Wave-absorbing composite material based on waste ternary positive electrode of lithium ion battery and preparation method of wave-absorbing composite material
By combining graphene oxide, carbon nanotubes with waste ternary positive electrode materials of lithium-ion batteries, porous carbon-based absorbing composite materials are prepared, which solves the problem of insufficient mass ratio of existing absorbing materials and achieves high-efficiency electromagnetic Improvement of absorption performance and secondary utilization of resources adapt to high load application scenarios and reduce production costs.
Patent Information
- Application Number
- CN202410980522.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
Due to the lower mass than absorption strength of existing wave absorbing materials, it is difficult to adapt to application scenarios with high load requirements. At the same time, the secondary utilization method of ternary positive electrode materials for waste lithium-ion batteries has not been effectively explored, resulting in waste of resources and high production costs.
By combining graphene oxide, carbon nanotubes and lithium-ion battery waste ternary positive electrode material, porous carbon-based wave absorbing composite materials are prepared, and high-temperature treatment is used to transform magnetic oxides and conductive materials to achieve effective absorption of electromagnetic waves. The specific steps include dispersing graphene oxide and carbon nanotubes in deionized water, adding PVA aqueous solution and glucose, dispersing ultrasonic and freeze-drying, and then sintering under a protective atmosphere to form an absorbing composite material with enhanced electromagnetic absorption properties.
It has achieved enhanced electromagnetic absorption performance of materials, reduced resource consumption and production costs, adapted to high-load application scenarios, and improved the absorbing performance per unit mass through the synergistic effect of multiple metals and carbon materials.
Smart Images

Figure CN118908303A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a wave-absorbing material and a preparation method thereof, and specifically to a wave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries and a preparation method thereof. Background Art
[0002] Lithium-ion battery ternary cathode materials are widely used in electronic devices due to their excellent energy density and cycle stability, and they occupy a prominent position in the consumer market. Due to the limited service life of electrode materials and the continuous growth of the new energy market, the scale of scrapped ternary materials is also increasing year by year. At a time when metal resources are limited and environmental management is becoming increasingly perfect, turning waste materials (such as lithium-ion battery ternary cathode materials) into "treasures" and reusing them meets the development requirements of a resource-saving and environmentally friendly society.
[0003] With the development of communication technology and wireless equipment, electromagnetic shielding materials (absorbing materials) have received great attention from the military and civilian fields, and they play an irreplaceable role in defending military security, reducing electromagnetic pollution, protecting human health, and maintaining the normal operation of fine electronic equipment. For absorbing composite materials formed by metal elements, they mainly rely on eddy currents and electromagnetic resonance to achieve electromagnetic wave loss. Compared with absorbing materials formed by a single metal element, multi-metal alloys rely on multi-element composition and resonant frequency, multi-scale structural effects and enhanced interface effects to achieve effective absorption of electromagnetic waves in a wide frequency domain. However, due to the high density of metal materials, their mass-to-weight absorption strength is low, making it difficult to adapt to application scenarios with high load requirements. Summary of the invention
[0004] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a simple, convenient, low-cost, energy-saving and environmentally friendly method for preparing an absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries. Another purpose of the present invention is to provide an absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries with enhanced electromagnetic absorption performance.
[0005] Technical solution: The method for preparing a wave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to the present invention comprises the following steps:
[0006] Step 1, dispersing graphene oxide and carbon nanotubes in deionized water to obtain a dispersion, and preparing a PVA aqueous solution;
[0007] Step 2: washing and drying the waste ternary positive electrode material of lithium-ion batteries, ball milling and sieving to obtain fine powder of electrode material;
[0008] Step 3, adding the electrode material fine powder, PVA aqueous solution, polyvinyl pyrrolidone and glucose into the dispersion liquid, ultrasonically dispersing and fully stirring to obtain a mixed slurry;
[0009] Step 4, placing the mixed slurry in liquid nitrogen for freeze drying to obtain a porous carbon-based precursor;
[0010] Step five, sintering and carbonizing the porous carbon-based precursor under a protective atmosphere to obtain a microwave-absorbing composite material.
