtain a vanadium ion mother liquor, and the vanadium ion mother liquor is discharged from the leaching tank; S3, reducing the vanadium ion mother liquor in S2, adding a reducing agent, sodium bisulfite, to the vanadium ion mother liquor to change the valence state of vanadium, filtering and leaving the precipitate, and obtaining sodium metavanadate; S32, acid hydrolysis and oxidation of sodium metavanadate, dissolving sodium metavanadate in a sufficient amount of water to obtain a sodium metavanadate solution, and then adding 2 mol / L hydrochloric acid to the sodium metavanadate solution for oxidation reaction, the reaction environment temperature is 40° C., and then adding a half amount of hydrogen peroxide solution to which the hydrochloric acid has been added to the sodium metavanadate solution, the concentration of the hydrogen peroxide solution is 35%, and vanadium pentoxide precipitation is generated; S33. Finally, the obtained vanadium pentoxide is dried to remove residual moisture and impurities to obtain pure vanadium pentoxide.

[0037] In this embodiment, the purity of vanadium pentoxide is tested, and the result shows that the purity of vanadium pentoxide is as high as 97.8%.

[0038] Embodiment 7 The difference between this embodiment and the eighth embodiment is that the hydrogen peroxide solution in step S32 is replaced with oxygen, and oxidation is performed through holes opened on the coil.

[0039] In this embodiment, the purity of vanadium pentoxide is tested, and the result shows that the purity of vanadium pentoxide is as high as 96.9%.

[0040] analyze By drawing a line graph of the vanadium concentrations of Example 1, Example 2, Example 3 and Comparative Example 1, as shown in FIG. Figure 1 As shown, it can be clearly seen that the discreteness of the embodiment is smaller, while the discreteness of the comparative example is larger, which proves that the adsorption of lithium mica carried out in a pH range other than the present invention can also adsorb vanadium ions, resulting in a reduction of vanadium in the subsequent vanadium ion mother liquor.

[0041] According to the data of Example 4, Example 5 and Comparative Example 2, the vanadium substance preservation rate in the examples is above 88%, which can greatly promote the adsorption of non-vanadium ions, thereby preserving the content of vanadium ions in the leaves. Too low temperature and too high temperature will promote the bonding of vanadium ions with the changed lattice structure in lithium mica.

[0042] The experiments in Example 6 and Example 7 prove that secondary oxidation can greatly increase the purity of vanadium pentoxide.

[0043] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for extracting vanadium pentoxide from composite oxide ore doped with lepidolite, characterized in that: Using lepidolite as an adsorbent, non-vanadium ion substances in the vanadium leaching solution are adsorbed and exchanged under alkaline conditions to obtain a vanadium ion mother liquor mainly composed of vanadium ions, and then vanadium pentoxide is obtained by vanadium extraction treatment. The alkaline conditions and main steps are as follows: S1. Leaching the composite oxide ore with an alkaline solution to convert the vanadium substance and soluble metal elements therein into salt ion form to obtain a vanadium-containing alkaline leaching solution; S2, adding flaky lithium mica to the vanadium-containing alkaline leachate, stirring and circulating the vanadium-containing alkaline leachate, adjusting the pH to 8.5-11.3, adjusting the temperature to 25° C. to 60° C. for 8-12 hours, removing the lithium mica and insoluble substances to obtain a vanadium ion mother liquor; S3, extracting vanadium from the vanadium ion mother liquor to obtain vanadium pentoxide.

2. The method for extracting vanadium pentoxide from lepidolite doped with composite oxide ore according to claim 1, characterized in that: The solution used in the leaching step in S1 is a sodium hydroxide solution, the concentration of the sodium hydroxide solution is 4 mol / L, the temperature is 55-70° C., and the stirring speed is 120 rpm / min.

3. The method for extracting vanadium pentoxide from lepidolite doped with composite oxide ore according to claim 1, characterized in that: The thickness of the lepidolite flakes in S2 is 3-5 mm, and the distance between each piece of lepidolite is controlled to be 1-2 cm.

4. The method for extracting vanadium pentoxide from lepidolite doped with composite oxide ore according to claim 1, characterized in that: The vanadium extraction process comprises the following steps: S31, reducing the vanadium ion mother liquor in S2, using a reducing agent to change the valence state of vanadium, and filtering to obtain sodium metavanadate; S32, performing acid hydrolysis and oxidation on sodium metavanadate, dissolving the sodium metavanadate in water to obtain a sodium metavanadate solution, and then adding an acid solution to the sodium metavanadate solution for oxidation reaction to produce a vanadium pentoxide precipitate; S33. Finally, the obtained vanadium pentoxide is dried to remove residual moisture and impurities to obtain pure vanadium pentoxide.

5. The method for extracting vanadium pentoxide from lepidolite doped with composite oxide ore as claimed in claim 1, characterized in that: The reducing agent in S31 is sodium bisulfite, sodium sulfite and thiosulfur.

6. The method for extracting vanadium pentoxide from composite oxide ore doped with lepidolite as claimed in claim 1, characterized in that: The acid in S32 is hydrochloric acid or sulfuric acid.

7. The method for extracting vanadium pentoxide from composite oxide ore doped with lepidolite as claimed in claim 1, characterized in that: The temperature of the reaction of sodium metavanadate and acid solution is 20-60° C., the concentration range of the acid solution is 1-5 mol / L, and the reaction is terminated when no gas is generated.

8. The method for extracting vanadium pentoxide from composite oxide ore doped with lepidolite as claimed in claim 1, characterized in that: The oxidation reaction may be followed by a secondary oxidation, wherein an oxidant is used to carry out the secondary oxidation reaction.