[0011] Furthermore, in step 1, the mass ratio of graphene oxide, carbon nanotubes and deionized water is 0.2-20:1:500-10000. The dispersion is assisted by stirring and ultrasound, stirring for 1.5-2 hours, ultrasonic dispersion for 25-35 minutes, and repeated for more than 10 times. The mass percentage of the PVA aqueous solution is 10-15%.
[0012] Furthermore, in step 2, an ethanol solution is used for washing, and the drying temperature is 75-85° C. The ball mill is a planetary ball mill with a rotation speed of 250-300 rpm, and the sieving is a 200-300 mesh sieve. If the sieving is less than 200 mesh, the electrode material powder particles are larger after sieving, which is not conducive to its efficient dispersion in the dispersion liquid.
[0013] Further, in step 2, the waste ternary positive electrode material of lithium-ion batteries is LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2. Preferably, the waste ternary positive electrode material of lithium-ion batteries is LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2.
[0014] Furthermore, in step three, the mass ratio of the electrode material fine powder, polyvinyl pyrrolidone and glucose is 6:3:5-10, and the volume ratio of the PVA aqueous solution to the dispersion is 2:4-5.
[0015] Furthermore, in step 3, deionized water is added during stirring to adjust the viscosity of the slurry, and the mass of the added deionized water is 0-15% of the mass of the dispersion. The viscosity of the mixed slurry is 2000-8000 mPa·s. If no water is added, the viscosity of the dispersion is too high, which is not conducive to sufficient stirring and mixing.
[0016] Furthermore, in step five, the protective atmosphere is argon, and the sintering is first pre-carbonized at 250-300° C. for 3-4 hours, and then sintered at 700-900° C. for 3-4 hours, with a heating rate of 3-5° C. / minute.
[0017] The electromagnetic absorption composite material based on waste ternary positive electrodes of lithium-ion batteries described in the present invention achieves enhancement of the electromagnetic absorption performance of the material.
[0018] Preparation principle: Waste battery powder is transformed into magnetic oxide material after heat treatment, which effectively dissipates electromagnetic wave energy mainly through magnetic loss. Graphene oxide is transformed into reduced graphene after high-temperature treatment, which enhances conductivity and dissipates electromagnetic wave energy through efficient dielectric loss. The two materials complement each other in wave absorption mechanism, thus achieving synergistic absorption.
[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0020] 1. By reusing waste materials (waste ternary cathode materials of lithium-ion batteries), resource consumption and the production cost of absorbing composite materials are reduced, and it can adapt to application scenarios with high load requirements;
[0021] 2. By combining multi-metal materials with carbon materials, the unit mass of the absorbing composite material is reduced. In addition, based on the "synergistic effect" between the components, the electromagnetic absorption performance of the material is enhanced;
[0022] 3. The process flow of the present invention is relatively simple and has strong scalability and practicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a graph showing the relationship between reflection loss and frequency of the wave-absorbing composite material obtained in Example 1 of the present invention;
[0024] Figure 2 is a graph showing the relationship between reflection loss and frequency of the wave-absorbing composite material obtained in Example 2 of the present invention;
[0025] Figure 3 is a graph showing the relationship between reflection loss and frequency of the wave-absorbing composite material obtained in Example 3 of the present invention;
[0026] Figure 4 is a graph showing the relationship between reflection loss and frequency of the wave-absorbing composite material obtained in Example 4 of the present invention;
[0027] Figure 5 4 is a graph showing the relationship between the reflection loss and frequency of the wave-absorbing composite material obtained in Example 5 of the present invention. DETAILED DESCRIPTION
[0028] Unless otherwise specified, the materials, reagents, instruments, etc. used in the following examples can be obtained from commercial sources. Experimental methods without specific conditions in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0029] Example 1
[0030] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0031] (1) Weigh 400 mg of graphene oxide and 50 mg of carbon nanotubes, and fully disperse them in 50 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 2 hours and ultrasonic dispersion for 30 minutes are repeated 10 times.
[0032] (2) Prepare a 10 wt% PVA aqueous solution.
[0033] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 0.8 Co 0.15 Al 0.05 O2(NCA) was washed with an ethanol solution, dried at 80°C for 24 hours, and then ball-milled at 300 rpm for 6 hours using a planetary ball mill and passed through a 200-mesh sieve to obtain fine powder of the electrode material.
[0034] (4) 6 g of electrode material powder, 20 ml of PVA solution, 3 g of PVP, and 3 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 4013 mPa·s.
[0035] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0036] (6) In an argon atmosphere, the precursor was first pre-carbonized at 300 °C for 3 h and then sintered at 700 °C for 3 h with a heating rate of 5 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0037] The wave absorbing composite material obtained in this embodiment was tested for wave absorbing performance by coaxial line transmission method. Figure 1 It can be seen that as the thickness of the sample increases, the effective absorption range of the material continues to move towards the low-frequency range. When the thickness is 1.0mm, the reflection loss of the material can reach -15dB (at 14GHz frequency).
[0038] Example 2
[0039] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0040] (1) Weigh 400 mg of graphene oxide and 50 mg of carbon nanotubes, and fully disperse them in 50 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 2 hours and ultrasonic dispersion for 30 minutes are repeated 10 times.
[0041] (2) Prepare a 10 wt% PVA aqueous solution.
[0042] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 0.8 Co 0.1 Mn 0.1 O2(811) was washed with an ethanol solution, dried at 80°C for 24 hours, and then ball-milled at 300 rpm for 6 hours using a planetary ball mill and passed through a 200-mesh sieve to obtain fine powder of the electrode material.
[0043] (4) 6 g of electrode material powder, 20 ml of PVA solution, 3 g of PVP, and 6 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 3768 mPa·s, during which 1 ml of deionized water was added.
[0044] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0045] (6) In an argon atmosphere, the precursor was first pre-carbonized at 300 °C for 3 h and then sintered at 700 °C for 3 h with a heating rate of 5 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0046] The absorbing composite material obtained in this example was subjected to the same absorbing performance test as in Example 1. The results are as follows: Figure 2 As shown in the figure, it can be seen that as the thickness of the sample increases, the effective absorption range of the material continues to move towards the low-frequency range. When the thickness is 1.5mm, the reflection loss of the material can reach nearly -8dB (at 11GHz frequency).
[0047] Example 3
[0048] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0049] (1) Weigh 400 mg of graphene oxide and 50 mg of carbon nanotubes, and fully disperse them in 50 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 2 hours and ultrasonic dispersion for 30 minutes are repeated 10 times.
[0050] (2) Prepare a 10 wt% PVA aqueous solution.
[0051] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 0.6 Co 0.2 Mn 0.2 O2(622) was washed with an ethanol solution, dried at 80°C for 24 hours, and then ball-milled at 300 rpm for 6 hours using a planetary ball mill and passed through a 200-mesh sieve to obtain fine powder of the electrode material.
[0052] (4) 6 g of electrode material powder, 20 ml of PVA solution, 3 g of PVP, and 7 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 5143 mPa·s, during which 2 ml of deionized water was added.
[0053] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0054] (6) In an argon atmosphere, the precursor was first pre-carbonized at 300 °C for 3 h and then sintered at 700 °C for 3 h with a heating rate of 5 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0055] The absorbing composite material obtained in this example was subjected to the same absorbing performance test as in Example 1. The results are as follows: Figure 3 As shown in the figure, it can be seen that as the thickness of the sample increases, the effective absorption range of the material continues to move towards the low-frequency range. When the thickness is 1.5mm, the reflection loss of the material can reach nearly -11dB (at 11GHz frequency).
[0056] Example 4
[0057] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0058] (1) Weigh 400 mg of graphene oxide and 50 mg of carbon nanotubes, and fully disperse them in 50 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 2 hours and ultrasonic dispersion for 30 minutes are repeated 10 times.
[0059] (2) Prepare a 10 wt% PVA aqueous solution.
[0060] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 0.5 Co 0.2 Mn 0.3 O2(523) was washed with an ethanol solution, dried at 80°C for 24 hours, and then ball-milled at 300 rpm for 6 hours using a planetary ball mill and passed through a 200-mesh sieve to obtain fine powder of the electrode material.
[0061] (4) 6 g of electrode material powder, 20 ml of PVA solution, 3 g of PVP, and 8 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 3490 mPa·s, during which 3 ml of deionized water was added.
[0062] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0063] (6) In an argon atmosphere, the precursor was first pre-carbonized at 300 °C for 3 h and then sintered at 700 °C for 3 h with a heating rate of 5 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0064] The absorbing composite material obtained in this example was subjected to the same absorbing performance test as in Example 1. The results are as follows: Figure 4 As shown in the figure, it can be seen that as the thickness of the sample increases, the effective absorption range of the material continues to move towards the low-frequency range. When the thickness is 1.5mm, the reflection loss of the material can reach nearly -10dB (at 11GHz frequency).
[0065] Example 5
[0066] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0067] (1) Weigh 400 mg of graphene oxide and 50 mg of carbon nanotubes, and fully disperse them in 50 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 2 hours and ultrasonic dispersion for 30 minutes are repeated 10 times.
[0068] (2) Prepare a 10 wt% PVA aqueous solution.
[0069] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 1 / 3 Co 1 / 3 Mn 1 / 3 O2(111) was washed with an ethanol solution, dried at 80°C for 24 hours, and then ball-milled at 300 rpm for 6 hours using a planetary ball mill and passed through a 200-mesh sieve to obtain fine powder of the electrode material.
[0070] (4) 6 g of electrode material powder, 20 ml of PVA solution, 3 g of PVP, and 9 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 5243 mPa·s. During this period, 4 ml of deionized water was added.
[0071] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0072] (6) In an argon atmosphere, the precursor was first pre-carbonized at 300 °C for 3 h and then sintered at 700 °C for 3 h with a heating rate of 5 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0073] The absorbing composite material obtained in this example was subjected to the same absorbing performance test as in Example 1. The results are as follows: Figure 5 As shown in the figure, it can be seen that as the thickness of the sample increases, the effective absorption range of the material continues to move towards the low-frequency range. When the thickness is 1.5mm, the reflection loss of the material can reach nearly -17dB (at 12GHz frequency).
[0074] Example 6
[0075] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0076] (1) Weigh 10 mg of graphene oxide and 50 mg of carbon nanotubes and fully disperse them in 25 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 1.5 hours and ultrasonic dispersion for 25 minutes are repeated 10 times.
[0077] (2) Prepare a 15 wt% PVA aqueous solution.
[0078] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 0.8 Co 0.1 Mn 0.1 O2(811) was washed with an ethanol solution, dried with forced air at 75°C for 24 hours, and then ball-milled with a planetary ball mill at 250 rpm for 6 hours and passed through a 300-mesh sieve to obtain fine powder of the electrode material.
[0079] (4) 6 g of electrode material powder, 10 ml of PVA solution, 3 g of PVP, and 5 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 8000 mPa·s, during which 15 ml of deionized water was added.
[0080] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0081] (6) In an argon atmosphere, the precursor was first pre-carbonized at 250 °C for 4 h and then sintered at 900 °C for 4 h with a heating rate of 4 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0082] Example 7
[0083] A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries comprises the following steps:
[0084] (1) Weigh 1000 mg of graphene oxide and 50 mg of carbon nanotubes, and fully disperse them in 500 ml of deionized water to obtain a dispersion. The dispersion process is assisted by stirring and ultrasound. Stirring for 1.5 hours and ultrasonic dispersion for 35 minutes are repeated 20 times.
[0085] (2) Prepare a PVA aqueous solution with a mass percentage of 13 wt%.
[0086] (3) Recycling of LiNi, a waste ternary cathode material of lithium-ion batteries 0.8 Co 0.15 Al 0.05 O2(NCA) was washed with an ethanol solution, dried with forced air at 85°C for 24 hours, and then ball-milled with a planetary ball mill at 280 rpm for 6 hours and passed through a 300-mesh sieve to obtain fine powder of the electrode material.
[0087] (4) 6 g of electrode material powder, 200 ml of PVA solution, 3 g of PVP, and 10 g of glucose were added to the graphene oxide / carbon nanotube dispersion, and ultrasonically dispersed and stirred for 12 hours to prepare a mixed slurry with a viscosity of 2000 mPa·s, during which 10 ml of deionized water was added.
[0088] (5) The mixed slurry was placed in liquid nitrogen and frozen for 6 hours, and then freeze-dried to prepare a dry porous carbon-based precursor.
[0089] (6) In an argon atmosphere, the precursor was first pre-carbonized at 280 °C for 3.5 hours and then sintered at 800 °C for 3.5 hours with a heating rate of 3 °C / min to obtain a microwave-absorbing composite material based on the waste ternary positive electrode of a lithium-ion battery.
[0090] Comparative Example 1
[0091] The remaining steps of this comparative example are the same as those of Example 1, except that the graphene oxide is replaced by reduced graphene. It is found that the reduced graphene has extremely poor dispersibility during the preparation of the dispersion, resulting in poor consistency and uniformity of the obtained material.
[0092] Comparative Example 2
[0093] The remaining steps of this comparative example are the same as those of Example 1, except that 400 mg of graphene oxide is replaced by 1500 mg of graphene oxide, that is, the mass ratio of graphene oxide to carbon nanotubes is 30: 1. The results show that the overall wave absorption performance is reduced due to the reduced magnetic loss efficiency of the material to electromagnetic waves.
[0094] Comparative Example 3
[0095] The remaining steps of this comparative example are the same as those of Example 1, except that the number of repetitions is changed from 10 to 3. The results show that the dispersion of carbon nanotubes in the system is poor, which affects the uniformity of the final material.
[0096] Among the above embodiments, embodiment 5 is the best embodiment.
Claims
1. A method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries, characterized in that: The following steps are involved: Step 1, dispersing graphene oxide and carbon nanotubes in deionized water to obtain a dispersion, and preparing a PVA aqueous solution; Step 2: washing and drying the waste ternary positive electrode material of lithium-ion batteries, ball milling and sieving to obtain fine powder of electrode material; Step 3, adding the electrode material fine powder, PVA aqueous solution, polyvinyl pyrrolidone and glucose into the dispersion liquid, ultrasonically dispersing and fully stirring to obtain a mixed slurry; Step 4, placing the mixed slurry in liquid nitrogen for freeze drying to obtain a porous carbon-based precursor; Step five, sintering and carbonizing the porous carbon-based precursor under a protective atmosphere to obtain a microwave-absorbing composite material.
2. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 1, the mass ratio of graphene oxide, carbon nanotubes and deionized water is 0.2-20:1:500-10000.
3. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 1, the dispersion is assisted by stirring and ultrasound, stirring for 1.5 to 2 hours and ultrasonic dispersion for 25 to 35 minutes, and this is repeated more than 10 times.
4. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 1, the mass percentage of the PVA aqueous solution is 10-15%.
5. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 2, ethanol solution is used for washing, and the drying temperature is 75-85°C.
6. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 2, the ball mill is a planetary ball mill with a rotation speed of 250-300 rpm, and the sieving is through a 200-300 mesh sieve.
7. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 3, the mass ratio of the electrode material fine powder, polyvinyl pyrrolidone and glucose is 6:3:5-10, and the volume ratio of the PVA aqueous solution to the dispersion is 2:4-5.
8. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 3, the mass of the added deionized water is 0 to 15% of the mass of the dispersion.
9. The method for preparing a microwave-absorbing composite material based on waste ternary positive electrodes of lithium-ion batteries according to claim 1, characterized in that: In the step 5, the protective atmosphere is argon, and the sintering is first pre-carbonized at 250-300° C. for 3-4 hours, and then sintered at 700-900° C. for 3-4 hours, with a heating rate of 3-5° C. / minute.